Shell preparation method, shell and electronic equipment
By hot-pressing the composite material plate in the mold, a shell with multi-directional appearance surfaces is formed, which solves the problems of composite material CNC processing surface defects and insufficient three-dimensionality, realizes the direct formation of various appearance effects, and simplifies the process flow. and save costs.
Patent Information
- Application Number
- CN202310413257.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-22
AI Technical Summary
The CNC machined surface of composite materials is prone to defects when making exterior parts. Avoiding the use of CNC machined surfaces as exterior surfaces will result in a weak three-dimensional effect and the inability to achieve multi-directional matte and texture effects.
The composite material plate is hot-pressed in a molding mold of a preset shape to form a shell with an appearance surface in the first direction and a second direction. The molten resin in the semi-solid composite material is used to flow and fill the mold to achieve a fine and uniform appearance surface. And films can be added during the molding process to achieve various appearance requirements.
It solves the problem of defects in the CNC machining surface of composite materials, improves the three-dimensional effect of the shell, avoids the grinding and spraying process, realizes the direct formation of multi-directional appearance effects, simplifies the process and saves costs.
Smart Images

Figure CN118810079A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of shell manufacturing, and in particular to a shell preparation method, a shell and an electronic device. Background Art
[0002] With the growing demand for lightweight structural parts, composite materials with high specific strength and high specific modulus have gradually become common materials for manufacturing lightweight structural parts. Among them, the appearance processing technology of composite materials is usually CNC processing (computer numerical control processing) technology. When composite materials are directly used as appearance parts, the CNC-processed surface of the composite material will inevitably be used as the appearance surface, but the CNC-processed surface of the composite material often has obvious defects, which leads to the need to cover the defects of the CNC-processed surface used as the appearance surface by grinding and spraying. In addition, if the CNC-processed surface of the composite material is to be avoided from being used as the appearance surface, it will result in the appearance surface being made in only a single direction, without appearance surfaces in other directions. The three-dimensional sense of the appearance part is not strong, and it is impossible to achieve multiple directions at the same time with various matte surfaces, textures, etc. that can be produced on the surface of the composite material. Summary of the invention
[0003] In order to solve the problems existing in the related art, the present disclosure provides a method for preparing a shell, a shell and an electronic device.
[0004] According to a first aspect of an exemplary embodiment of the present disclosure, a method for preparing a housing is provided, the method comprising:
[0005] Under preset conditions, the composite material plate to be hot-pressed is hot-pressed in a forming mold to form the shell, wherein the composite material plate includes a semi-solid composite material plate and the forming mold has a preset shape; the preset shape is configured so that during the hot-pressing process, the molten resin in the composite material plate flows and fills the forming mold, so that the shell forms appearance surfaces in the first direction and the second direction.
[0006] In some embodiments, the preset shape includes an "S" shape.
[0007] In some embodiments, the first direction and the second direction form a first preset angle, and the first preset angle is greater than or equal to 60 degrees.
[0008] In some embodiments, the thickness of the shell in the second direction is greater than or equal to 0.5 mm.
[0009] In some embodiments, a width of the to-be-processed portion of the shell in the second direction is less than or equal to 0.3 mm.
[0010] In some embodiments, the step of hot-pressing the composite material sheet to be hot-pressed in a forming mold under preset conditions to form the shell includes:
[0011] stacking a preset number of layers of composite material panels in the forming mold according to a preset rule;
[0012] The shell is formed by hot pressing under preset conditions.
[0013] In some embodiments, the preset conditions include:
[0014] The molding pressure includes 15 to 25 MPa; the molding temperature includes 150 to 190° C.; and the molding time includes 5 to 15 minutes.
[0015] In some embodiments, stacking a preset number of layers of composite material panels in the forming mold according to a preset rule includes:
[0016] The warp threads and / or weft threads of the adjacent composite material panels are stacked in the forming mold at a second preset angle.
[0017] In some embodiments, the second preset angle includes 0 to 90 degrees.
[0018] In some embodiments, the preset number of layers includes 5 to 8 layers.
[0019] According to a second aspect of an exemplary embodiment of the present disclosure, there is provided a shell, wherein the shell is manufactured according to the method for manufacturing a shell as described in any one of the first aspects above.
[0020] According to a third aspect of an exemplary embodiment of the present disclosure, an electronic device is provided, wherein the electronic device comprises the housing as described in the second aspect above.
[0021] The beneficial effects of the present disclosure include but are not limited to: the preparation method of the shell provided by the present disclosure, by hot pressing a composite material plate in a molding mold with a preset shape, the molten resin in the composite material plate flows to fill the molding mold with a preset shape, and a shell with appearance surfaces in a first direction and a second direction is formed, thereby improving the three-dimensional appearance of the shell, and solving the problem of needing to grind and spray the processed surface to cover defects when the composite material is directly used as the appearance surface.
