A high temperature piezoelectric ceramic for pressure sensor and preparation method thereof
By introducing doping of CaBi2Nb2O9 and BiTiO3 into high-temperature piezoelectric ceramic materials, combined with doping of Dy2O3, the problems of toxic oxidation and low piezoelectric properties of existing ceramics under high temperature conditions are solved, and high Curie temperature and good The ceramic material preparation with piezoelectric properties is suitable for pressure sensors and meets environmental and health requirements.
Patent Information
- Application Number
- CN202411271318.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-11
AI Technical Summary
Existing piezoelectric ceramic materials have problems of toxic lead oxide volatility and low piezoelectric properties under high temperature conditions, which limits their application under high temperature and high frequency conditions and poses a threat to the environment and human health.
High-temperature piezoelectric ceramic material with structural formula (1-x)(Bi2O2)2+ (Am-1BmO3m+1)2-x(BinCn-1)TiO3-αwt%Dy2O3 is adopted, and the mixed price of A and B positions of CaBi2Nb2O9 is passed. State ion doping, combined with the doping of BiTiO3 and Dy2O3, improves the piezoelectric properties of the material, and prepares ceramics with high Curie temperature and good piezoelectric properties through a specific sintering process.
It improves the piezoelectric properties and Curie temperature of the ceramic, reduces porosity, enhances density, is suitable for pressure sensors, and avoids the environmental and health hazards caused by the use of toxic lead oxide.
Smart Images

Figure CN118812261B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of piezoelectric ceramic materials, in particular to a high-temperature piezoelectric ceramic for a pressure sensor and a preparation method thereof. Background Art
[0002] As a type of piezoelectric material, piezoelectric ceramics are widely used in pressure sensors, ultrasonic transducers, piezoelectric transformers, audio transducers and other device fields. Compared with other piezoelectric materials, piezoelectric ceramics have the advantages of high electromechanical coupling coefficient, easy mass production and low preparation cost, so they play an important role in modern economy, construction and military defense.
[0003] Lead zirconate titanate PZT is a binary solid solution composed of antiferroelectric PbZrO3 and ferroelectric PbTiO3, with ABO3 perovskite structure. PZT piezoelectric ceramics have attracted widespread attention from the industry due to their high Curie temperature, low coercive field, and high piezoelectric performance. However, its main raw material, lead oxide, is toxic and volatile at high temperatures, so it will cause serious harm to human health and the environment during production, preparation, use and disposal. In order to meet people's requirements for health and environmental protection, the development of new lead-free piezoelectric ceramics has become a hot topic in the field of piezoelectric materials.
[0004] Bismuth layered piezoelectric ceramic materials have great potential for use under high temperature and high frequency conditions due to their advantages such as high Curie temperature, high resistivity, high dielectric breakdown strength, low dielectric constant, low aging rate, excellent fatigue resistance and large anisotropy. However, since their spontaneous polarization only rotates in two-dimensional directions, the piezoelectric properties of this series of materials are relatively low, which seriously limits their application. Summary of the invention
[0005] Purpose of the invention: In view of the above technical problems, the present invention proposes a high-temperature piezoelectric ceramic for a pressure sensor and a preparation method thereof.
[0006] The technical solutions adopted are as follows:
[0007] A high temperature piezoelectric ceramic for pressure sensor, the structural formula of which is as follows:
[0008] (1-x)(Bi2O2) 2+ (A m-1 B m O 3m+1 ) 2- -x(Bi n C n-1 )TiO3-αwt%Dy2O 3;
[0009] Where A is Na + , K + and Ca2+ ;
[0010] Among them, Na + , K + The molar ratio is 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1;
[0011] Na + , K + The molar ratio is preferably 1:1;
[0012] Ca 2+ with (Na + +K + )'s molar ratio is 95:5, 90:10, 85:15, 80:20, 75:25, 70:30, 65:35, 60:40, 55:45, 50:50;
[0013] Ca 2+ with (Na + +K + ) is preferably in a molar ratio of 85:15;
[0014] B is Nb 5+ and Ta 5+ ;
[0015] Nb 5+ and Ta 5+ The molar ratio is 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1;
[0016] Nb 5+ and Ta 5+ The molar ratio is preferably 9:1;
[0017] C is Li + ;
[0018] m is an integer between 1 and 4;
[0019] 0.4≤n≤0.6;
[0020] 0<x≤0.15;
[0021] 0.1≤α≤2.
