Method and system for recovering glycollic acid crystals by using waste degradable plastics

By using Al2O3-doped SO42-/Ti02 solid super acid catalyst in waste degradable plastics for hydrolysis reaction, the problems of low selectivity and low purity of glycolic acid recovery in the existing technology are solved, and the recovery of high-purity glycolic acid is achieved. , has economic and environmental advantages.

CN118812342AInactive Publication Date: 2024-10-22MADIGREE (SHANGHAI) MATERIALS TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410752207.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, the recovery of glycolic acid from polyglycolic acid copolymer blends has problems such as low selectivity, low product purity, and uneconomical and environmentally friendly methods.

Method used

Use waste degradable plastics for selective hydrolysis reaction, use Al2O3 doped SO42-/Ti02 solid super acid catalyst, and perform hydrolysis under normal pressure conditions of 293.15K ~ 353.15K to obtain high-purity glycolic acid crystals.

Benefits of technology

It achieves high-value glycolic acid recovery with a purity greater than 99.5wt%, does not contain CI- and Fe2+, has mild reaction conditions and does not require organic solvents. It has the advantages of economy, green and environmental protection, and solves the difficulty of processing and recycling waste degradable materials. Reuse issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118812342A_ABST
    Figure CN118812342A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of polyglycolic acid recovery, in particular to a method and a system for recovering glycolic acid crystals by adopting waste degradable plastics. According to the method, the waste degradable plastic containing polyglycolic acid is selectively hydrolyzed by adopting an A < l > 2O3 doped SO4 < 2-> / T < i02 > solid superacid catalyst, and high-quality glycolic acid crystals are obtained. The method is high in hydrolysis selectivity, mild in reaction condition and large in processable analysis amount range, and the finally obtained glycollic acid crystal is high in purity and good in quality. The method does not use an organic solvent, is wide in raw material source, and has the advantages of economy and environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polyglycolic acid recovery, and in particular to a method and system for recovering glycolic acid crystals by using waste degradable plastics. Background Art

[0002] Biodegradable materials will degrade and age over time, and products that have exceeded their shelf life cannot be used. After products containing polyglycolic acid are discarded, waiting for them to degrade naturally is not only a long process, but also a waste of resources.

[0003] Glycolic acid is an industrial product with a wide range of uses. Specifically, it can be used as a cosmetic additive or electronic-grade detergent. It can also be used as a raw material for high-strength fully biodegradable material polyglycolic acid, which is used in the medical and other industries and has high commercial value.

[0004] In the prior art, the production processes of glycolic acid mainly include chloroacetic acid hydrolysis method, formaldehyde carbonylation method and polyester hydrolysis method, and these processes all have many disadvantages.

[0005] For example, when chloroacetic acid is hydrolyzed to produce glycolic acid, the yield of glycolic acid prepared by chloroacetic acid hydrolysis catalyzed by sodium hydroxide can reach more than 95%, and the product mass fraction can reach more than 98%. However, oxyacetic acid is highly toxic and corrosive, which is not conducive to environmental protection, and the obtained product contains chloride ions, which makes the quality of glycolic acid low. For another example, the formaldehyde carbonylation method uses formaldehyde, CO and water to synthesize glycolic acid under the action of a catalyst. This method has high requirements for equipment and complex separation and purification methods for the product.

[0006] The polyester hydrolysis method has a long reaction time and a low conversion rate, and the catalysts commonly used in this method are tin halides, organic acid compounds, antimony oxides, halides or organic acid compounds, zinc oxides, halides, organic compounds or complexes, organic aluminum compounds or aluminum complexes, and rare earth metal complexes, etc. Among the catalysts used in the polyglycolic acid hydrolysis reaction, tin catalysts have high activity, but as heavy metal compounds, their dosage is limited. If strong acid catalysis is used, the selectivity will be reduced and other monomer impurities will be generated.

[0007] There is no solution in the prior art for recovering glycolic acid from polyglycolic acid copolymer blends with high selectivity. Summary of the invention

[0008] The technical problem to be solved by the present invention is to provide a method and system for recovering glycolic acid crystals using waste biodegradable plastics, so as to solve the problems of low selectivity, low product purity and uneconomical and environmentally unfriendly methods in the prior art for recovering glycolic acid from polyglycolic acid copolymer blends.