[0022] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings incorporated into the specification and constituting a part of the specification illustrate embodiments of the present disclosure and are used together with the description to explain the principles of the embodiments of the present disclosure. In these drawings, similar reference numerals are used to represent similar elements. The drawings described below are some embodiments of the present disclosure, rather than all embodiments. For those skilled in the art, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 A method for preparing a housing according to an exemplary embodiment of the present disclosure;
[0025] Figure 2 is a schematic diagram of a housing of an exemplary embodiment of the present disclosure;
[0026] Figure 3a A schematic longitudinal cross-sectional view of a rear cover of a mobile terminal device according to an exemplary embodiment of the present disclosure;
[0027] Figure 3b A schematic longitudinal cross-sectional view of a back cover of a mobile terminal device in a related art of an exemplary embodiment of the present disclosure;
[0028] Figure 4a A schematic diagram of a rear cover blank of a mobile terminal device in a related art of an exemplary embodiment of the present disclosure;
[0029] Figure 4b A schematic diagram of a back cover blank of a mobile terminal device according to an exemplary embodiment of the present disclosure;
[0030] Figure 5 It is a schematic diagram of a process of hot-pressing a composite material plate to be hot-pressed in a forming mold to form a shell under preset conditions according to an exemplary embodiment of the present disclosure;
[0031] Figure 6 It is a schematic diagram of the stacking of a composite material plate according to an exemplary embodiment of the present disclosure. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solutions and advantages of the embodiments of the present disclosure clearer, the technical solutions of the present disclosure will be clearly and completely described below in combination with the embodiments of the present disclosure. Obviously, the described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure. It should be noted that the embodiments in the present disclosure and the features in the embodiments can be arbitrarily combined with each other without conflict.
[0033] In the related art, when composite materials with high specific strength and high specific modulus are used to manufacture lightweight structural parts, CNC technology is usually required to process the composite materials. If the composite materials are to be used directly as appearance parts, the CNC-machined surface of the composite materials will inevitably be used as the appearance surface, but the CNC-machined surface of the composite materials often has obvious defects and needs to be covered by grinding and spraying. In addition, if the CNC-machined surface of the composite materials is to be avoided from being used as the appearance surface, it will result in only a single-direction surface being used as the appearance surface, without appearance surfaces in other directions. The three-dimensional sense of the appearance parts is not strong, and it is impossible to achieve multiple directions with various matte surfaces, textures, and other appearance effects that can be produced on the surface of the composite materials at the same time.
[0034] Based on this, the exemplary embodiment of the present disclosure provides a method for preparing a housing, and the method for preparing a housing provided by the present disclosure can be applied to any field requiring housing manufacturing, such as the manufacturing of exterior structural parts of electronic equipment, automobile interiors, sporting goods, etc. Figure 1 As shown, the preparation method of the shell provided by the present disclosure includes:
[0035] S100: Under preset conditions, the composite material plate to be hot-pressed is hot-pressed in a forming mold to form a shell.
[0036] Among them, the composite material plate in this step includes a semi-solid composite material plate, and the molding mold has a preset shape; the preset shape is set so that during the hot pressing molding process, the molten resin in the composite material plate flows and fills the molding mold, so that the shell forms an appearance surface in the first direction and the second direction.
[0037] In the preparation method of the shell provided by the present disclosure, a semi-solid composite material plate is selected, and the semi-solid composite material plate contains resin. The semi-solid composite material plate to be hot-pressed is hot-pressed in a molding mold with a preset shape. When the semi-solid composite material is heated, the resin therein softens and flows to fill, for example, fills the entire cavity of the molding mold. The shell appearance surface is filled with the resin in the composite material plate, and after cooling, a shell having an appearance surface with a delicate and uniform appearance in the first direction and the second direction is obtained. The shell prepared by the preparation method of the shell provided by the present disclosure, its surfaces in the first direction and the second direction can be directly used as the appearance surface, and its surface is smooth and flat, and no processing is required, which avoids the problem of defects in the processing process, and there is no need to cover the defective surface through grinding and spraying processes.
[0038] In addition, if the shell needs to meet appearance requirements such as matte, glossy and special textures, it is only necessary to attach a film with corresponding effects to the appearance side of the semi-solid composite material when the molding mold is heated and pressed. During heating and pressing, the resin in the semi-solid composite material softens and flows, and the effect of the film will appear on the appearance surface of the composite material. There is no need for processing and engraving to achieve various appearance requirements of the shell. The preparation process is convenient, simple and efficient. At the same time, it avoids waste loss during the processing and engraving process, saving costs.
[0039] In the exemplary embodiment provided in the present disclosure, the preset shape includes an "S" shape. In the preparation method of the shell provided in the present disclosure, the preset shape of the molding die includes an "S" shape. When the semi-solid composite material plate to be hot-pressed is hot-pressed in the "S"-shaped molding die, the semi-solid composite material is heated, and the resin therein softens and flows to fill, for example, filling the entire cavity of the "S"-shaped molding die. The composite material in the cavity is arranged in an "S" shape, and finally the appearance surfaces in the first direction and the second direction are filled with the resin in the composite material, so as to obtain a shell with a delicate and uniform appearance.
[0040] The shell can also be sprayed according to actual needs to make its appearance have anti-dizziness or other specific arrangement of textures.
[0041] In the prior art, when molding plates, only an "I"-shaped mold is often used. Heating and pressing can only achieve an appearance in a single direction, and the three-dimensional effect is not strong, and it is impossible to achieve a variety of appearance shapes of the shell. In the shell preparation method provided in the present disclosure, an "S"-shaped mold is selected, so that the shell obtained after hot pressing has appearance surfaces in different directions, thereby enhancing the three-dimensional effect of the shell.
