Flexible polymer optical fiber device with adjustable refractive index and preparation method and application thereof

Polymer optical fiber devices with adjustable refractive index are prepared by stretching and UV-curing NOA optical glue in flexible molds, which solves the problems of flexibility and difficulty in adjusting quartz optical fibers in short-distance communications and wearable devices, and achieves high flexibility. and low-cost optical fiber preparation suitable for wearable sensors and optical signal transmission.

CN118810091APending Publication Date: 2024-10-22HUZHOU COLLEGE
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410752019.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing quartz optical fibers have poor flexibility, difficult to adjust refractive index and size in short-distance communications and wearable devices, and the preparation process is complex and costly, making it difficult to meet the needs of optical fiber communication technology.

Method used

NOA optical glue is used to fill a flexible tubular mold for stretching and shaping, and polymer optical fiber devices with adjustable refractive index are prepared through UV curing, and a cladding is added to the core layer of the polymer optical fiber to improve adhesion.

Benefits of technology

A polymer optical fiber device with adjustable refractive index and size, high flexibility and low cost is realized, which is suitable for wearable sensing devices and optical signal communication transmission, and improves the surface finish and viscosity stability of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118810091A_ABST
    Figure CN118810091A_ABST
Patent Text Reader

Abstract

The invention provides a flexible polymer optical fiber device with an adjustable refractive index and a preparation method and application thereof. The preparation method of the flexible polymer optical fiber device comprises the following steps that (1) a capillary effect is adopted to enable NOA optical glue to be filled into a flexible tubular mold, stretching and shaping are conducted, a polymer optical fiber core layer is obtained, and the NOA optical glue is at least selected from two kinds of NOA optical glue with different refractive indexes; and (2) dipping the polymer optical fiber core layer in a mixed solution containing NOA glue and cyclopentane, and performing ultraviolet curing to obtain the flexible polymer optical fiber device. According to the invention, the NOA glue with the required refractive index is prepared, the small-size polymer optical fiber with controllable diameter and refractive index and high flexibility can be prepared by stretching and curing, and then the mixed solution of the NOA glue and cyclopentane on the surface of the core layer of the polymer optical fiber is subjected to ultraviolet curing, so that the surface smoothness of a polymer optical fiber device can be improved; and the internal stress of the curing layer can be reduced, and the viscosity stability and reliability are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of optical fiber device preparation, and in particular to a flexible polymer optical fiber device with adjustable refractive index, and a preparation method and application thereof. Background Art

[0002] With the rapid development of information technology, fiber optic communication, as a high-speed, high-capacity transmission method, plays a vital role in modern communication networks. Traditional quartz optical fiber has the advantages of low cost and low energy consumption, and has been widely used in the construction of long-distance communication network systems. However, in the field of short-distance communication, especially in the field of on-chip optical interconnection, quartz optical fiber is difficult to use in wearable devices due to its poor flexibility and fixed refractive index of the material. In addition, the refractive index and size of quartz optical fiber are fixed, making it difficult to customize in a low-cost manner. The preparation of quartz optical fiber mainly involves stretching the material from a molten state, and the material is strong and brittle after cooling.

[0003] At present, the technology for adjusting the refractive index of silica optical fiber usually adopts the ion doping method, while the engraving of the optical fiber microstructure relies on the photolithography process. These processes are complicated, require strict parameter control, and have a limited adjustment range of refractive index and size. In addition, these technologies have high requirements on the processing platform, expensive equipment, and high cost.

[0004] Based on the above problems, there is an urgent need for a low-cost, efficient preparation method with high flexibility, refractive index and adjustable size of optical fiber preparation process to meet the application of optical fiber communication technology in wearable sensor devices. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies of the prior art, the present invention provides a flexible polymer optical fiber device with adjustable refractive index and a preparation method and application thereof, which solves the problems raised in the above background technology.

[0007] (II) Technical solution

[0008] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0009] According to a first aspect of the present invention, there is provided a method for preparing a flexible polymer optical fiber device with adjustable refractive index, comprising the following steps:

[0010] (1) using a capillary effect to fill a flexible tubular mold with NOA optical glue, stretching, and shaping to obtain a polymer optical fiber core layer, wherein the NOA optical glue is selected from at least two NOA optical glues with different refractive indices;

[0011] (2) The polymer optical fiber core layer is immersed in a mixed solution containing NOA glue and cyclopentane, and ultraviolet curing is performed to obtain a flexible polymer optical fiber device.

[0012] Due to the development of polymer materials, polymer optical fibers have the advantages of flexibility, lightness, adjustable refractive index and resistance to electromagnetic interference. Polymers can not only be used to design on-chip waveguide arrays or inter-chip connections, but also their plasticity and dopability can be used to design optical fiber sensors. They have broad application prospects in short-distance communications, biomedicine and other fields.