[0022] Furthermore, m is 1, 2, 3, or 4, and m is preferably 2.
[0023] Further, 0.45≤n≤0.55;
[0024] n can be 0.45, 0.46, 0.47, 0.48, 0.49, 0.50, 0.51, 0.52, 0.53, 0.54, 0.55, which are only for the convenience of understanding and are not intended to be limiting;
[0025] Furthermore, n=0.5.
[0026] Furthermore, 0.05≤x≤0.1, 0.5≤α≤1.5.
[0027] x can be 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, which are only for the convenience of understanding and are not intended to be limiting;
[0028] α can be 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, which are only for the convenience of understanding and are not intended to be limiting;
[0029] Furthermore, x=0.08, α=1.
[0030] The present invention also provides a method for preparing high-temperature piezoelectric ceramics for pressure sensors:
[0031] Bi2O3, oxide A and oxide B are mixed and ball-milled, dried and pre-calcined at 600-800°C to obtain a first pre-calcined product;
[0032] The Bi2O3, C oxide and TiO2 are mixed and ball-milled, dried and pre-calcined at 700-900°C to obtain a second pre-calcined product;
[0033] The first pre-calcined product, the second pre-calcined product and Dy2O3 are mixed again, ball-milled and dried, granulated, pressed, debinded, and finally sintered at 1050-1200°C for 1-4h.
[0034] Beneficial effects of the present invention:
[0035] The present invention provides a high-temperature piezoelectric ceramic for a pressure sensor, wherein the piezoelectric performance of CaBi2Nb2O9 is improved by doping CaBi2Nb2O9 with mixed valence ions at the A and B positions. The reason may be that the doping of ions with different ionic radii causes the NbO6 octahedron to be distorted, thereby improving the piezoelectric performance.
[0036] BiTiO3 is a perovskite structure compound. The introduction of alkali metal-doped BiTiO3 in the present application can lead to lattice distortion and a decrease in the concentration of oxygen vacancies generated by Bi volatilization, thereby weakening the pinning effect, increasing the number of reversible domains, and improving the polarizability and piezoelectric activity of the piezoelectric ceramic material, thereby achieving the effect of improving its piezoelectric performance.
[0037] Appropriate amount of Dy2O3 doping can refine the grain size, reduce the porosity of high-temperature piezoelectric ceramics, improve the density, and facilitate the optimization of its piezoelectric properties;
[0038] The high-temperature piezoelectric ceramics prepared by the present invention have a high Curie temperature (about 700°C) and good piezoelectric properties (piezoelectric constant d 33 At around 30pC / N), the piezoelectric performance is significantly improved compared to the current conventional bismuth layered piezoelectric ceramic materials, and can be used to make pressure sensors. Moreover, its preparation raw materials do not contain toxic lead oxide, so it will not cause harm to human health and the environment during the production, preparation, use and waste recycling process, meeting the health and environmental protection requirements of modern society. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a SEM photograph of the polished and hot-corroded surface of the high-temperature piezoelectric ceramic in Example 1. It can be seen that the internal density is relatively high and no obvious pores are observed. DETAILED DESCRIPTION
[0040] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.
