Triazinetrione compound containing carbon-carbon double bonds and application of triazinetrione compound

By using a triazinetrione compound containing a carbon-carbon double bond in combination with a polyimide precursor, a photoinitiator and a silane coupling agent, a photosensitive resin composition with high resolution and excellent mechanical properties is prepared, solving the current problem. There are problems with insufficient resolution and mechanical properties in the technology, and it is suitable for high-performance electronic devices and semiconductor devices.

CN118812451APending Publication Date: 2024-10-22POME TECH CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410788556.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing photosensitive resin compositions have low resolution and insufficient mechanical properties in electronic devices and semiconductor devices, and cannot meet the requirements for high performance.

Method used

A photosensitive resin composition is prepared using a triazinetrione compound containing a carbon-carbon double bond, a polyimide precursor, a photoinitiator and a silane coupling agent through specific reaction conditions to form a high-resolution, excellent mechanical property. Cured film.

Benefits of technology

It significantly improves the resolution, mechanical properties and adhesion of the photosensitive resin composition, and is suitable for high-sensitivity, high-resolution, and high-mechanical-strength applications in high-tech fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118812451A_ABST
    Figure CN118812451A_ABST
Patent Text Reader

Abstract

The invention relates to a triazinetrione compound containing a carbon-carbon double bond and application thereof, the triazinetrione compound has a structural formula as shown in the following formula (1) or (2): # imgabs0 # formula (1), in the formula (1), R1 is phenyl, ester group, alkyl with the carbon atom number of 1-10, alkoxy, halogen atom and hydrogen atom; r2 is phenyl, carbonyl, ester group, alkyl with the carbon atom number of 1-10, and alkoxy; in formula (2), R3 represents a C3-10 cyclic hydrocarbon group containing an unsaturated bond. The structure contains a triazinetrione group, the group has the effects of reducing the refractive index, improving the adhesive force with a base material and improving the flexibility of the composition, the photosensitivity of the photosensitive resin composition can be remarkably improved, the composition has higher light transmittance in the exposure process, the adhesive force and the flexibility can be improved through a carbonyl structure, and the light transmittance of the composition is improved. Furthermore, the mechanical property, the photoetching property and the adhesion property with a base material of a photosensitive resin composition cured film are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a triazinetrione compound containing a carbon-carbon double bond and application thereof, belonging to the field of organic synthesis. Background Art

[0002] To date, polyimide resins with excellent heat resistance, dielectric properties and mechanical properties have been used for passivation layers, surface protection films and interlayer insulating films in thermal insulation materials of electronic devices and semiconductor devices. In order to meet the above requirements, it is necessary to use a resin composition that can be patterned by photolithography, and the resin composition used needs to meet the characteristics of high resolution, high tensile strength, high elongation at break, high Tg and high adhesion.

[0003] Photosensitive resin compositions are usually composed of a base resin, additives and solvents. Depending on the base resin, they can be divided into acrylic resin, epoxy resin, polyimide resin, etc. Polyimide materials have the advantages of good heat resistance, excellent insulation, low stress and high adhesion. They are often used in semiconductor packaging materials, but there are still problems such as poor mechanical properties and low resolution.

[0004] Patent document CN107850844A uses dianhydride or diamine containing ether bond structure to prepare a photosensitive resin composition, thereby obtaining a cured film with excellent adhesion to copper wiring. Patent document CN105829968A discloses a negative photosensitive resin composition, which can obtain a cured film with excellent mechanical properties by adding a monofunctional photopolymerizable compound with a molecular weight less than or equal to 300. Patent document CN1668980B discloses a negative photosensitive resin composition to which a melamine resin with thermal crosslinking properties is added. The composition has good pattern processability, and the obtained cured film has high heat resistance and high chemical resistance. Patent document CN102985505B discloses a negative photosensitive resin composition, which can form a pattern by an alkaline developer, has excellent thermal compression bonding and adhesion, and a resolution of 30μm.

[0005] The negative photosensitive resin compositions reported in the above prior art have low resolution and need to improve their mechanical properties. With the high performance requirements of electronic devices, the miniaturization, high speed of operation and high density of wiring of semiconductor devices have been developed, which puts forward higher requirements on semiconductor packaging materials, requiring not only high adhesion and insulation reliability, but also higher photosensitivity, resolution and mechanical properties. Therefore, it is necessary to further study the photosensitive resin compositions with respect to these properties in order to meet the high performance requirements of electronic devices. Summary of the invention

[0006] In view of the problems existing in the prior art, the present invention provides a photosensitive resin composition, which can be developed by a developer after exposure, has good adhesion, high resolution, excellent mechanical properties and good insulation when hot-pressed on a substrate, and can therefore be used in high-tech fields requiring high sensitivity, high resolution and high mechanical strength.

[0007] The photosensitive resin composition film formed by the photosensitive resin composition of the present invention has high resolution, excellent mechanical properties, high Tg and good adhesion.

[0008] The technical solution of the present invention to solve the above problems is as follows:

[0009] In a first aspect of the present invention, a triazinetrione compound containing a carbon-carbon double bond is provided, wherein the triazinetrione compound has a structural formula shown in the following formula (1) or (2):

[0010]

[0011] In formula (1), R1 is a phenyl group, an ester group, a hydrocarbon group having 1 to 10 carbon atoms, an alkoxy group, a halogen atom, or a hydrogen atom;

[0012] R2 is a phenyl group, a carbonyl group, an ester group, a hydrocarbon group having 1 to 10 carbon atoms, or an alkoxy group;

[0013] In the formula (2), R3 is a cyclic hydrocarbon group having 3 to 10 carbon atoms and containing an unsaturated bond.