[0009] The technical solution of the present invention to solve the above technical problems is as follows:

[0010] The present invention provides a method for recovering glycolic acid crystals by using waste degradable plastics, wherein the waste degradable plastics include polyglycolic acid, and the method comprises the following steps:

[0011] S1, crushing and obtaining the powder of the waste biodegradable plastic;

[0012] S2, mixing the powder with water and a catalyst and stirring, and performing a selective hydrolysis reaction at a temperature of 293.15K to 353.15K under normal pressure to obtain a hydrolysis product containing glycolic acid; the reaction time is 1 to 3 hours; the catalyst is Al2O3-doped SO4 2- / TiO2 solid superacid catalyst;

[0013] S3, post-treating the hydrolyzate to obtain glycolic acid crystals.

[0014] Based on the above technical solution, the present invention can also be improved as follows.

[0015] Furthermore, in the catalyst, the molar percentage of Al2O3 is 0.1% to 99%.

[0016] Furthermore, the preparation method of the catalyst is to use Ti compound, AI(NO3)3·9H20 and concentrated ammonia water to react to obtain a mixed hydroxide precipitate; after centrifuging, washing, filtering and drying the mixed hydroxide precipitate with ammonium acetate solution, immersing it in 0.3-3 mol / L H2S04, and then filtering, drying, and calcining in a static air atmosphere in sequence to obtain the Al2O3-doped SO4 2- / Ti02 solid superacid catalyst.

[0017] Furthermore, the Ti compound is one of TiCl4, TiBr4, tetramethyl titanate, tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate, tetrabutyl titanate, tetrastearate titanate, tetra(2-ethylhexyl) titanate, and titanium tetramethacrylate.

[0018] Furthermore, in the step S1, the particle size of the powder is 0.1 to 1 mm.

[0019] Furthermore, in the step S2, the mass ratio of water to the powder is 1:(1-20), and the mass of the catalyst is 0.2-7wt% of the mass of the powder.

[0020] Furthermore, the post-treatment includes filtering, concentrating, crystallizing and drying the hydrolyzate.

[0021] Furthermore, the concentration is evaporation concentration, and the crystallization is cooling crystallization.

[0022] Furthermore, the components of the waste biodegradable plastics also include one or more of PBAT, PLA, PCL, PHA, PBS, talcum powder, calcium carbonate, and bentonite.

[0023] The present invention also provides a system for recovering glycolic acid crystals using waste biodegradable plastics, comprising a crushing unit, a hydrolysis unit, a first solid-liquid separation unit, an evaporation crystallization unit and a second solid-liquid separation unit connected in sequence; the crushing unit is used to crush the waste biodegradable plastics, the hydrolysis unit is used to perform a selective hydrolysis reaction on the crushed waste biodegradable plastics, the first solid-liquid separation unit is used to filter the hydrolysis product, the evaporation crystallization unit is used for evaporation concentration and crystallization, and the second solid-liquid separation unit is used to recover the glycolic acid crystals.

[0024] The beneficial effects of the present invention are:

[0025] (1) The method of recycling glycolic acid crystals from waste biodegradable plastics of the present invention uses Al2O3-doped SO4 2- / TiO2 solid superacid catalyst selectively hydrolyzes waste biodegradable plastics containing polyglycolic acid, converting them into glycolic acid crystals to achieve high-value recovery;

[0026] (2) The method of the present invention for recovering glycolic acid crystals from waste biodegradable plastics does not require the use of organic solvents, and the reaction conditions are mild and easy to implement;

[0027] (3) The method of recycling glycolic acid crystals from waste biodegradable plastics of the present invention can process polyglycolic acid with a molecular weight of 100,000 to 200,000, and the purity of the obtained polyglycolic acid crystals is greater than 99.5 wt %, and the crystals do not contain CI - , Fe 2+ , high crystal quality;

[0028] (4) The method of recovering glycolic acid crystals from waste biodegradable plastics of the present invention has a wide range of raw material sources and is not limited to raw materials such as chloroacetic acid and formaldehyde from traditional chemical routes, so it has a wide range of application prospects;