[0042] In the method for preparing the shell provided in the present disclosure, Figure 2 As shown in the schematic diagram of the shell, a shell having an appearance surface 1 in a first direction 100 and an appearance surface 2 in a second direction 200 can be directly formed by an S-shaped mold, so that the appearance surface can be presented in both the first direction and the second direction, thereby improving the three-dimensional effect of the shell.
[0043] The shell prepared by the shell preparation method provided by the present disclosure has an appearance surface in a first direction and an appearance surface in a second direction, and a first preset angle 10 between the appearance surface in the first direction and the appearance surface in the second direction is greater than or equal to 60 degrees, for example, the first preset angle 10 can be 60 degrees, 80 degrees, 90 degrees, 100 degrees, 120 degrees, 150 degrees. Figure 2In the illustrated exemplary embodiment, the first preset angle 10 is 90 degrees. If the first preset angle 10 between the appearance surface in the first direction and the appearance surface in the second direction is too small, it is easy to produce a "dead angle" in the modeling, which is not conducive to the flow of resin in the hot pressing process to fully fill the inner cavity of the molding mold, and will cause modeling defects. In addition, if the first preset angle 10 between the appearance surface in the first direction and the appearance surface in the second direction is too small, it is not conducive to the demolding of the shell after the hot pressing is completed, and it is easy to cause defective products. Therefore, the shell prepared by the preparation method of the shell provided in the present disclosure, the first preset angle 10 between the appearance surface in the first direction and the appearance surface in the second direction is limited to be greater than or equal to 60 degrees, which can not only meet the diverse modeling of the shell, but also ensure the yield of the prepared shell.
[0044] In an exemplary embodiment provided by the present disclosure, the thickness of the shell in the second direction is greater than or equal to 0.5 mm.
[0045] Compared with the related art in which an "I"-shaped mold is used to mold a sheet material to produce a shell with a single-direction appearance surface, the shell preparation method provided in the present disclosure uses an "S"-shaped mold, so that after hot pressing, a shell with appearance surfaces in the first direction and the second direction is obtained. Compared with the shell prepared in the related art, the shell has more appearance surfaces with a thickness of more than 0.5 mm in different directions, and can realize the appearance surface design in the second direction, enhance the three-dimensional effect, and eliminate the grinding and spraying processes.
[0046] For example, Figure 2 As shown, when the preparation method of the shell provided by the present disclosure is applied to prepare the back cover of the mobile terminal device, the prepared shell has a horizontal appearance surface 1 and a vertical appearance surface 2 that can be directly used as the appearance surface, and the aforementioned appearance surfaces 1 and 2 do not need to be processed, and can be directly used as the appearance surface after hot pressing, eliminating the process of grinding and spraying the vertical processing surface in the related art.
[0047] In an exemplary embodiment provided by the present disclosure, a width of the to-be-processed portion of the shell in the second direction is less than or equal to 0.3 mm.
[0048] In the method for preparing a shell provided by the present disclosure, the prepared shell has an appearance surface in a first direction and an appearance surface in a second direction, and has a portion to be processed on the appearance surface in the second direction. In the method for preparing a shell provided by the present disclosure, by hot pressing a semi-solid composite material plate in an "S"-shaped forming mold, the portion to be processed on the appearance surface in the second direction of the shell prepared after hot pressing is reduced to less than 0.3 mm, without affecting the appearance surface presentation of the shell in the second direction. The portion to be processed may be in the same plane direction as the appearance surface in the second direction, may protrude from the appearance surface in the second direction, or may be recessed in the appearance surface in the second direction, and the present disclosure does not limit this.
[0049] For example, in the related art, when preparing the back cover of a mobile terminal device, Figure 3b As shown, only the hot-pressed composite material can be directly used as the appearance surface in the horizontal direction. If the appearance surface in the vertical direction is desired, the thicker processed surface 22 needs to be polished and sprayed before it can be used as the appearance surface, because the processed surface 22 before polishing and spraying is Figure 4a As shown, after the CNC process cuts off the excess material, the fiber end surface 31 of the processed surface is exposed, resulting in defects and cannot be directly used as an appearance surface.
[0050] In the method for preparing the shell provided in the present disclosure, Figure 3a As shown, when the shell preparation method provided by the present disclosure is applied to the preparation of the back cover of a mobile terminal device, the prepared back cover shell has a horizontal appearance surface and a vertical appearance surface, and the part to be processed 21 protrudes from the vertical appearance surface with a very small width. After the hot pressing of the shell preparation method provided by the present disclosure is completed, the blank of the back cover shell is taken out from the molding die, and the redundant feature parts on the part to be processed 21 are cut off by CNC process to obtain the final required back cover shell, as shown in FIG. Figure 4b As shown, the shell only has a very slight whitish position on the bottom edge, which does not affect the appearance surface of the rear cover shell in the first direction and the appearance surface of the rear cover shell in the second direction, and the appearance surface 32 is directly made. It should be noted that the appearance surface of the rear cover shell and the milling cutter used for CNC processing cannot be on the same side to avoid knife marks, scratches, bumps and other undesirable phenomena. When assembling a mobile terminal device, the appearance surface of the horizontal direction and the appearance surface of the vertical direction of the rear cover shell are directly made into the appearance surface of the mobile terminal device, which can ensure that the substrate on the appearance surface is uniform and consistent, and avoid unevenness caused by inconsistent materials or processing procedures; the processing surface of the rear cover shell is buried under the middle frame to cover the processing surface so that it is not exposed on the appearance surface of the mobile terminal device. In addition, burying the protruding processing surface under the middle frame can also make the rear cover shell directly fixed on the device body, making the connection between the rear cover and the device body more stable.