[0014] Optionally, 1,3,5-tris(2-chloroethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione is reacted with the compound of formula (3) by reaction I, as shown in reaction formula a, to obtain the compound of formula (1);

[0015]

[0016] Reaction II of 1,3,5-tris(2-chloroethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione with the compound of formula (4), as shown in reaction formula b, to obtain the compound of formula (2);

[0017] H2N-R3

[0018] Formula (4);

[0019]

[0020] Optionally, the reaction conditions of the reaction I are as follows:

[0021] The reaction temperature of the reaction I is -5 to 80°C;

[0022] The reaction time of the reaction I is 3 to 9 h;

[0023] In the reaction I, the molar ratio of 1,3,5-tris(2-chloroethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione to the compound of formula (3) is 1:1.

[0024] Optionally, the reaction conditions of reaction II are as follows:

[0025] The reaction conditions of the reaction II are as follows:

[0026] The reaction temperature of the reaction II is -5 to 80°C;

[0027] The reaction time of reaction II is 3 to 9 hours;

[0028] In the reaction II, the molar ratio of 1,3,5-tris(2-chloroethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione to the compound of formula (4) is 1:1.

[0029] Optionally, the reaction I and reaction II are carried out in an organic solvent.

[0030] Optionally, the organic solvent is selected from at least one of acetone, tetrahydrofuran, toluene and xylene.

[0031] Optionally, the reaction I and reaction II include three reaction stages: the first reaction stage is at -5°C to 0°C for 3 hours; the second reaction stage is at 20°C to 30°C for 3 hours; and the third reaction stage is at 60°C to 80°C for 3 hours.

[0032] Optionally, the reaction I and reaction II require the addition of a reagent for removing HCl, preferably NaHCO3 and N,N-diisopropylethylamine (DIPEA).

[0033] Optionally, the reagent for removing HCl needs to be dissolved in the organic solvent or distilled water of the above reaction and added dropwise into the reaction system.

[0034] Alternatively, the reaction solution is transferred to a separatory funnel, washed with pure water three times, and separated to remove the aqueous layer to obtain an organic layer.

[0035] Optionally, anhydrous magnesium sulfate is added to the organic layer to remove water and dry it, and then filtered to obtain a clear filtrate.

[0036] Optionally, the filtrate is concentrated under reduced pressure to obtain a white solid, thereby obtaining a triazinetrione compound containing a carbon-carbon double bond.

[0037] In a second aspect of the present application, a photosensitive resin composition is provided, comprising a polyimide precursor, a photoinitiator, a photopolymerizable compound containing an unsaturated bond, and a silane coupling agent;

[0038] Optionally, the photopolymerizable compound containing an unsaturated bond is selected from triazinetrione compounds containing a carbon-carbon double bond.

[0039] Optionally, the method for preparing the polyimide precursor comprises the following steps:

[0040] The tetracarboxylic dianhydride compound and the diamine compound are mixed and reacted to obtain a polyimide precursor.

[0041] Optionally, the tetracarboxylic dianhydride compound is selected from at least one of pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride and 1,2,3,4-cyclobutanetetracarboxylic dianhydride;

[0042] The diamine compound is selected from diamines having an aromatic ring.

[0043] Optionally, the diamine of the aromatic ring includes at least one of a diamine having a hydroxyl group and an aromatic ring and a diamine having a carboxyl group and an aromatic ring;

[0044] Optionally, the diamine having an aromatic ring is selected from at least one of 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfide, 2,2'-bis(trifluoromethyl)biphenylenediamine, benzyl diamine, m-phenylenediamine, p-phenylenediamine, 1,5-naphthalene diamine, bis(4-aminophenoxyphenyl) sulfone, bis(3-aminophenoxyphenyl) sulfone, bis(4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl] ether, and 1,4-bis(4-aminophenoxy)benzene.

[0045] Optionally, the diamine having a hydroxyl group and an aromatic ring is selected from at least one of 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 2,2'-bis(3-amino-4-hydroxyphenyl)propane, 3,3'-diamino-4,4'-dihydroxybiphenyl, 3,3'-dihydroxy-4,4'-diaminobiphenyl, 3,3'-diamino-4,4'-dihydroxydiphenylmethane, 3,3'-diamino-4,4'-dihydroxydiphenyl sulfide and 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone.

[0046] Optionally, the diamine having a carboxyl group and an aromatic ring is selected from at least one of 2,5-diaminobenzoic acid, 3,4-diaminobenzoic acid, 2,5-diaminoterephthalic acid, bis(4-amino-3-carboxyphenyl)methane, bis(4-amino-3-carboxyphenyl)ether, 4,4'-diamino-3,3'-dicarboxybiphenyl, and 4,4'-diamino-5,5'-dicarboxy-2,2'-dimethylbiphenyl.

[0047] Optionally, the reaction conditions of the reaction are as follows:

[0048] The tetracarboxylic dianhydride compound and the diamine compound are reacted in a ratio of 1:0.5 to 1:1;

[0049] The reaction temperature is 25 to 180°C;

[0050] The reaction time is 1 to 5 hours.