[0029] (5) The method of recycling glycolic acid crystals from waste biodegradable plastics of the present invention can solve the problem that waste biodegradable material products that have exceeded their shelf life are difficult to handle and recycle, and has the advantages of being economical and environmentally friendly;

[0030] (5) The method of recovering glycolic acid crystals from waste biodegradable plastics of the present invention uses waste biodegradable plastics as raw materials for preparing glycolic acid crystals, thereby greatly reducing the preparation cost of glycolic acid;

[0031] (6) The system for recovering glycolic acid crystals using waste biodegradable plastics of the present invention can use waste biodegradable plastics to prepare glycolic acid crystals, thereby achieving high-value recovery of glycolic acid. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a schematic diagram of the system structure for recycling glycolic acid crystals using waste biodegradable plastics according to the present invention;

[0033] Figure 2 In the method of the present invention for recovering glycolic acid crystals from waste biodegradable plastics, the measured 27 Al MAS NMR spectrum. DETAILED DESCRIPTION

[0034] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0035] The method for recovering glycolic acid crystals by using waste biodegradable plastics of the present invention, wherein the waste biodegradable plastics include polyglycolic acid, comprises the following steps:

[0036] S1, crushing and obtaining powder of waste biodegradable plastic;

[0037] S2. Mix the powder with water and the catalyst and stir, and carry out a selective hydrolysis reaction at a temperature of 293.15K to 353.15K under normal pressure to obtain a hydrolysis product containing glycolic acid; the reaction time is 1 to 3 hours; the catalyst is Al2O3-doped SO4 2- / TiO2 solid superacid catalyst;

[0038] S3. Post-treating the hydrolyzate to obtain glycolic acid crystals.

[0039] The method for recovering glycolic acid crystals by using waste degradable plastics of the present invention adopts Al2O3 doped SO4 2- / TiO2 solid superacid catalyst selectively hydrolyzes waste biodegradable plastics containing polyglycolic acid, which can be converted into glycolic acid crystals to achieve high-value recovery; this method does not require the use of organic solvents, the reaction conditions are mild and easy to implement, and the molecular weight Mn of polyglycolic acid that can be processed can reach 100,000 to 200,000. The purity of the obtained polyglycolic acid crystals is greater than 99.5wt%, and the crystals do not contain CI - , Fe 2+ , the crystal quality is high.

[0040] SO4 2- / M x O ySolid acid catalysts have the advantages of no corrosion to equipment, little pollution, high temperature resistance, good water stability and reusability. They can react at lower temperatures and have the advantages of both the reproducibility of heterogeneous catalysts and the high activity and selectivity of liquid superacids. The Al2O3-doped SO4 2- / TiO2 solid superacid catalyst, selectivity greater than 99.5%.

[0041] The method of recycling glycolic acid crystals from waste biodegradable plastics of the present invention has a wide range of raw materials and is not limited to raw materials such as chloroacetic acid and formaldehyde from traditional chemical routes. The method can solve the problem that waste biodegradable material products that have exceeded their shelf life are difficult to handle and recycle, and has the advantages of being economical and environmentally friendly.

[0042] Preferably, the present invention uses Al2O3 doped SO4 2- / Ti02 solid superacid catalyst, wherein the molar percentage of Al2O3 is 0.1% to 99%.

[0043] Preferably, the Al2O3-doped SO4 2- The preparation method of the Al2O3 / TiO2 solid superacid catalyst comprises the following steps: using a Ti compound, Al(NO3)3·9H20 and concentrated ammonia water to react to obtain a mixed hydroxide precipitate; using an ammonium acetate solution to centrifuge, wash, filter and dry the mixed hydroxide precipitate, and then immerse it in 0.3-3 mol / L H2S04, and then filtering, drying and calcining in a static air atmosphere in turn to obtain Al2O3-doped SO4 2- / Ti02 solid superacid catalyst.

[0044] Further preferably, the specific preparation method of the above catalyst is to dissolve the Ti compound and AI(NO3)3·9H20 in water, slowly add concentrated ammonia water under strong stirring until the pH value of the solution is 9-10, and then age at room temperature for 12-36 hours to obtain a mixed hydroxide precipitate; after eluting the mixed hydroxide precipitate with a 4% ammonium acetate solution by mass, centrifuge, wash, filter, dry at 373K for 12-36 hours, and then soak in 0.3-3 mol / L H2S04 for 0.5-2 hours, with a liquid-solid ratio of 15mL / g. Continue to filter and dry at 373K for 12-36 hours, and then calcine in a static air atmosphere at 773K-873K for 2-4 hours to obtain the Al2O3-doped SO4 2- / Ti02 solid superacid catalyst. Compared with direct treatment with sulfuric acid, the catalyst washed and precipitated with ammonium acetate has a larger specific surface area, smaller crystals and more acidic sites.