[0041] Embodiment 1:
[0042] This embodiment provides a high temperature piezoelectric ceramic for a pressure sensor, and its structural formula is as follows:
[0043] 0.92(Na 0.5 K 0.5 ) 0.15 Ca 0.85 Bi 1.8 Ta 0.2 O9-0.08(Bi 0.5 Li 0.5 )TiO3-1wt%Dy2O 3;
[0044] The preparation method of the high temperature piezoelectric ceramic for the pressure sensor is as follows:
[0045] Bi2O3, Na2CO3, K2CO3, CaCO3, Nb2O5 and Ta2O5 are mixed and added into a ball mill, anhydrous ethanol is used as the ball milling medium, the mixture is ball milled for 10 hours on a planetary ball mill, dried, placed in a mold and pressed into sheets at 10 MPa, and then heated to 800°C at a speed of 5°C / min and pre-calcined for 2 hours. After the pre-calcination, the product is crushed to obtain a first pre-calcined product;
[0046] Bi2O3, Li2CO3 and TiO2 are mixed and added into a ball milling jar, and anhydrous ethanol is used as the ball milling medium. After the mixture is ball milled for 10 hours on a planetary ball mill, it is dried, placed in a mold and pressed into a sheet at 10 MPa, and then heated to 850°C at a rate of 5°C / min and pre-calcined for 2 hours. After the pre-calcination, the product is crushed to obtain a second pre-calcined product.
[0047] The first pre-calcined product, the second pre-calcined product and Dy2O3 are mixed and added into a ball mill. Anhydrous ethanol is used as the ball milling medium. The mixture is ball milled again on a planetary ball mill for 10 hours and then dried. A 10wt% concentration of PVA solution is added as a binder to form granules. The granules are passed through a 120-mesh sieve and placed in a mold and pressed into a billet at a pressure of 100 MPa. The billet is heated to 650°C at a rate of 1°C / min and kept for 1 hour to debind, then the temperature is continued to be raised to 1080°C and kept for sintering for 4 hours.
[0048] Embodiment 2:
[0049] This embodiment provides a high temperature piezoelectric ceramic for a pressure sensor, and its structural formula is as follows:
[0050] 0.92CaBi2Nb 1.8 Ta 0.2 O9-0.08(Bi 0.5 Li 0.5 )TiO3-1wt%Dy2O 3;
[0051] The preparation method of the high temperature piezoelectric ceramic for the pressure sensor is as follows:
[0052] Bi2O3, CaCO3, Nb2O5 and Ta2O5 are mixed and added into a ball mill, anhydrous ethanol is used as the ball milling medium, the mixture is ball milled for 10 hours on a planetary ball mill, dried, placed in a mold and pressed into sheets at 10 MPa, and then heated to 800°C at a rate of 5°C / min for pre-calcination for 2 hours. After the pre-calcination, the product is crushed to obtain a first pre-calcined product;
[0053] Bi2O3, Li2CO3 and TiO2 are mixed and added into a ball milling jar, and anhydrous ethanol is used as the ball milling medium. After the mixture is ball milled for 10 hours on a planetary ball mill, it is dried, placed in a mold and pressed into a sheet at 10 MPa, and then heated to 850°C at a rate of 5°C / min and pre-calcined for 2 hours. After the pre-calcination, the product is crushed to obtain a second pre-calcined product.
[0054] The first pre-calcined product, the second pre-calcined product and Dy2O3 are mixed and added into a ball mill. Anhydrous ethanol is used as the ball milling medium. The mixture is ball milled again on a planetary ball mill for 10 hours and then dried. A 10wt% concentration of PVA solution is added as a binder to form granules. The granules are passed through a 120-mesh sieve and placed in a mold and pressed into a billet at a pressure of 100 MPa. The billet is heated to 650°C at a rate of 1°C / min and kept for 1 hour to debind, then the temperature is continued to be raised to 1080°C and kept for sintering for 4 hours.