[0051] Among them, when the redundant feature parts on the part to be processed 21 are cut off by CNC process, the parameter settings of the digital control machine tool include: the Z-axis tool feed amount includes 0.01~0.03 mm / revolution, and the feed rate includes 1800 mm / minute. Within this parameter setting range, it can ensure that the finished product has no knife marks while increasing the stability of the finished product by 5%.
[0052] When the preparation method of the shell provided by the present disclosure is applied to the preparation of the colored battery back cover of the mobile terminal device, after the back cover shell is prepared by the above method, the back cover shell is sprayed. First, when spraying the primer, an acrylic paint with good leveling property is used to fill the surface unevenness generated in the previous process and provide the appearance color effect; for example, when the required colored battery back cover is a white back cover, adding a small amount of white filler to the primer can further cover the surface unevenness of the material. After spraying the primer, a back cover shell with a color effect is obtained, and then a topcoat is sprayed on it to achieve the purpose of providing wear resistance and strength, and finally the required colored battery back cover is obtained; wherein, the sprayed topcoat uses a high-functionality (greater than or equal to 25%) difunctional polyurethane-modified acrylic material, which can enhance the performance of the colored battery cover after vibration and friction, making it smooth, without paint collapse, and without step feel.
[0053] In the exemplary embodiments provided in the present disclosure, Figure 5 As shown, under preset conditions, the composite material plate to be hot-pressed is hot-pressed in a forming mold to form a shell, including:
[0054] S1: stacking composite material panels with a preset number of layers in a forming mold according to preset rules.
[0055] In this step, the composite material plate is cut into the required size and shape according to the modeling drawing of the shell. For example, the composite material plate can be cut into a rectangle, a square, a rounded rectangle, or a rounded square, and the shape and size of each composite material plate can be the same or different, so as to better meet the requirements of the appearance or mechanical properties of the shell produced by the shell preparation method provided by the present disclosure in the application; an "S"-shaped molding mold is obtained, and in the "S"-shaped molding mold, the cut composite material plates of a preset number of layers are stacked according to preset rules. When stacking, the preset rules can be set according to the required shell shape and the stress conditions or other requirements during application.
[0056] S2: Hot pressing and forming under preset conditions to form a shell.
[0057] In this step, the composite material plates stacked in the "S"-shaped forming mold are hot-pressed under preset conditions to obtain a formed shell.
[0058] For example, the composite material plates are stacked in an "S"-shaped forming mold, and under preset conditions, the stacked composite material plates are hot-pressed into a shell blank in the forming mold by closing the upper and lower molds. The hot-pressed shell blank is cut off with a CNC process to remove the redundant feature parts on the part to be processed, and the final required shell is obtained.
[0059] The shell preparation method provided in this embodiment is as follows: composite material plates having higher modulus and better impact resistance than traditional plastic materials are stacked in an "S"-shaped molding mold according to preset rules, and the stacked composite material plates are hot-pressed in the "S"-shaped molding mold under preset conditions, so that the high-fluidity viscous resin in the composite material plates flows to fill the entire mold cavity, so that the final shell has a delicate and uniform appearance.
[0060] Different from the related art in which the shell is prepared by injection molding of plastic materials, the shell preparation method provided by the present invention stacks composite material plates in an "S"-shaped molding mold according to preset rules, so that the pressed shell can meet the needs of various complex shapes. At the same time, it can avoid the problem of high local stress and poor flatness caused by large changes in shape and size when preparing an integrated shell with complex shape.
[0061] In the exemplary embodiments provided in the present disclosure, the preset conditions include:
[0062] The molding pressure includes 15 to 25 MPa; the molding temperature includes 150 to 190° C.; and the molding time includes 5 to 15 minutes.
[0063] After the composite material plates are stacked in the "S"-shaped forming mold, the composite material plates can be pressed together by closing the upper and lower molds. The temperature of the "S"-shaped forming mold needs to reach 150-190°C. Within this temperature range, the viscous resin in the composite material plates melts and flows to fill, for example, filling the entire "S"-shaped mold cavity. The molding pressure of the "S"-shaped forming mold needs to be set at 15-25MPa. Within this pressure range, the stacked composite material plates in the "S"-shaped forming mold can be pressed into shape. After the "S"-shaped forming mold is closed, it should be kept at the preset molding temperature and preset molding pressure for 5-15 minutes to ensure that the viscous resin in the composite material plates in the "S"-shaped forming mold is fully melted and flows to fill the entire mold cavity, so that the final first and second direction appearance surfaces are filled with the resin in the composite material, and ensure that the composite material plates are pressed tightly by the "S"-shaped forming mold to form a shell with a delicate and uniform appearance.
[0064] In an exemplary embodiment provided by the present disclosure, stacking a preset number of composite material panels in a forming mold according to a preset rule includes:
[0065] The warp threads and / or weft threads of adjacent composite material panels are stacked in a forming mold at a second preset angle.