[0045] Preferably, the Ti compound is an inorganic titanium halide or a tetraalkoxy titanium compound.

[0046] More preferably, the Ti compound is one of TiCl4, TiBr4, tetramethyl titanate, tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate, tetrabutyl titanate, tetrastearate titanate, tetra(2-ethylhexyl) titanate, and titanium tetramethacrylate.

[0047] Preferably, in the method of the present invention, in step S1, the particle size of the powder is 0.1 to 1 mm; processing the raw material into a powder of this fineness can make its hydrolysis reaction more complete, which can further improve the recovery rate of glycolic acid crystals.

[0048] Preferably, in step S1, stirring is continued during the reaction process.

[0049] Preferably, in step S2, the reaction formula of the selective hydrolysis reaction is as shown in formula (1):

[0050]

[0051] In the above reaction, the mass ratio of water to polyglycolic acid powder is 1:(1-20), Al2O3 doped SO4 2- / TiO2 solid superacid catalyst mass is 0.2 to 7wt% of the powder mass; further preferably, Al2O3 doped SO4 2- The mass of the / TiO2 solid superacid catalyst is 1 to 5wt% of the powder mass; this ratio can make the hydrolysis reaction more efficient.

[0052] In the method of the present invention, the post-treatment includes filtering, concentrating, crystallizing and drying the hydrolyzate to improve the purity of the glycolic acid crystals and achieve a good recovery effect.

[0053] Preferably, the concentration is evaporation concentration, and the temperature of evaporation concentration is 293.15K to 363.15K, and more preferably, the temperature of evaporation concentration is 313.15K to 358.15K; further preferably, 323.15K to 353.15K is preferred. The pressure of evaporation concentration is 1kPa to 101.3kPa, and more preferably, the pressure of evaporation concentration is 10 to 90kPa; further preferably, 20 to 80kPa is preferred. The time of evaporation concentration is 2 to 4h.

[0054] Preferably, the crystallization is cooling crystallization. Specifically, the concentrated solution obtained by evaporation and concentration is cooled and crystallized under normal pressure conditions of 263.15K to 293.15K, and the crystals are dried and recovered to obtain glycolic acid crystals.

[0055] Further preferably, the crystallization method comprises the following steps:

[0056] (1) The high-concentration ethanolic acid mother liquor obtained after evaporation and concentration is cooled and crystallized at 263.15K to 293.15K and normal pressure to obtain crystals.

[0057] (2) Washing the crystals with mother liquor, and then drying and recovering them to obtain glycolic acid crystals; the washing process can remove ppm-level hydrolysis products of other components, such as terephthalic acid, lactic acid, adipic acid, 6-hydroxy-caproic acid, 1,4-butanediol, 1,4-succinic acid, β-hydroxybutyric acid, etc., and the purity of the glycolic acid crystals finally obtained can reach more than 99.5wt%.

[0058] In the method of the present invention, the waste degradable plastic components used specifically include one or more of PBAT, PLA, PCL, PHA, PBS, talcum powder, calcium carbonate, and bentonite, and the mass percentage of these components in the waste degradable plastic can be between 1% and 99%. These components do not participate in the hydrolysis reaction and become solid residues.

[0059] like Figure 1 As shown, the present invention also provides a system for recovering glycolic acid crystals using waste biodegradable plastics, comprising a crushing unit 1, a hydrolysis unit 2, a first solid-liquid separation unit 3, an evaporation crystallization unit 4 and a second solid-liquid separation unit 5 connected in sequence. The system can be used to implement the method for recovering glycolic acid crystals of the present invention, wherein the crushing unit 1 is used to crush the waste biodegradable plastics, the hydrolysis unit is used to selectively hydrolyze the crushed waste biodegradable plastics, the first solid-liquid separation unit 3 is used to filter the hydrolyzate, the evaporation crystallization unit 4 is used for evaporation concentration and crystallization, and the second solid-liquid separation unit 5 is used to recover the glycolic acid crystals.