[0051] Optionally, the polyimide precursor is 100 parts by mass as a measurement basis;

[0052] Photoinitiator 0.01~30 parts by weight

[0053] 1 to 100 parts by weight of a photopolymerizable compound containing an unsaturated bond

[0054] Silane coupling agent: 0.01 to 1 part by mass

[0055] Optionally, the polyimide precursor is selected from at least one of polyamic acid, polyamide ester and polyimide;

[0056] The photoinitiator is selected from at least one of benzophenone compounds, benzylidene compounds, coumarin compounds, anthraquinone compounds, benzoin compounds, thioxanthone compounds, thiol compounds, glycine compounds, oxime compounds, α-aminoalkylphenone compounds, 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide;

[0057] The silane coupling agent is selected from at least one of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, bis(γ-aminopropyl)tetramethylsiloxane, bis(γ-aminobutyl)tetramethylsiloxane, bis(γ-aminopropyl)tetraphenylsiloxane, bis(γ-aminopropyl)tetraphenylpolysiloxane, bis(γ-aminopropyl)tetraphenylsiloxane, bis(γ-aminobutyl)tetraphenylpolysiloxane, 3-(2,3-epoxypropyloxy)propyltriethoxysilane and vinyltriethoxysilane.

[0058] Optionally, the benzophenone compound is selected from at least one of benzophenone, 4,4-bis(diethylamino)benzophenone, 3,3,4,4-tetra(tert-butylperoxycarbonyl)benzophenone, etc.; the coumarin compound is selected from at least one of 3,5-bis(diethylaminobenzylidene)-N-methyl-4-piperidone, 3,5-bis(diethylaminobenzylidene)-N-ethyl-4-piperidone and the like benzylidene compounds; 7-diethylamino-3-nonylcoumarin, 4,6-dimethyl-3-ethylaminocoumarin, 3,3-carbonylbis(7-diethylaminocoumarin), 7-diethylamino-3-(1-methylbenzimidazolyl)coumarin, 3-(2-benzothiazolyl)-7-diethylaminocoumarin;

[0059] The anthraquinone compound is selected from at least one of 2-tert-butylanthraquinone, 2-ethylanthraquinone and 1,2-benzanthraquinone;

[0060] At least one of the benzoin compounds benzoin methyl ether, benzoin ethyl ether and benzoin isopropyl ether;

[0061] The thioxanthone compound is selected from at least one of 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone and 2-isopropylthioxanthone;

[0062] The mercapto compound is selected from at least one of ethylene glycol di(3-mercaptopropionate), 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, 2-mercaptobenzimidazole, etc.;

[0063] The glycine compound is selected from at least one of N-phenylglycine, N-methyl-N-phenylglycine, N-ethyl-N-(p-chlorophenyl)glycine, N-(4-cyanophenyl)glycine, etc.;

[0064] The oxime compound is selected from 1-phenyl-1,2-butanedione-2-(o-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-benzoyl)oxime, 1-[4-(phenylthio)phenyl]-1,2-octanedione-2- At least one of (0-benzoyl oxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethanone 1-(0-acetyl oxime); the α-aminoalkylphenone compound is selected from at least one of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butane-1-one and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one.

[0065] Optionally, the photosensitive resin composition further contains epoxy compounds and / or photopolymerizable compounds of other structures.

[0066] Optionally, based on 100 parts by mass of the polyimide precursor:

[0067] 1 to 100 parts by mass of other photopolymerizable compounds and / or epoxy compounds.

[0068] Optionally, the epoxy compound of other structures is selected from at least one of bisphenol A epoxy compounds, novolac epoxy compounds, biphenol epoxy compounds, bisphenol F glycidyl ether epoxy compounds, cyclic aliphatic epoxy compounds, heterocyclic epoxy compounds, and aromatic epoxy compounds;

[0069] The photopolymerizable compound of other structures is selected from diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane diacrylate, trimethylolpropane dimethacrylate, trimethylolpropane trimethacrylate, styrene, α-methylstyrene, 1,2-dihydronaphthalene, 1,3-diisopropenylbenzene, 3-methylstyrene, 4-methylstyrene, p-vinylbenzene, 2-vinylnaphthalene, butyl acrylate, butyl methacrylate Ester, isobutyl acrylate, hexyl acrylate, isooctyl acrylate, isobornyl acrylate, isobornyl methacrylate, cyclohexyl methacrylate, 1,3-butanediol diacrylate, 1,3-butanediol dimethacrylate, neopentyl glycol diacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, 1,10-decanediol dimethacrylate, tricyclodecane dimethanol diacrylate, pentaerythritol Pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, dipentaerythritol hexaacrylate, dipentaerythritol hexamethacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 1,3-diacryloxy-2-hydroxypropane, 1,3-dimethacryloxy-2-hydroxypropane, methylenebisacrylamide, N,N-dimethylacrylamide, N-hydroxymethylacrylamide, 2,2,6,6-tetramethylpiperidinyl methacrylate, N-methyl-2,2,6, At least one of 6-tetramethylpiperidinyl acrylate, N-methyl-2,2,6,6-tetramethylpiperidinyl methacrylate, N-methyl-2,2,6,6-tetramethylpiperidinyl acrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, propoxylated bisphenol A diacrylate, propoxylated bisphenol A methacrylate, propoxylated ethoxylated bisphenol A diacrylate, propoxyethoxylated bisphenol A dimethacrylate, N-vinyl caprolactam, polyethylene glycol diacrylate, and 2-isocyanatoethyl methacrylate.