[0066] For example, in the method for preparing the shell provided by the present disclosure, a preset number of layers of composite materials are stacked at a second preset angle between the warps of adjacent composite materials; or a preset number of layers of composite materials are stacked at a second preset angle between the wefts of adjacent composite materials; or some composite materials are stacked at a second preset angle between the warps of adjacent composite materials, and the remaining composite materials are stacked at a second preset angle between the wefts of adjacent composite materials. The stacking directions between adjacent composite materials can be the same or different, and similarly, the second preset angles between adjacent composite materials can be the same or different to meet different requirements of the shell, such as the shape, thickness or strength requirements of the shell.
[0067] In the exemplary embodiments provided in the present disclosure, Figure 6 As shown, Figure 6 The method of stacking any two adjacent layers of composite panels in the shell is exemplarily shown in the figure. The angle α between the warp 301 of the first composite panel 300 and the warp 401 of the second composite panel 400 can be used as the second preset angle. The angle β between the weft 302 of the first composite panel 300 and the weft 402 of the second composite panel 400 can also be used as the second preset angle. When stacking multiple layers of composite panels, some composite panels can be arranged at the second preset angle between the warp lines of adjacent composite panels, and the remaining composite panels can be arranged at the second preset angle between the weft lines of adjacent composite panels.
[0068] In an exemplary embodiment provided by the present disclosure, the second preset angle includes 0 to 90 degrees.
[0069] The shell preparation method provided in the present disclosure stacks composite material plates according to preset rules, for example, by changing the stacking angle of the composite material plates to perform stacking optimization, so that the composite material plates with different stacking angles can meet the appearance requirements of different shapes after being pressed into a shell, and can withstand stresses from different directions, so that the overall force strength of the shell is higher and the structure is more stable. At the same time, it can avoid the problem of high local stress and poor flatness caused by large changes in shape and size when preparing a shell with a complex shape.
[0070] In actual production and application, the second preset angle between adjacent composite material plates in the shell can be selected within the range of 0 to 90 degrees according to specific needs. For example, the second preset angle between adjacent composite material plates in the shell can be selected in combination with the number of layers of composite material plates in the shell, the appearance surface shape of the shell, the force direction and the degree of force. For example, the second preset angle can be in the range of 15 to 75 degrees. In an exemplary example of the present disclosure, the shell includes 6 layers of composite material plates, and the stacking angle between each composite material plate, that is, the warp and / or weft between adjacent composite material plates is "0 degrees / 45 degrees / 0 degrees / 45 degrees / 0 degrees / 45 degrees", and the second preset angle is 45 degrees. Or "0 degrees / 45 degrees / 45 degrees / 45 degrees / 45 degrees / 0 degrees", the second preset angle is 45 degrees and 0 degrees. Or the warp and / or weft between adjacent composite material plates is "0 degrees / 60 degrees / 60 degrees / 60 degrees / 60 degrees / 0 degrees", and the second preset angle is 0 degrees and 60 degrees. Or "0 degrees / 60 degrees / 0 degrees / 60 degrees / 0 degrees / 60 degrees", the second preset angle is 60 degrees. Or the warp and / or weft of adjacent composite panels are "0 degrees / 45 degrees / 15 degrees / 30 degrees / 60 degrees / 0 degrees", the second preset angle includes 45 degrees, 30 degrees, 15 degrees and 60 degrees. The second preset angles between adjacent composite panels can be the same or different, and can be flexibly selected according to actual needs, and the present disclosure does not limit it here.
[0071] In the exemplary embodiment provided in the present disclosure, the preset number of layers includes 5 to 8 layers.
[0072] In the preparation method of the shell provided in the present disclosure, the preset number of layers of the stacked composite materials is limited to 5 to 8 layers. For example, the preset number of layers of the composite materials can be 5, 6, 7, or 8 layers. By stacking the composite materials according to preset rules, for example, by changing the stacking angle between the composite materials, stacking optimization is performed. This allows the composite materials with different stacking angles to be pressed into a shell to meet the requirements of different appearance surfaces, while ensuring the strength of the shell. This ensures that the overall force strength of the shell is high enough and the structure is stable enough under the complex appearance surface shape.
[0073] In an exemplary embodiment provided by the present disclosure, the semi-solid composite material plate includes a reinforced epoxy resin composite fiberglass plate.
[0074] In the preparation method of the shell provided by the present disclosure, the selected composite material board includes a reinforced epoxy resin composite glass fiber board. Among them, epoxy resin is a thermosetting resin, which has excellent mechanical properties, electrical insulation, and heat resistance. In addition, epoxy resin has low curing shrinkage and strong bonding force; glass fiber has the characteristics of non-flammability, heat insulation, high tensile strength, and good electrical insulation; the reinforced epoxy resin composite glass fiber board made of glass fiber as a reinforcing material and epoxy resin as an adhesive has strong mechanical properties and dielectric properties, and has good processability and flatness. In the preparation method of the shell provided by the present disclosure, a reinforced epoxy resin composite glass fiber board is selected, and it is stacked in an "S"-shaped molding mold according to preset rules, and the stacked reinforced epoxy resin composite glass fiber board is hot-pressed in an "S"-shaped molding mold with preset conditions, so that the high-fluidity epoxy resin in the composite material board flows and fills, for example, fills the entire mold cavity, so that the final shell has a delicate and uniform appearance. In addition, since the reinforced epoxy resin composite glass fiber board itself has high strength and a modulus of more than 20GPa, the shell prepared by the shell preparation method provided in the present invention can have high strength and impact resistance, avoiding the shell deformation problem caused by stress concentration when the shell is subjected to force under complex shapes.