[0013] In the present invention, NOA optical glue is used to mix to the required refractive index, and the polymer optical fiber with adjustable refractive index, high flexibility and low cost is prepared by stretching and shaping in a deformable mold. In addition, by curing a layer of polymer optical fiber cladding outside the polymer optical fiber core layer, the polymer optical fiber device can be tightly bonded to glass or electronic components, which has high practical value.

[0014] Preferably, in step (1), the NOA optical glue is selected from at least two of NOA61, NOA63, NOA65, NOA68, NOA71, NOA72, NOA73, NOA74, NOA75, NOA76, NOA78, NOA81, NOA83H, NOA84, NOA85, NOA86, NOA87, NOA88, and NOA89.

[0015] Preferably, in step (1), the inner diameter of the flexible tubular mold is 0.1-0.5 mm, the outer diameter of the flexible tubular mold is 1.0-1.5 mm, and the material of the flexible tubular mold is selected from at least one of silicone, PE or PU. Further preferably, the inner diameter of the flexible tubular mold is 0.2 mm, and the outer diameter is 1.2 mm.

[0016] Preferably, in step (1), the stretching length is 50 to 250% of the flexible tubular mold.

[0017] Preferably, in step (1), the shaping condition is: curing under ultraviolet light for 50 to 70 seconds. Further preferably, in step (1), the shaping condition is: curing under ultraviolet light for 60 seconds.

[0018] Preferably, in step (2), the mass ratio of the NOA glue to cyclopentane is 1 to 3:1, and further preferably, the mass ratio of the NOA glue to cyclopentane is 2:1.

[0019] Preferably, in step (2), the immersion time is 10 to 20 seconds, and more preferably, the immersion time is 15 seconds.

[0020] Preferably, in step (2), the UV curing time is 50 to 70 seconds, and further preferably, the UV curing time is 60 seconds.

[0021] In the above steps (1) and (2), the optimal wavelength of ultraviolet rays for ultraviolet curing is 350 to 380 nm.

[0022] According to a second aspect of the present invention, a flexible polymer optical fiber device with adjustable refractive index obtained according to the above preparation method is provided, comprising a polymer optical fiber core layer and a polymer optical fiber cladding coated on the surface of the polymer optical fiber core layer.

[0023] In the preparation of the present invention, the polymer optical fiber cladding coated on the surface of the polymer optical fiber core layer is sticky and can be adhered to glass or electronic components, which is easy to operate.

[0024] According to a third aspect of the present invention, there is provided a flexible polymer optical fiber device with adjustable refractive index for use as a bending sensor in a wearable sensor device.

[0025] (III) Beneficial effects

[0026] The present invention provides a flexible polymer optical fiber device with adjustable refractive index and a preparation method and application thereof. It has the following beneficial effects:

[0027] (1) The present invention provides a method for preparing a flexible polymer optical fiber device with adjustable refractive index. NOA glue with a desired refractive index is prepared, and after stretching and curing, a small-sized polymer optical fiber with controllable diameter and refractive index and high flexibility can be prepared. Then, the NOA glue and cyclopentane mixed solution on the surface of the polymer optical fiber core layer is ultraviolet-cured, which can not only improve the surface finish of the polymer optical fiber device, but also reduce the internal stress of the cured layer, thereby improving the stability and reliability of the viscosity.

[0028] (2) This scheme provides a flexible polymer optical fiber device with adjustable refractive index. The polymer core layer is wrapped with a polymer outer layer, which has high flexibility and high sensitivity. In addition, the surface of the polymer optical fiber is also sticky. It can not only be connected with traditional quartz optical fiber, but also adhere to glass or electronic components for optical signal communication transmission. The operation is simple and the results are accurate. It can even be used in wearable sensor devices such as human activity detection. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a process flow chart for preparing a NOA optical fiber core layer according to Example 1 of the present invention;

[0030] Among them, 1. mixed NOA glue; 2. silicone tube; 3. clamp; 4. silicone tube in stretched state; 5. UV curing lamp; 6. NOA optical fiber core layer. DETAILED DESCRIPTION

[0031] In order to better illustrate the content of the present invention, a detailed description is given below in conjunction with specific embodiments.