[0060] Preferably, the crushing unit 1 is also connected to a raw material conveying device so that the waste biodegradable plastics can be moved into the crushing unit.

[0061] Preferably, the hydrolysis unit 2 is also provided with a water inlet so that water can enter the hydrolysis unit 2 to participate in the hydrolysis reaction.

[0062] Preferably, the first solid-liquid separation unit 3 is provided with a discharge port so that the solid residue can be separated.

[0063] Preferably, the evaporation crystallization unit 4 is provided with a waste liquid outlet for the distilled solvent water to flow out; the evaporation crystallization unit 4 is connected to the second solid-liquid separation unit 5 through a mother liquor pipeline, the inlet of the mother liquor pipeline is connected to the second solid-liquid separation unit 5, and the outlet of the mother liquor pipeline is connected to the evaporation crystallization unit 4, so that the mother liquor can reflux to wash the crystals.

[0064] Preferably, the second solid-liquid separation unit 5 is also provided with a product outlet for recovering glycolic acid crystals.

[0065] The present invention is illustrated below by means of specific examples.

[0066] Example 1

[0067] The purity of glycolic acid crystals is tested in the following way:

[0068] (1) The melting point of glycolic acid crystals was tested by capillary method. In this embodiment, a Mettler Toledo melting point meter MP30 was used for testing. The melting point of glycolic acid at normal pressure is 351.15K to 352.15K. By comparing with this melting point, the purity of the obtained glycolic acid crystals can be examined.

[0069] (2) Liquid chromatography is used to detect whether the glycolic acid crystals contain ppm-level hydrolysis product impurities, and the crystal purity % = 1-∑ impurity %.

[0070] (3) The glycolic acid crystals are prepared into a 70% aqueous solution, and the platinum-cobalt colorimetric method of GB 11903 is used to test the platinum-cobalt colorimetry. The lower the color value, the higher the purity.

[0071] Example 2

[0072] In this example, Al2O3-doped SO4 2- / Ti02 solid super acid catalyst, the molar percentage of Al2O3 doped in the catalyst is 0.5%, recorded as 0.5STA.

[0073] The specific preparation process is as follows: 34.03g of tetrabutyl titanate and 0.1885g of AI(NO3)3·9H20 are dissolved in 300ml of water, and concentrated ammonia is slowly added under strong stirring until the final pH of the solution is 9-10, and then aged at room temperature for 24h. The obtained mixed hydroxide precipitate is washed by centrifugation using a 4% ammonium acetate solution as the eluent. After filtration, it is dried at 373K for 24h, and then soaked in 1.5mol / L H2SO4 for 1h, with a liquid-solid ratio of 15mL / g. After filtration, it is dried at 373K for 24h, and then calcined at 773K in a static air atmosphere for 2h to obtain 0.5STA.

[0074] Example 3

[0075] In this example, Al2O3-doped SO4 2- / Ti02 solid super acid catalyst, the molar percentage of Al2O3 doped in the catalyst is 1%, recorded as 1STA.

[0076] The specific preparation process is as follows: 18.971g titanium tetrachloride and 0.3789g AI(NO3)3·9H20 are dissolved in 100ml water, and concentrated ammonia is slowly added under strong stirring until the final pH of the solution is 9-10, and then aged at room temperature for 18h. The obtained mixed hydroxide precipitate is washed by centrifugation using a 4% ammonium acetate solution as the eluent. After filtration, it is dried at 373K for 24h, and then soaked in 1mol / L H2SO4 for 1h, with a liquid-solid ratio of 15mL / g. After filtration, it is dried at 373K for 24h, and then calcined at 823K in a static air atmosphere for 2h to obtain 1STA.

[0077] Example 4

[0078] In this example, Al2O3-doped SO4 2- / Ti02 solid super acid catalyst, the molar percentage of Al2O3 doped in the catalyst is 3%, recorded as 3STA.