[0075] An exemplary embodiment of the present disclosure provides a shell, which is manufactured according to the shell manufacturing method provided by the present disclosure.
[0076] The housing provided by the exemplary embodiment of the present disclosure includes: an appearance surface in a first direction and an appearance surface in a second direction.
[0077] The housing provided by the exemplary embodiment of the present disclosure is as follows: Figure 2 As shown, the shell having an appearance surface 1 in the first direction 100 and an appearance surface 2 in the second direction 200 can present an appearance surface in both the first direction and the second direction. The surface is smooth and flat, and no processing is required, thus avoiding the problem of defects in the processing process, and there is no need to cover the defective surface through grinding and spraying processes.
[0078] In the exemplary embodiment provided by the present disclosure, the shell provided by the present disclosure has an appearance surface in a first direction and an appearance surface in a second direction, and a first preset angle 10 between the appearance surface in the first direction and the appearance surface in the second direction is greater than or equal to 60 degrees, for example, the first preset angle 10 can be 60 degrees, 80 degrees, 90 degrees, 100 degrees, 120 degrees, 150 degrees. Figure 2In the illustrated exemplary embodiment, the first preset angle 10 is 90 degrees. If the first preset angle 10 between the appearance surface in the first direction and the appearance surface in the second direction is too small, it is easy to produce a "dead angle" in the modeling during hot pressing in the molding die, which is not conducive to the flow of resin to fully fill the inner cavity of the molding die during the hot pressing process, and will cause modeling defects. In addition, if the first preset angle 10 between the appearance surface in the first direction and the appearance surface in the second direction is too small, it is not conducive to the demolding of the shell after the hot pressing in the molding die is completed, and it is easy to cause defective products. Therefore, the shell provided by the present disclosure, the first preset angle 10 between the appearance surface in the first direction and the appearance surface in the second direction is limited to be greater than or equal to 60 degrees, which can not only meet the diverse modeling of the shell, but also ensure the yield of the shell.
[0079] In an exemplary embodiment provided by the present disclosure, the thickness of the shell in the second direction is greater than or equal to 0.5 mm.
[0080] Compared with the related art in which an "I"-shaped mold is used to produce a shell with a single-direction appearance surface when molding a sheet material, the shell provided by the present invention has appearance surfaces in the first direction and the second direction. Compared with the shell produced in the related art, it has appearance surfaces with a thickness of more than 0.5 mm in different directions, which can realize the appearance surface design in the second direction, enhance the three-dimensional effect, and eliminate the grinding and spraying processes.
[0081] For example, Figure 2 As shown, when the shell provided by the present disclosure is applied to the back cover of a mobile terminal device, the back cover has a horizontal appearance surface 1 and a vertical appearance surface 2 that can be directly used as appearance surfaces. The aforementioned appearance surfaces 1 and 2 do not need to be processed and can be directly used as appearance surfaces, eliminating the process of grinding and spraying the vertical processing surface in the related art.
[0082] In an exemplary embodiment provided by the present disclosure, a width of the to-be-processed portion of the shell in the second direction is less than or equal to 0.3 mm.
[0083] The shell provided by the present disclosure has an appearance surface in the first direction and an appearance surface in the second direction, and has a portion to be processed on the appearance surface in the second direction. The width of the portion to be processed on the appearance surface in the second direction of the shell provided by the present disclosure is as low as 0.3 mm or less, which does not affect the appearance of the shell in the second direction. The portion to be processed can be in the same plane direction as the appearance surface in the second direction, or can be protruding from the appearance surface in the second direction, or can be recessed in the appearance surface in the second direction, and the present disclosure does not limit this.
[0084] For example, in the related art, when preparing the back cover of a mobile terminal device, Figure 3bAs shown, only the hot-pressed composite material can be directly used as the appearance surface in the horizontal direction. If the appearance surface in the vertical direction is desired, the thicker processed surface 22 needs to be polished and sprayed before it can be used as the appearance surface, because the processed surface 22 before polishing and spraying is Figure 4a As shown, after the CNC process cuts off the excess material, the fiber end surface 31 of the processed surface is exposed, resulting in defects and cannot be directly used as an appearance surface.
[0085] The housing provided in the present disclosure, such as Figure 3a As shown, when the shell provided by the present disclosure is applied to the back cover of a mobile terminal device, the back cover shell has a horizontal appearance surface and a vertical appearance surface, and the part to be processed 21 protrudes from the vertical appearance surface with a very small width. The redundant feature part on the part to be processed 21 can be cut off by CNC technology to obtain the final required back cover shell, such as Figure 4b As shown, the shell only has a very slight whitish position at the bottom edge, which does not affect the appearance surface of the rear cover shell in the first direction and the appearance surface of the rear cover shell in the second direction. When assembling the mobile terminal device, the appearance surface of the rear cover shell in the horizontal direction and the appearance surface in the vertical direction are directly used as the appearance surface of the mobile terminal device, which can ensure that the base material on the appearance surface is uniform and avoid unevenness caused by inconsistent materials or processing procedures; the processing surface of the rear cover shell is buried under the middle frame to cover the processing surface so that it is not exposed on the appearance surface of the mobile terminal device. In addition, burying the protruding processing surface under the middle frame can also make the rear cover shell directly fixed on the device body, making the connection between the rear cover and the device body more stable.