[0070] Optionally, the photosensitive resin composition further contains a solvent.

[0071] Optionally, the solvent is selected from at least one of polar aprotic solvents, ether solvents, ketone solvents, ester solvents, alcohol solvents, and aromatic hydrocarbon solvents.

[0072] Optionally, the polar aprotic solvent is selected from at least one of N-methyl-2-pyrrolidone, γ-butyrolactone, γ-valerolactone, δ-valerolactone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, 1,3-dimethyl-2-imidazolidinone, N,N-dimethylpropylene urea, N,N-dimethylisobutyramide, and methoxy-N,N-dimethylpropionamide;

[0073] The ether solvent is at least one of tetrahydrofuran, dioxane, propylene glycol monomethyl ether, and propylene glycol monoethyl ether;

[0074] At least one of the ketone solvents acetone, methyl ethyl ketone, and diisobutyl ketone;

[0075] The ester solvent is at least one of ethyl acetate, butyl acetate, isobutyl acetate, propyl acetate, propylene glycol monomethyl ether acetate, 3-methyl-3-methoxybutyl acetate, ethyl lactate, and methyl lactate;

[0076] The alcohol solvent is selected from at least one of diacetone alcohol and 3-methyl-3-methoxybutanol;

[0077] The aromatic hydrocarbon solvent is selected from at least one of toluene and xylene.

[0078] Optionally, based on 100 parts by mass of the polyimide precursor:

[0079] 50 to 1000 parts by mass of solvent.

[0080] Optionally, the solvent is selected from at least one of N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, N-vinylpyrrolidone, N,N-diethylformamide, γ-butyrolactone, ethyl lactate; methyl monoglycol dimethyl ether, methyl diglycol dimethyl ether, methyl triglycol dimethyl ether, ethyl monoglycol dimethyl ether, ethyl diglycol dimethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol dimethyl ether, and ethylene glycol diethyl ether.

[0081] Optionally, the photosensitive resin composition is coated on a substrate, the substrate is heated to form a photosensitive resin layer, and the photosensitive resin layer is exposed, developed, and heated to form a cured film.

[0082] According to a third aspect of the present application, an electronic component or a semiconductor device is provided, wherein a plurality of substrates are bonded together or a substrate is bonded to other components through a cured film of the photosensitive resin composition.

[0083] The beneficial effects of this application:

[0084] 1) The photopolymerizable compound of a special structure provided in the present application contains a triazinetrione group in the structure, which has the effect of reducing the refractive index, improving the adhesion to the substrate and improving the flexibility of the composition, and can significantly improve the photosensitivity of the photosensitive resin composition.

[0085] 2) The photopolymerizable compound provided in the present application has a higher light transmittance during the exposure process and the carbonyl group contained in the compound can improve the adhesion and flexibility, thereby improving the mechanical properties, photolithographic properties, and bonding properties with the substrate of the cured film of the photosensitive resin composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0086] Figure 1 Compatibility test for this application (poor compatibility)

[0087] Figure 2 Compatibility test for this application (good compatibility) DETAILED DESCRIPTION

[0088] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the embodiments of the present invention will be described clearly and completely below, and the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the technical scheme of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The present application is described in detail below in conjunction with the embodiments, but the present application is not limited to these embodiments.

[0089] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0090] The weight average molecular weight Mw and number average molecular weight Mn of the photosensitive resin or the photosensitive resin composition precursor in the embodiment of the present invention can be easily measured in the form of polystyrene-converted values ​​by gel permeation chromatography (GPC).

[0091] Example 1

[0092] Synthesis of photopolymerizable compounds

[0093] Synthesis Example 1: Synthesis of Photopolymerizable Compound C-1

[0094] In a four-necked reaction flask with a stirrer and a thermometer, dissolve 1,3,5-tris(2-chloroethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione (94.97 g, 0.3 mol) in 150 ml of tetrahydrofuran and cool to 0°C. Add p-aminostyrene (107.244 g, 0.9 mol) and 240 ml of tetrahydrofuran dropwise to the solution. After the addition is complete, add an aqueous solution of NaHCO3 (75.69 g, 0.9 mol) (300 ml of water) dropwise. Stir the reaction at 0°C for 3 h, then heat to 25°C for 3 h, and finally heat to 65°C for 3 h.

[0095] After the reaction is completed, the temperature is cooled to room temperature, and the reaction solution is transferred to a separatory funnel, and 100 g of tetrachloromethane and 100 ml of pure water are added for extraction. The aqueous layer is separated and removed. The above operation is repeated 3 times. Finally, the organic layer is dried over MgSO4 and filtered to obtain a clear filtrate, which is concentrated by a rotary evaporator to obtain a white solid C-1, whose structural formula is as follows:

[0096]

[0097] The NMR information of compound C-1 is as follows:

[0098] 1 H NMR: δ: 3.27(6H,t,J=6.9Hz), 3.96(6H,t,J=6.9Hz), 4.87(3H,dd,J=10.9,1.4Hz), 5.73(3H,dd,J=18.0,1. 4Hz), 6.66 (3H, dd, J = 18.0, 10.9 Hz), 6.90 (6H, ddd, J = 8.2, 1.5, 0.5 Hz), 7.42 (6H, ddd, J = 8.2, 2.0, 0.5 Hz).