[0079] The specific preparation process is as follows: 28.426g of isopropyl titanate and 1.1602g of AI(NO3)3·9H20 are dissolved in 200ml of water, and concentrated ammonia is slowly added under strong stirring until the final pH of the solution is 9-10, and then aged at room temperature for 12h. The obtained mixed hydroxide precipitate is washed by centrifugation using a 4% ammonium acetate solution as the eluent. After filtration, it is dried at 373K for 36h, and then soaked in 0.8mol / L H2SO4 for 1h, with a liquid-solid ratio of 15mL / g. After filtration, it is dried at 373K for 24h, and then calcined at 873K in a static air atmosphere for 2h to obtain 3STA.

[0080] Example 5

[0081] In this example, 0.5STA, 1STA and 3STA prepared in Examples 2 to 4 were subjected to 27 Al MAS NMR characterization was performed to examine the microstructure of the crystal. This example was performed using a Bruker DSX-300 NMR instrument. 27 Al MAS NMR characterization, 27 AlMAS NMR spectrum Figure 2 shown.

[0082] according to Figure 2 It can be seen that 0.5STA, 1STA and 3STA all belong to hexacoordinated aluminum, which means that the coordination environment of Al in these three catalysts is the same. Only hexacoordinated aluminum exists, and there is no tetracoordinated aluminum or pentacoordinated aluminum. Considering that Ti in tetragonal TiO2 is also hexacoordinated, it means that Al may have isomorphously replaced Ti and entered the lattice site of Ti. Such a lattice structure makes these catalysts more selective.

[0083] Example 6

[0084] This embodiment adopts the invented system to prepare glycolic acid crystals, and the catalyst is 0.5STA. The specific process is: crush the waste biodegradable plastics. The specific components of the waste biodegradable plastics used in this embodiment are polyglycolic acid, polylactic acid, and talcum powder. Put 100g of powder obtained after crushing and 1g of catalyst 0.5STA into 1500g of water, stir and react for 2h under normal pressure and 343.15K, and then filter. Collect the clear liquid, evaporate and concentrate at 5kPa and 335.15K for 2h. The concentrated liquid crystallizes at 283.15K under normal pressure to obtain crystals. After rinsing the crystals with concentrated mother liquor, vacuum dry to obtain the final product glycolic acid crystals.

[0085] The test showed that the melting point of the obtained glycolic acid crystals was 352.65K, the impurity lactic acid contained 1580.6ppm, and no Fe was detected. 2+ , C l - , purity 99.84194%, the platinum-cobalt chromaticity value of the obtained solution is 10.

[0086] Example 7

[0087] This embodiment adopts the system of the invention to prepare glycolic acid crystals, and the catalyst is 3STA to prepare glycolic acid crystals. The specific process is: crush the waste biodegradable plastics. The specific components of the waste biodegradable plastics used in this embodiment are polyglycolic acid, polybutylene terephthalate-adipate, and calcium carbonate. Put 100g of powder obtained after crushing and 2g of catalyst 3STA into 1200g of water, stir and react for 1h under normal pressure and 333.15K, and then filter. Collect the clear liquid, evaporate and concentrate at 15kPa and 353.15K for 1h. The concentrated liquid crystallizes at 273.15K under normal pressure to obtain crystals. After the crystals are rinsed with concentrated mother liquor, they are vacuum dried to obtain the final product glycolic acid crystals.

[0088] The test showed that the melting point of the obtained glycolic acid crystals was 352.95K, and the impurities contained 1738mg / kg of terephthalic acid, 7.3mg / kg of adipic acid, and 77.8mg / kg of 1,4-butanediol. No Fe was detected. 2+ , Cl - , purity 99.73545%, the platinum-cobalt chromaticity value of the obtained solution is 10.

[0089] Example 8

[0090] This embodiment adopts the system of the invention to prepare glycolic acid crystals, and the catalyst is 1STA crystals. The specific process is: crush the waste biodegradable plastics. The specific components of the waste biodegradable plastics used in this embodiment are polyglycolic acid and polycaprolactone. Put 100g of powder obtained after crushing and 1g of catalyst 1STA into 1800g of water, stir and react for 2h under normal pressure and 353.15K, and then filter. Collect the clear liquid, evaporate and concentrate at 5kPa and 340.15K for 3h. The concentrated liquid is crystallized at 263.15K under normal pressure to obtain crystals. After rinsing the crystals with concentrated mother liquor, vacuum dry to obtain the final product glycolic acid crystals.