[0086] In an exemplary embodiment provided by the present disclosure, the shell includes: a preset number of layers of composite material plates; the composite material plates are stacked according to a preset rule.
[0087] The shell provided in this embodiment includes a preset number of layers of composite material plates, and the shapes and sizes of each composite material plate can be the same or different. For example, the shape of each composite material plate can be selected from a rectangle, a square, a rounded rectangle, and a rounded square to better meet the requirements of the appearance or mechanical properties of the shell in the application; the composite material plate has a higher modulus and better impact resistance than traditional plastic materials, and can better ensure the strength of the shell provided by the present disclosure.
[0088] The shell provided by the present disclosure is optimized by stacking composite material plates according to preset rules, for example, by changing the stacking angles between the composite material plates, so that the shell can meet the needs of various complex shapes, and can also avoid the problem of poor flatness caused by high local stress due to large changes in shape and size when preparing a shell with a complex appearance surface.
[0089] In the exemplary embodiment provided by the present disclosure, the composite material plates are stacked according to a preset rule, including:
[0090] The warp lines and / or weft lines of adjacent composite material panels form a second preset angle therebetween.
[0091] For example, adjacent composite panels are arranged at a second preset angle between the warps of adjacent composite panels; or adjacent composite panels are arranged at a second preset angle between the wefts of adjacent composite panels; or some composite panels are arranged at a second preset angle between the warps of adjacent composite panels, and the remaining composite panels are arranged at a second preset angle between the wefts of adjacent composite panels. The stacking directions between adjacent composite panels can be the same or different, and can be flexibly selected according to actual needs to meet different requirements of the shell, such as the shape, thickness or strength requirements of the shell.
[0092] In the exemplary embodiment of the present disclosure, Figure 6 As shown, Figure 6 The stacking method between any two adjacent layers of composite material plates in the shell is exemplarily shown in the figure, and the angle α between the warp 301 of the first composite material plate 300 and the warp 401 of the second composite material plate 400 can be used as the second preset angle. The angle β between the weft 302 of the first composite material plate 300 and the weft 402 of the second composite material plate 400 can also be used as the second preset angle. When multiple layers of composite material plates are stacked, some composite material plates can be arranged at the second preset angle between the warp lines of adjacent composite material plates, and the remaining composite material plates can be arranged at the second preset angle between the weft lines of adjacent composite material plates.
[0093] In an exemplary embodiment provided by the present disclosure, the second preset angle includes 0 to 90 degrees.
[0094] The shell provided by the present invention is optimized by stacking composite material plates according to preset rules, for example, by changing the stacking angle of the composite material plates, so that the composite material plates with different stacking angles can meet the appearance requirements of different shapes after being pressed into a shell, and can withstand stresses from different directions, so that the overall force strength of the shell is higher and the structure is more stable. At the same time, it can avoid the problem of poor flatness caused by high local stress due to large changes in shape and size of the shell with complex appearance.
[0095] In actual production and application, the second preset angle between adjacent composite material plates in the shell can be selected within the range of 0 to 90 degrees according to specific needs. For example, the second preset angle between adjacent composite material plates in the shell can be selected in combination with the number of layers of composite material plates in the shell, the appearance surface shape of the shell, the force direction and the degree of force. For example, the second preset angle can be in the range of 15 to 75 degrees. In an exemplary example of the present disclosure, the shell includes 6 layers of composite material plates, and the stacking angle between each composite material plate, that is, the warp and / or weft between adjacent composite material plates is "0 degrees / 45 degrees / 0 degrees / 45 degrees / 0 degrees / 45 degrees", and the second preset angle is 45 degrees. Or "0 degrees / 45 degrees / 45 degrees / 45 degrees / 45 degrees / 0 degrees", the second preset angle is 45 degrees and 0 degrees. Or the warp and / or weft between adjacent composite material plates is "0 degrees / 60 degrees / 60 degrees / 60 degrees / 60 degrees / 0 degrees", and the second preset angle is 0 degrees and 60 degrees. Or "0 degrees / 60 degrees / 0 degrees / 60 degrees / 0 degrees / 60 degrees", the second preset angle is 60 degrees. Or the warp and / or weft of adjacent composite panels are "0 degrees / 45 degrees / 15 degrees / 30 degrees / 60 degrees / 0 degrees", the second preset angle includes 45 degrees, 30 degrees, 15 degrees and 60 degrees. The second preset angles between adjacent composite panels can be the same or different, and can be flexibly selected according to actual needs, and the present disclosure does not limit it here.
[0096] In the exemplary embodiment provided in the present disclosure, the preset number of layers includes 5 to 8 layers.
[0097] The shell provided by the present disclosure limits the preset number of layers of the composite material plates to 5 to 8 layers. For example, the preset number of layers of the composite material plates can be 5 layers, 6 layers, 7 layers, or 8 layers. By stacking the composite material plates according to preset rules, for example, by changing the stacking angles between the composite material plates to perform stacking optimization, the composite material plates with different stacking angles can be pressed into a shell to meet the appearance requirements of different shapes, and the strength of the shell can be guaranteed, so that the overall force strength of the shell is high enough and the structure is stable enough under the complex appearance surface shape.