[0099] Synthesis Example 2: Synthesis of Photopolymerizable Compound C-2

[0100] Photopolymerizable compound C-2 was prepared in the same manner as in Synthesis Example 1, except that p-aminostyrene (107.244 g, 0.9 mol) was replaced with 3-methylenecyclobutylamine (74.817 g, 0.9 mol). The following compound C-2 was obtained, and its structure is as follows:

[0101]

[0102] The NMR information of compound C-2 is as follows:

[0103] 1H NMR: δ2.39-2.54(12H,2.47(dd,J=14.4,4.6Hz),2.47(dd,J=14.4,4.5Hz)),2.84(6H,t,J=6.9Hz),3.7 8(3H,tt,J=6.8,2.3Hz), 4.18(6H,t,J=6.9Hz), 4.93-5.04(6H, 4.98(d,J=1.3Hz), 4.98(d,J=1.3Hz)).

[0104] Synthesis Example 3: Synthesis of Photopolymerizable Compound C-3

[0105] Photopolymerizable compound C-3 was prepared in the same manner as in Synthesis Example 1, except that p-aminostyrene (107.244 g, 0.9 mol) was replaced with acrylamide (63.972 g, 0.9 mol). The following compound C-3 was obtained, and its structure is as follows:

[0106]

[0107] The NMR information of compound C-4 is as follows:

[0108] 1 H NMR: δ3.41(6H,t,J=7.1Hz), 3.91(6H,t,J=7.1Hz), 5.86(3H,dd,J=10.9,1.5Hz), 6.17(3H,dd,J=17.0,1.5Hz), 6.54(3H,dd,J=17.0,10.9Hz).

[0109] Synthesis Example 4: Synthesis of Photopolymerizable Compound C-4

[0110] Photopolymerizable compound C-4 was prepared in the same manner as in Synthesis Example 1, except that p-aminostyrene (107.244 g, 0.9 mol) was replaced with compound N-4 (112.689 g, 0.9 mol). The following compound C-4 was obtained, and its structure is as follows:

[0111]

[0112] The NMR information of compound C-4 is as follows:

[0113] 1H NMR: δ1.25-1.99(18H,1.35(ddddd,J=13.3,10.2,8.7,2.1,1.4Hz),1.51(dddd,J=13.2,10.2,8.7,2.1Hz),1.61(ddddd,J=13.3,5.8,3.7,2.3 ,1.4Hz),1.66(dtt,J=12.9,3.7,2.1Hz),1.78(dddd,J=13.2,3.7,2.3,1.4Hz),1.91(dtt,J=12.9,10.2,2.3Hz)),2.12-2.38(6H,2.20(dddd, J=14.3,5.8,2.5,1.4Hz),2.30(dddd,J=14.3,8.7,1.9,1.4Hz)),2.80-2.92(6H,2.86(t,J=6.9Hz),2.86(t,J=6.9Hz)),3.40(3H,ddd,J=8.7, 3.7, 1.4Hz), 4.13-4.24 (6H, 4.18 (t, J = 6.9Hz), 4.18 (t, J = 6.9Hz)), 5.36-5.54 (6H, 5.43 (ddd, J = 11.0, 2.5, 1.9Hz), 5.47 (dd, J = 11.0, 3.7Hz)).

[0114] Synthesis Example 5: Synthesis of Photopolymerizable Compound C-5

[0115] Photopolymerizable compound C-5 was prepared in the same manner as in Synthesis Example 1, except that p-aminostyrene (107.244 g, 0.9 mol) was replaced with compound N-5 (100.066 g, 0.9 mol). The following compound C-5 was obtained, and its structure is as follows:

[0116]

[0117] The NMR information of compound C-5 is as follows:

[0118] 1H NMR: δ1.24-1.49(6H,1.34(dddd,J=12.9,10.1,10.0,3.9Hz), 1.34(dddd,J=12.9,10.1,10.0,3.9Hz), 1.41(dddd,J=12.9,4. 0,2.1,1.9Hz),1.41(dddd,J=12.9,4.0,2.1,1.9Hz)),1.53-1.70(3H,1.61(ddtdd,J=10.1,10.0,4.6,3.9,2.1Hz),1.61(ddt dd,J=10.1,10.0,4.6,3.9,2.1Hz)),2.00-2.28(12H,2.09(dddd,J=14.2,10.0,4.0,2.2Hz),2.09(dddd,J=14.2,10.0,4.0,2 .2Hz),2.11(dddd,J=14.2,3.9,2.3,1.9Hz),2.12(dddd,J=14.2,3.9,2.3,1.9Hz),2.19(dddd,J=14.3,10.0,2.5Hz),2.19(ddd ,J=14.3,10.0,2.5Hz),2.19(ddd,J=14.3,3.9,2.2Hz),2.21(ddd,J=14.3,3.9,2.2Hz)),2.47-2.58(6H,2.52(d,J=4.6Hz),2 .52(d,J=4.6Hz),2.52(d,J=4.6Hz),2.52(d,J=4.6Hz)),2.75-2.87(6H,2.81(t,J=7.2Hz),2.81(t,J=7.2Hz),2.81(t,J=7.2 Hz),2.81(t,J=7.2Hz)),4.12-4.24(6H,4.18(t,J=7.2Hz),4.18(t,J=7.2Hz),4.18(t,J=7.2Hz),4.18(t,J=7.2Hz)),5.13-5 .27(6H,5.20(ddd,J=10.1,2.5,2.2Hz),5.20(ddd,J=10.1,2.5,2.2Hz),5.20(dt,J=10.1,2.2Hz),5.20(dt,J=10.1,2.2Hz)).