[0055] Embodiment 3:
[0056] This embodiment provides a high temperature piezoelectric ceramic for a pressure sensor, and its structural formula is as follows:
[0057] 0.92Na 0.15 Ca 0.85 Bi 1.8 Ta 0.2 O9-0.08(Bi 0.5 Li 0.5 )TiO3-1wt%Dy2O 3;
[0058] The preparation method of the high temperature piezoelectric ceramic for the pressure sensor is as follows:
[0059] Bi2O3, Na2CO3, CaCO3, Nb2O5 and Ta2O5 are mixed and added into a ball mill, anhydrous ethanol is used as the ball milling medium, the mixture is ball milled for 10 hours on a planetary ball mill, dried, placed in a mold and pressed into sheets at 10 MPa, and then heated to 800°C at a speed of 5°C / min for pre-calcination for 2 hours. After the pre-calcination, the product is crushed to obtain a first pre-calcined product;
[0060] Bi2O3, Li2CO3 and TiO2 are mixed and added into a ball milling jar, and anhydrous ethanol is used as the ball milling medium. After the mixture is ball milled for 10 hours on a planetary ball mill, it is dried, placed in a mold and pressed into a sheet at 10 MPa, and then heated to 850°C at a rate of 5°C / min and pre-calcined for 2 hours. After the pre-calcination, the product is crushed to obtain a second pre-calcined product.
[0061] The first pre-calcined product, the second pre-calcined product and Dy2O3 are mixed and added into a ball mill. Anhydrous ethanol is used as the ball milling medium. The mixture is ball milled again on a planetary ball mill for 10 hours and then dried. A 10wt% concentration of PVA solution is added as a binder to form granules. The granules are passed through a 120-mesh sieve and placed in a mold and pressed into a billet at a pressure of 100 MPa. The billet is heated to 650°C at a rate of 1°C / min and kept for 1 hour to debind, then the temperature is continued to be raised to 1080°C and kept for sintering for 4 hours.
[0062] Embodiment 4:
[0063] This embodiment provides a high temperature piezoelectric ceramic for a pressure sensor, and its structural formula is as follows:
[0064] 0.92K 0.15 Ca 0.85 Bi 1.8 Ta 0.2 O9-0.08(Bi 0.5 Li 0.5 )TiO3-1wt%Dy2O 3;
[0065] The preparation method of the high temperature piezoelectric ceramic for the pressure sensor is as follows:
[0066] Bi2O3, K2CO3, CaCO3, Nb2O5 and Ta2O5 are mixed and added into a ball mill, anhydrous ethanol is used as the ball milling medium, the mixture is ball milled for 10 hours on a planetary ball mill, dried, placed in a mold and pressed into sheets at 10 MPa, and then heated to 800°C at a rate of 5°C / min for pre-calcination for 2 hours. After the pre-calcination, the product is crushed to obtain a first pre-calcined product;
[0067] Bi2O3, Li2CO3 and TiO2 are mixed and added into a ball milling jar, and anhydrous ethanol is used as the ball milling medium. After the mixture is ball milled for 10 hours on a planetary ball mill, it is dried, placed in a mold and pressed into a sheet at 10 MPa, and then heated to 850°C at a rate of 5°C / min and pre-calcined for 2 hours. After the pre-calcination, the product is crushed to obtain a second pre-calcined product.
[0068] The first pre-calcined product, the second pre-calcined product and Dy2O3 are mixed and added into a ball mill. Anhydrous ethanol is used as the ball milling medium. The mixture is ball milled again on a planetary ball mill for 10 hours and then dried. A 10wt% concentration of PVA solution is added as a binder to form granules. The granules are passed through a 120-mesh sieve and placed in a mold and pressed into a billet at a pressure of 100 MPa. The billet is heated to 650°C at a rate of 1°C / min and kept for 1 hour to debind, then the temperature is continued to be raised to 1080°C and kept for sintering for 4 hours.