[0098] In an exemplary embodiment provided by the present disclosure, the composite material board includes a reinforced epoxy resin composite fiberglass board.
[0099] The shell provided by the present disclosure, the composite material board contained therein includes a reinforced epoxy resin composite glass fiber board. Among them, epoxy resin is a thermosetting resin, which has excellent mechanical properties, electrical insulation, and heat resistance. In addition, epoxy resin has low curing shrinkage and strong bonding force; glass fiber has the characteristics of non-flammability, heat insulation, high tensile strength, and good electrical insulation; the reinforced epoxy resin composite glass fiber board made of glass fiber as a reinforcing material and epoxy resin as an adhesive has strong mechanical properties and dielectric properties, and has good processability and flatness. The shell provided by the present disclosure includes a reinforced epoxy resin composite glass fiber board. In the process of preparing the shell, it is stacked in an "S"-shaped molding mold according to preset rules, and the stacked reinforced epoxy resin composite glass fiber board is hot-pressed in an "S"-shaped molding mold with preset conditions, so that the high-fluidity epoxy resin in the composite material board flows and fills, for example, fills the entire mold cavity, so that the final shell has a delicate and uniform appearance. In addition, since the reinforced epoxy resin composite glass fiber board itself has high strength and a modulus of more than 20GPa, the shell provided by the present invention can have high strength and impact resistance, avoiding the problem of shell deformation caused by stress concentration when the shell is subjected to force under complex shapes.
[0100] An exemplary embodiment of the present disclosure provides an electronic device, which includes the housing provided by the present disclosure.
[0101] The electronic device provided by the exemplary embodiment of the present disclosure includes the housing provided by the present disclosure, see Figure 2 As shown, the shell has a horizontal appearance surface and a vertical appearance surface, and the part to be processed (not shown in the figure) protrudes from the vertical appearance surface with a very small width, and the redundant feature part on the part to be processed can be cut off by CNC technology. When assembling a mobile terminal device, the horizontal appearance surface and the vertical appearance surface of the shell are directly used as the appearance surface of the electronic device to ensure that the base material on the appearance surface is uniform and consistent, avoiding unevenness caused by inconsistent materials or processing procedures; the processed part of the shell protruding from the vertical appearance surface is buried under the middle frame of the electronic device to cover the processed part so that it is not exposed on the appearance surface of the mobile terminal device. In addition, burying the protruding processing surface under the middle frame can also make the back cover shell directly fixed on the device body, making the connection between the back cover and the device body more stable.
[0102] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present disclosure, rather than to limit them. Although the present disclosure has been described in detail with reference to the above embodiments, a person skilled in the art should understand that the technical solutions described in the above embodiments can still be modified, or some of the technical features can be replaced by equivalents; and these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present disclosure.
Claims
1. A method for preparing a shell, It is characterized in that The preparation method comprises: Under preset conditions, the composite material plate to be hot-pressed is hot-pressed in a forming mold to form the shell, wherein the composite material plate includes a semi-solid composite material plate and the forming mold has a preset shape; the preset shape is configured so that, during the hot-pressing process, the molten resin in the composite material plate flows and fills the forming mold, so that the shell forms appearance surfaces in the first direction and the second direction.
2. The method for preparing the housing according to claim 1, It is characterized in that The preset shape includes an "S" shape.
3. The method for preparing the shell according to claim 2, It is characterized in that The first direction and the second direction form a first preset angle, and the first preset angle is greater than or equal to 60 degrees.
4. The method for preparing the shell according to claim 3, It is characterized in that The thickness of the shell in the second direction is greater than or equal to 0.5 mm.
5. The method for preparing the shell according to claim 4, It is characterized in that The width of the to-be-processed portion of the shell in the second direction is less than or equal to 0.3 mm.
6. The method for preparing the housing according to claim 1, It is characterized in that The method of hot-pressing the composite material plate to be hot-pressed in a forming mold under preset conditions to form the shell comprises: stacking a preset number of layers of composite material panels in the forming mold according to a preset rule; The shell is formed by hot pressing under preset conditions.
7. The method for preparing a shell according to any one of claims 1 to 6, It is characterized in that The preset conditions include: The molding pressure includes 15 to 25 MPa; the molding temperature includes 150 to 190° C.; and the molding time includes 5 to 15 minutes.
8. The method for preparing the housing according to claim 6, It is characterized in that The step of stacking a preset number of layers of composite material plates in the forming mold according to a preset rule comprises: The warp threads and / or weft threads of the adjacent composite material panels are stacked in the forming mold at a second preset angle.
9. The method for preparing the housing according to claim 8, It is characterized in that The second preset angle includes 0 to 90 degrees.
10. The method for preparing a housing according to claim 6, It is characterized in that The preset number of layers includes 5 to 8 layers.
11. A housing, It is characterized in that The shell is made according to the shell preparation method according to any one of claims 1-10.
12. An electronic device, It is characterized in that The electronic device comprises the housing according to claim 11.
Citation Information
Patent Citations
Manufacturing method of composite shell
CN108237704A