[0032] Example 1

[0033] In this embodiment, a polymer optical fiber with a refractive index of 1.5292 at 637 nm and a core diameter of 141.0 μm is prepared. The process flow is as follows: Figure 1 As shown:

[0034] Step 1, select two types of NOA65 glue and NOA68 glue with refractive indexes above and below the target refractive index, mix them in a mass ratio of 1:1, place them in a vacuum chamber and let them stand for 30 minutes to discharge bubbles in the liquid, and obtain mixed NOA glue 1;

[0035] Step 2, cut a silicone tube 2 with a length of 5 cm, an inner diameter of 0.2 mm, and an outer diameter of 1.2 mm and place it parallel to the desktop, with one end of the silicone tube 2 on the glass slide;

[0036] Step 3, draw 1 mL of mixed NOA glue 1 with a syringe, drop it on the end of the silicone tube 2 on the glass slide, and let it stand at room temperature for 60 minutes. Under the action of capillary effect, the mixed NOA glue 1 spontaneously fills the cavity of the silicone tube 2;

[0037] Step 4, clamp the two ends of the silicone tube 2 with the clip 3, stretch the filled silicone tube 2 to 250% of the original length and fix it, keep it stable for 1 minute, stably place the ultraviolet curing lamp 5 with a power of 35w and a wavelength of 365nm at a distance of 10cm from the silicone tube, irradiate the silicone tube 4 in the stretched state for shaping for 60s, cut one end of the silicone tube, and take it out with tweezers to obtain the cured NOA optical fiber core layer 6;

[0038] Step 5, preparing a diluent containing NOA65 glue and cyclopentane, wherein the mass ratio of NOA65 glue to cyclopentane is 2:1;

[0039] Step 6, immerse the NOA fiber core layer in a diluent containing NOA65 glue and cyclopentane for 15 seconds, take out the NOA fiber core layer and let it stand for 1 minute, and place it under a UV curing lamp with a wavelength of 365nm for 60 seconds to completely cure the polymer fiber cladding to obtain a polymer fiber device with a refractive index of 1.5292, such as Figure 1 shown.

[0040] Comparative Example 1

[0041] The preparation method of this comparative example is the same as that of Example 1, except that in step 6, the prepared NOA optical fiber core layer is immersed in a glue containing only NOA65 for 15 seconds, allowed to stand for 1 minute, and then irradiated under a UV curing lamp with a wavelength of 365nm for 60 seconds to obtain a polymer optical fiber device.

[0042] By comparing Example 1 with Comparative Example 1, it can be seen that during the preparation of the polymer optical fiber cladding, if cyclopentane is not added to dilute the NOA glue, the thickness of the polymer optical fiber cladding is uneven and the surface is not smooth.

[0043] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a flexible polymer optical fiber device with adjustable refractive index, characterized in that: The following steps are involved: (1) using a capillary effect to fill a flexible tubular mold with NOA optical glue, stretching, and shaping to obtain a polymer optical fiber core layer, wherein the NOA optical glue is selected from at least two NOA optical glues with different refractive indices; (2) The polymer optical fiber core layer is immersed in a mixed solution containing NOA glue and cyclopentane, and ultraviolet curing is performed to obtain a flexible polymer optical fiber device.

2. The method for preparing a flexible polymer optical fiber device with adjustable refractive index according to claim 1, characterized in that: In step (1), the NOA optical glue is selected from at least two of NOA61, NOA63, NOA65, NOA68, NOA71, NOA72, NOA73, NOA74, NOA75, NOA76, NOA78, NOA81, NOA83H, NOA84, NOA85, NOA86, NOA87, NOA88, and NOA89.

3. The method for preparing a flexible polymer optical fiber device with adjustable refractive index according to claim 1, characterized in that: In step (1), the inner diameter of the flexible tubular mold is 0.1-0.5 mm, the outer diameter of the flexible tubular mold is 1.0-1.5 mm, and the material of the flexible tubular mold is selected from at least one of silicone, PE or PU.

4. The method for preparing a flexible polymer optical fiber device with adjustable refractive index according to claim 1, characterized in that: In step (1), the stretching length is 50 to 250% of the flexible tubular mold.

5. The method for preparing a flexible polymer optical fiber device with adjustable refractive index according to claim 1, characterized in that: In step (1), the setting conditions are: curing under ultraviolet light for 50 to 70 seconds.

6. The method for preparing a flexible polymer optical fiber device with adjustable refractive index according to claim 1, characterized in that: In step (2), the mass ratio of the NOA glue to cyclopentane is 1 to 3:

1.

7. The method for preparing a flexible polymer optical fiber device with adjustable refractive index according to claim 1, characterized in that: In step (2), the immersion time is 10 to 20 seconds.

8. The method for preparing a flexible polymer optical fiber device with adjustable refractive index according to claim 1, characterized in that: In step (2), the UV curing time is 50 to 70 seconds.

9. A flexible polymer optical fiber device with adjustable refractive index obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The invention comprises a polymer optical fiber core layer and a polymer optical fiber cladding layer coated on the surface of the polymer optical fiber core layer.

10. Use of the flexible polymer optical fiber device with adjustable refractive index as claimed in claim 9 as a bending sensor in a wearable sensor device.

Citation Information

Patent Citations

  • Method for preparing a POF device

    LU509480B1