[0069] Embodiment 5:
[0070] This embodiment provides a high temperature piezoelectric ceramic for a pressure sensor, and its structural formula is as follows:
[0071] 0.92(Na 0.5 K 0.5 ) 0.15 Ca 0.85 Bi2Nb2O9-0.08(Bi 0.5 Li 0.5 )TiO3-1wt%Dy2O 3;
[0072] The preparation method of the high temperature piezoelectric ceramic for the pressure sensor is as follows:
[0073] Bi2O3, Na2CO3, K2CO3, CaCO3 and Nb2O5 are mixed and added into a ball mill, anhydrous ethanol is used as the ball milling medium, the mixture is ball milled for 10 hours on a planetary ball mill, dried, placed in a mold and pressed into sheets at 10 MPa, and then heated to 800°C at a rate of 5°C / min for pre-calcination for 2 hours. After the pre-calcination, the product is crushed to obtain a first pre-calcined product;
[0074] Bi2O3, Li2CO3 and TiO2 are mixed and added into a ball milling jar, and anhydrous ethanol is used as the ball milling medium. After the mixture is ball milled for 10 hours on a planetary ball mill, it is dried, placed in a mold and pressed into a sheet at 10 MPa, and then heated to 850°C at a rate of 5°C / min and pre-calcined for 2 hours. After the pre-calcination, the product is crushed to obtain a second pre-calcined product.
[0075] The first pre-calcined product, the second pre-calcined product and Dy2O3 are mixed and added into a ball mill. Anhydrous ethanol is used as the ball milling medium. The mixture is ball milled again on a planetary ball mill for 10 hours and then dried. A 10wt% concentration of PVA solution is added as a binder to form granules. The granules are passed through a 120-mesh sieve and placed in a mold and pressed into a billet at a pressure of 100 MPa. The billet is heated to 650°C at a rate of 1°C / min and kept for 1 hour to debind, then the temperature is continued to be raised to 1080°C and kept for sintering for 4 hours.
[0076] Comparative Example 1:
[0077] The same as Example 1, except that BiTiO3 is used instead of (Bi 0.5 Li 0.5 )TiO3.
[0078] This comparative example provides a high-temperature piezoelectric ceramic for a pressure sensor, and its structural formula is as follows:
[0079] 0.92(Na 0.5 K 0.5 ) 0.15 Ca 0.85 Bi 1.8 Ta 0.2 O9-0.08BiTiO3-1wt%Dy2O3
[0080] The preparation method of the high temperature piezoelectric ceramic for the pressure sensor is as follows:
[0081] Bi2O3, Na2CO3, K2CO3, CaCO3, Nb2O5 and Ta2O5 are mixed and added into a ball mill, anhydrous ethanol is used as the ball milling medium, the mixture is ball milled for 10 hours on a planetary ball mill, dried, placed in a mold and pressed into sheets at 10 MPa, and then heated to 800°C at a speed of 5°C / min and pre-calcined for 2 hours. After the pre-calcination, the product is crushed to obtain a first pre-calcined product;
[0082] Bi2O3 and TiO2 are mixed and added into a ball milling jar, anhydrous ethanol is used as the ball milling medium, ball milled for 10 hours on a planetary ball mill, dried, placed in a mold and pressed into sheets at 10 MPa, and then heated to 850°C at a rate of 5°C / min for 2 hours. After the pre-burning, the product is crushed to obtain a second pre-burned product;
[0083] The first pre-calcined product, the second pre-calcined product and Dy2O3 are mixed and added into a ball mill. Anhydrous ethanol is used as the ball milling medium. The mixture is ball milled again on a planetary ball mill for 10 hours and then dried. A 10wt% concentration of PVA solution is added as a binder to form granules. The granules are passed through a 120-mesh sieve and placed in a mold and pressed into a billet at a pressure of 100 MPa. The billet is heated to 650°C at a rate of 1°C / min and kept for 1 hour to debind, then the temperature is continued to be raised to 1080°C and kept for sintering for 4 hours.