[0091] The test showed that the melting point of the obtained glycolic acid crystals was 352.95K, the impurity 6-hydroxyhexanoic acid was 900.2mg / kg, and no Fe was detected. 2+ , Cl - , purity 99.90998%, the platinum-cobalt chromaticity value of the obtained solution is 5.

[0092] It can be seen from the above test results that the melting points of the glycolic acid crystals prepared in each embodiment are close to the melting point of glycolic acid, the impurity content is low, and there is no Fe ion and Cl ion. The chromaticity values ​​are low, the purity reaches more than 99.7%, and the crystal quality is high.

[0093] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for recovering glycolic acid crystals from waste biodegradable plastics, characterized in that: The waste degradable plastic comprises polyglycolic acid, and the method comprises the following steps: S1, crushing and obtaining the powder of the waste biodegradable plastic; S2, mixing the powder with water and a catalyst and stirring, and performing a selective hydrolysis reaction at a temperature of 293.15K to 353.15K under normal pressure to obtain a hydrolysis product containing glycolic acid; the reaction time is 1 to 3 hours; the catalyst is Al2O3-doped SO4 2- / TiO2 solid superacid catalyst; S3, post-treating the hydrolyzate to obtain glycolic acid crystals.

2. The method for recovering glycolic acid crystals from waste biodegradable plastics according to claim 1, characterized in that: In the catalyst, the molar percentage of Al2O3 is 0.1% to 99%.

3. The method for recovering glycolic acid crystals from waste biodegradable plastics according to claim 2, characterized in that: The preparation method of the catalyst comprises the following steps: using a Ti compound, Al(NO3)3·9H20 and concentrated ammonia water to react to obtain a mixed hydroxide precipitate; using an ammonium acetate solution to centrifuge, wash, filter and dry the mixed hydroxide precipitate, and then immersing it in 0.3-3 mol / L H2S04, and then filtering, drying, and calcining in a static air atmosphere in sequence to obtain the Al2O3-doped SO4 2- / Ti02 solid superacid catalyst.

4. The method for recovering glycolic acid crystals from waste biodegradable plastics according to claim 3, characterized in that: The Ti compound is one of TiCl4, TiBr4, tetramethyl titanate, tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate, tetrabutyl titanate, tetrastearate titanate, tetra(2-ethylhexyl) titanate, and titanium tetramethacrylate.

5. A method for recovering glycolic acid crystals from waste biodegradable plastics according to any one of claims 1 to 4, characterized in that: In the step S1, the particle size of the powder is 0.1-1 mm.

6. The method for recovering glycolic acid crystals from waste biodegradable plastics according to claim 5, characterized in that: In the step S2, the mass ratio of water to the powder is 1:1-20, and the mass of the catalyst is 0.2-7 wt % of the mass of the powder.

7. A method for recovering glycolic acid crystals from waste biodegradable plastics according to any one of claims 1 to 4, characterized in that: The post-treatment includes filtering, concentrating, crystallizing and drying the hydrolyzate.

8. The method for recovering glycolic acid crystals from waste biodegradable plastics according to claim 7, characterized in that: The concentration is evaporation concentration, and the crystallization is cooling crystallization.

9. A method for recovering glycolic acid crystals from waste biodegradable plastics according to any one of claims 1 to 4, characterized in that: The components of the waste biodegradable plastics also include one or more of PBAT, PLA, PCL, PHA, PBS, talcum powder, calcium carbonate, and bentonite.

10. A system for recovering glycolic acid crystals using waste biodegradable plastics, characterized in that: The invention comprises a crushing unit (1), a hydrolysis unit (2), a first solid-liquid separation unit (3), an evaporation crystallization unit (4) and a second solid-liquid separation unit (5) which are connected in sequence; the crushing unit (1) is used to crush the waste biodegradable plastic, the hydrolysis unit is used to selectively hydrolyze the crushed waste biodegradable plastic, the first solid-liquid separation unit (3) is used to filter the hydrolysis product, the evaporation crystallization unit (4) is used to evaporate, concentrate and crystallize, and the second solid-liquid separation unit (5) is used to recover the glycolic acid crystals.

Citation Information

Cited By

  • Method and system for recycling glycollic acid

    CN122608504A