[0119] Synthesis Example 6: Synthesis of Photopolymerizable Compound C-6

[0120] Photopolymerizable compound C-6 was prepared in the same manner as in Synthesis Example 1, except that p-aminostyrene (107.244 g, 0.9 mol) was replaced with 5-norbornene-2-methylamine (110.88 g, 0.9 mol). The following compound C-6 was obtained, and its structure is as follows:

[0121]

[0122] The NMR information of compound C-6 is as follows:

[0123] 1 H NMR: δ1.43-1.60(6H,1.50(ddd,J=13.0,4.3,1.5Hz), 1.51(ddd,J=13.0,4.3,1.5Hz), 1.53(dt,J=16.1,2.8Hz), 1.53(dt,J=16.1,2.8Hz)),1.61-1.80(6H,1.69(ddd,J=13.0,8.1,4.5Hz),1.70(ddd,J=13.0,8.1,4.5Hz),1.72 (dt,J=16.1,2.1Hz),1.72(dt,J=16.1,2.1Hz)),2.33-2.49(3H,2.41(dddt,J=8.1,4.6,4.3,4.2Hz),2.42(ddq, J=8.1,4.5,4.2Hz)),2.63-3.01(18H,2.69(d,J=4.2Hz),2.69(d,J=4.2Hz),2.69(d,J=4.2Hz),2.69(d,J=4.2Hz ),2.77(dddd,J=4.6,2.8,2.1,1.9Hz),2.81(t,J=7.2Hz),2.81(t,J=7.2Hz),2.81(t,J=7.2Hz),2.81(t,J=7.2H z),2.86(ddddd,J=4.5,2.8,2.0,1.9,1.5Hz),2.88(dddd,J=4.5,2.8,2.0,1.9Hz),2.95(ddddd,J=4.5,2.8,2.1 ,1.9,1.5Hz)),4.12-4.24(6H,4.18(t,J=7.2Hz),4.18(t,J=7.2Hz),4.18(t,J=7.2Hz),4.18(t,J=7.2Hz)),5.9 8-6.11 (6H, 6.04 (dd, J = 5.4, 1.9Hz), 6.04 (dd, J = 5.4, 1.9Hz), 6.05 (dd, J = 5.4, 1.9Hz), 6.05 (dd, J = 5.4, 1.9Hz)).

[0124] Synthesis of resin precursor and preparation of photosensitive resin composition

[0125] Synthesis of resin precursor

[0126] Under nitrogen atmosphere, BAHF (311.32 g, 0.85 mol), SiDA (12.43 g, 0.05 mol) and MAP (21.83 g, 0.20 mol) were dissolved in 984 g of GBL, and ODPA (310.21 g, 1.0 mol) was added, stirred at 60°C for 1 hour, then heated to 180°C, stirred for 2 hours, and cooled to room temperature to obtain an alkali-soluble polyimide solution. The reaction solution was dropped into pure water, the precipitate was collected by filtration, and dried under reduced pressure to obtain polyimide resin A-1. The number average molecular weight was 14684 and the weight average molecular weight was 19705.

[0127] Example 1

[0128] 100 g of polyimide resin A-1 as component (A), 2 g of photoinitiator B (OXE-1), 28 g of photopolymerizable C-1, and 0.2 g of silane coupling agent KBM-1403 were dissolved in N-methylpyrrolidone and mixed evenly. The resulting solution was pressure filtered using a filter with a pore size of 0.2 um to obtain a photosensitive resin composition Q-1.

[0129] Embodiments 2 to 6

[0130] A photosensitive resin composition was prepared in the same manner as in Example 1, except that 28 g of the photopolymerizable compound C-1 was replaced by 28 g of photopolymerizable compounds C-2, C-3, C-4, C-5, and C-6, respectively, to obtain photosensitive resin compositions Q-2, Q-3, Q-4, Q-5, and Q-6, respectively.

[0131] Example 7

[0132] 100 g of polyimide resin A-1 as component (A), 2 g of photoinitiator B (OXE-1), 14 g of photopolymerizable C-4 and 14 g of photopolymerizable C-1, and 0.2 g of silane coupling agent KBM-1403 were dissolved in N-methylpyrrolidone and mixed evenly. The resulting solution was pressure filtered using a filter with a pore size of 0.2 um to obtain a photosensitive resin composition Q-7.

[0133] Embodiments 8 to 11

[0134] A photosensitive resin composition was prepared in the same manner as in Example 7, except that 14 g of the photopolymerizable compound C-1 was replaced by 14 g of photopolymerizable compounds C-2, C-3, C-5, and C-6, respectively, to obtain photosensitive resin compositions Q-8, Q-9, Q-10, and Q-11, respectively.

[0135] Example 12

[0136] 100 g of polyimide resin A-1 as component (A), 2 g of photoinitiator B (OXE-1), 21 g of photopolymerizable C-4 and 7 g of photopolymerizable C-6, and 0.2 g of silane coupling agent KBM-1403 were dissolved in N-methylpyrrolidone and mixed evenly. The resulting solution was pressure filtered using a filter with a pore size of 0.2 um to obtain a photosensitive resin composition Q-12.