[0084] Comparative Example 2: The same as Example 1, except that (Bi 0.5 Li 0.5 )TiO3.
[0085] Comparative Example 3: Basically the same as Example 1, except that Dy2O3 is not added.
[0086] Performance test: The high-temperature piezoelectric ceramics prepared in Examples 1-5 and Comparative Examples 1-3 of the present invention were polished and then silvered, and polarized in an electric field of 7 kV / mm for 15 min in silicone oil at 100°C and then left for one day as test samples;
[0087] The high temperature dielectric temperature spectrum test system (GJW-I) was used to measure the change of the dielectric constant of the sample with temperature, and the Curie temperature Tc was determined. The ZJ-3A quasi-static d 33 The piezoelectric constant d of the test specimen is measured by the measuring instrument 33 The measurement frequency is 110 Hz, and the Agilent 4294A precision impedance analyzer is used to measure the electrical properties of the sample, such as the mechanical quality factor Qm and the planar electromechanical coupling coefficient kp.
[0088] The test results are shown in Table 1 below:
[0089] ;
[0090] It can be seen from Table 1 above that the high-temperature piezoelectric ceramics prepared by the present invention have a relatively high Curie temperature and good piezoelectric properties, and can be used to make pressure sensors;
[0091] By comparing the data of Example 1 with that of Comparative Example 1, it can be seen that the Li + Doping, and the obtained (Bi 0.5 Li 0.5 ) The introduction of TiO3 into the high temperature piezoelectric ceramic of the present invention improves its Curie temperature and piezoelectric properties to a certain extent;
[0092] By comparing the data of Example 1 with those of Comparative Examples 2 and 3, it can be seen that the high temperature piezoelectric ceramics of the present invention (Bi 0.5 Li 0.5 Although the introduction of TiO3 and Dy2O3 will cause a slight decrease in the Curie temperature, the piezoelectric performance is significantly improved. Overall, it plays a positive role in improving its performance.
[0093] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high temperature piezoelectric ceramic for a pressure sensor, characterized in that: Its structural formula is as follows: (1-x)(Bi2O2) 2+ (A m-1 B m O 3m+1 ) 2- -x(Bi n C 1-n )TiO3-αwt%Dy2O 3; Where A is Na + With K + Any one or both of these and Ca 2+ combination of; B is Nb 5+ and Ta 5+ ; C + ; m is 2; 0.4≤n≤0.6; 0<x≤0.15; 0.1≤α≤2。 2. The high temperature piezoelectric ceramic for pressure sensor according to claim 1, characterized in that: 0.45≤n≤0.55。 3. The high temperature piezoelectric ceramic for pressure sensor according to claim 1, characterized in that: n=0.5。 4. The high temperature piezoelectric ceramic for pressure sensor according to claim 1, characterized in that: 0.05≤x≤0.1,0.5≤α≤1.5。 5. The high temperature piezoelectric ceramic for pressure sensor according to claim 1, characterized in that: x=0.08,α=1。 6. A method for preparing a high temperature piezoelectric ceramic for a pressure sensor according to any one of claims 1 to 5, characterized in that: Bi2O3, oxide A and oxide B are mixed and ball-milled, dried and pre-calcined at 600-800°C to obtain a first pre-calcined product; The Bi2O3, C oxide and TiO2 are mixed and ball-milled, dried and pre-calcined at 700-900°C to obtain a second pre-calcined product; The first pre-calcined product, the second pre-calcined product and Dy2O3 are mixed again, ball-milled and dried, granulated, pressed, debinded, and finally sintered at 1050-1200°C for 1-4h.
Citation Information
Patent Citations
A modified CaBi₂Nb₂O₉ bismuth layered piezoelectric ceramic material and its preparation method
CN102260080A
Piezoelectric ceramic material in bismuth laminar composite structure and preparation method of piezoelectric ceramic material