[0137] Example 13

[0138] 100 g of polyimide resin A-1 as component (A), 2 g of photoinitiator B (OXE-1), 18 g of photopolymerizable C-4 and 10 g of photopolymerizable C-6, and 0.2 g of silane coupling agent KBM-1403 were dissolved in N-methylpyrrolidone and mixed evenly. The resulting solution was pressure filtered using a filter with a pore size of 0.2 um to obtain a photosensitive resin composition Q-13.

[0139] Embodiment 14

[0140] 100 g of polyimide resin A-1 as component (A), 2 g of photoinitiator B (OXE-1), 10 g of photopolymerizable C-4 and 18 g of photopolymerizable C-6, and 0.2 g of silane coupling agent KBM-1403 were dissolved in N-methylpyrrolidone and mixed evenly. The resulting solution was pressure filtered using a filter with a pore size of 0.2 um to obtain a photosensitive resin composition Q-14.

[0141] Embodiment 15

[0142] 100 g of polyimide resin A-1 as component (A), 2 g of photoinitiator B (OXE-1), 7 g of photopolymerizable C-4 and 21 g of photopolymerizable C-6, and 0.2 g of silane coupling agent KBM-1403 were dissolved in N-methylpyrrolidone and mixed evenly. The resulting solution was pressure filtered using a filter with a pore size of 0.2 um to obtain a photosensitive resin composition Q-15.

[0143] Comparative Example 1

[0144] A photosensitive resin composition R-1 was prepared in the same manner as in Example 1, except that 28 g of the photopolymerizable compound (C-1) was replaced with 28 g of the photopolymerizable compound PEG, to obtain a photosensitive resin composition R-1.

[0145] Comparative Example 2

[0146] A photosensitive resin composition R-2 was prepared in the same manner as in Example 1, except that 28 g of the photopolymerizable compound (C-1) was replaced with 28 g of the photopolymerizable compound THEICTA, to obtain a photosensitive resin composition R-2.

[0147] The specific examples and comparative examples are shown in Table 1 below:

[0148] Table 1

[0149]

[0150]

[0151] Evaluation of photosensitive resin composition

[0152] 1. Compatibility and resolution test

[0153] The compatibility and resolution analysis methods in the examples and comparative examples of the present application are as follows:

[0154] Compatibility and resolution analysis using an optical microscope (MX63-F, Olympus)

[0155] The photosensitive resin composition samples of the above-mentioned embodiments and comparative examples were coated onto a 4-inch silicon wafer, and then soft-baked at 120°C for 3 minutes using a heating table to obtain a resin film with a thickness of 15 μm. The exposure was performed using an ultraviolet lamp (i and g lines) with an exposure amount of 400 mJ / cm-2 through a mask. After exposure, an alkaline developer was used for spray development for 180 seconds to remove the unexposed parts. An optical microscope (MX63-F, Olympus) was used to observe the color uniformity of the film at a magnification of 100 times, and the minimum size of the pattern that could be distinguished was taken as the resolution. (1) The system has poor compatibility and there are black spots in the film, such as Figure 1 As shown; (2) The system has good compatibility, the color inside the film is uniform, and there are no black spots, such as Figure 2 shown.

[0156] 2. Mechanical properties test of cured film of resin composition

[0157] The mechanical testing method for the cured film of the photosensitive resin composition in the examples and comparative examples of the present application is as follows:

[0158] The photosensitive resin composition samples of the above-mentioned embodiments and comparative examples were coated onto a 4-inch silicon wafer, and then soft-baked at 120°C for 3 minutes using a heating table to obtain a resin film with a film thickness of 15 μm. The film was then placed in a vacuum oxygen-free oven (Zhenping Technology Co., Ltd., MOLZK-32D1) for heat treatment. Specifically as follows: first, the temperature was raised to 150°C for 1 hour of heat treatment, then the temperature was raised to 250°C for 20 minutes for 1 hour of heat treatment, and finally the temperature was raised to 350°C for 20 minutes for 1.5 hours of heat treatment, and then naturally cooled to below 50°C in the oven to finally obtain a cured film. The silicon wafer with the film was immersed in 47% HF for 5 to 10 minutes, and then rinsed with water to obtain a photosensitive resin composition film.

[0159] The photosensitive resin composition film was cut into strips with a length of 1590 mm and a width of 103 mm, and the mechanical properties of the film, tensile strength, were tested using DMA (TA, DMA850). The tensile test rate was 3 N / min, and 5 strips were collected in each group. The highest and lowest values ​​were removed, and the remaining 3 values ​​were averaged to obtain the tensile strength.

[0160] 3. Glass transition temperature (Tg) test

[0161] The resin of the present application was subjected to a film forming test, and the obtained resin film with a film thickness of 10 to 20 μm was filled into an aluminum standard container, and the glass transition temperature (Tg) was measured using a differential scanning calorimeter DSC-250 (TA Instruments Waters, USA). Test conditions: pre-drying at 80°C, holding for 60 minutes, and then heating at a heating rate of 20°C / min for measurement.

[0162] 4. Adhesion test

[0163] The photosensitive resin composition samples of the above-mentioned embodiments and comparative examples were coated onto a 4-inch silicon wafer, and then soft-baked at 120°C for 3 minutes using a heating table to obtain a resin film with a film thickness of 15 μm. Full exposure was performed using an ultraviolet lamp (i and g lines) with an exposure amount of 400 mJ / cm-2. After exposure, spray development was performed using an alkaline developer, and the development time was 180 seconds. The film was then placed in a vacuum oxygen-free oven (Zhenping Technology Co., Ltd., MOLZK-32D1) for heat treatment. Specifically as follows: first, the temperature was raised to 150°C for 1 hour of heat treatment, then the temperature was raised to 250°C for 20 minutes for 1 hour of heat treatment, and finally the temperature was raised to 350°C for 20 minutes for 1.5 hours of heat treatment, and then it was naturally cooled to below 50°C in the oven, and finally a cured film attached to the silicon wafer was obtained. The cured film with silicon wafer was subjected to PCT treatment for 200 hours at 121°C and 2 atmospheres of saturated conditions using a pressure test (PCT) device, and then a single-edged knife was used to cut 10 rows and 10 columns of checkerboard cuts at 2 mm intervals on the cured film. The number of squares peeled off by peeling with transparent tape was counted to evaluate the adhesion. The case where the number of peeled off in the peeling test was less than 10 was set as A, the case where the number of peeled off was more than 10 and less than 20 was set as B, and the case where the number of peeled off was more than 20 was set as C.

[0164] The resolution, mechanical properties, Tg, and adhesion of the photosensitive resin compositions prepared in the examples and comparative examples were tested, and the test results are shown in Table 2:

[0165] Table 2

[0166]

[0167] It can be seen from the results of Examples 1 to 6 and Comparative Examples 1 and 2 that the resolution, tensile strength, Tg and adhesion of the photosensitive resin composition film containing a photopolymerizable compound having a triazinetrione structure are significantly better than those of the photosensitive resin composition film containing a photopolymerizable compound not having a triazinetrione structure, among which the photosensitive resin composition using the photopolymerizable compound of Example 3 has the best performance.

[0168] From the results of Examples 7-11, it can be seen that when the synthesized photopolymerizable compounds are combined in pairs (ratio 1:1), the photosensitive resin composition formed also has excellent resolution, tensile strength, Tg and adhesion. Among them, when C-4 and C-6 are combined, the resolution, tensile strength, elongation at break, Tg and adhesion of the obtained photosensitive composition are the best.

[0169] From the results of Examples 11-15, it can be seen that when the photopolymerizable compounds C-4 and C-6 containing triazinetrione are combined in different proportions, the resolution and tensile strength of the photosensitive resin composition formed are further improved. Among them, the combination of 18g of photopolymerizable C-4 and 10g of photopolymerizable C-6 has the best effect.

[0170] In Comparative Example 1, when PEG is used as the photopolymerizable compound in the photosensitive resin composition, although the system has good solubility, it has low resolution, low tg, poor adhesion, and low L tensile strength; in Comparative Example 2, when THEICTA is used as the photopolymerizable compound in the photosensitive resin composition, the resolution and Tg are higher than PEG, but are lower than those of the photosensitive resin composition in the embodiment, and the adhesion is poor, the system solubility is poor, and there are black spots.

[0171] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A triazinetrione compound containing a carbon-carbon double bond, It is characterized in that The triazinetrione compound has a structural formula shown in the following formula (1) or (2): In formula (1), R 1 is a phenyl group, an ester group, a hydrocarbon group having 1 to 10 carbon atoms, an alkoxy group, a halogen atom, or a hydrogen atom; R 2 It is a phenyl group, a carbonyl group, an ester group, a hydrocarbon group having 1 to 10 carbon atoms, or an alkoxy group; In formula (2), R 3 It is a cyclic hydrocarbon group having 3 to 10 carbon atoms and containing an unsaturated bond.

2. The triazinetrione compound containing a carbon-carbon double bond according to claim 1, It is characterized in that Reaction I of 1,3,5-tris(2-chloroethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione with the compound of formula (3) to obtain a compound of formula (1); Among them, R 1 and R 2 The definition of is consistent with that in claim 1; Reaction II of 1,3,5-tris(2-chloroethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione with the compound of formula (4) to obtain a compound of formula (2); H 2 N-R 3 Formula (4); Among them, R 3 The definition is consistent with that in claim 1.

3. The compound according to claim 2, It is characterized in that The reaction conditions of the reaction 1 are as follows: The reaction temperature of the reaction I is -5 to 80°C; The reaction time of the reaction I is 3 to 9 hours; Preferably, the reaction conditions of reaction II are as follows: The reaction temperature of the reaction II is -5 to 80°C; The reaction time of the reaction II is 3 to 9 hours.

4. A photosensitive resin composition, It is characterized in that It contains a polyimide precursor, a photoinitiator, a photopolymerizable compound containing an unsaturated bond, and a silane coupling agent; The photopolymerizable compound containing an unsaturated bond is selected from the triazinetrione compound containing a carbon-carbon double bond according to claim 1.

5. The photosensitive resin composition according to claim 4, It is characterized in that The preparation method of the polyimide precursor comprises the following steps: The tetracarboxylic dianhydride compound and the diamine compound are mixed and reacted to obtain a polyimide precursor.

6. The photosensitive resin composition according to claim 5, It is characterized in that The tetracarboxylic dianhydride compound is selected from at least one of pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride and 1,2,3,4-cyclobutanetetracarboxylic dianhydride; The diamine compound is selected from diamines having an aromatic ring; Preferably, the diamine of the aromatic ring includes at least one of a diamine having a hydroxyl group and an aromatic ring and a diamine having a carboxyl group and an aromatic ring; The reaction conditions of the reaction are as follows: The tetracarboxylic dianhydride compound and the diamine compound are reacted in a ratio of 1:0.5 to 1:1; The reaction temperature is 25 to 180°C; The reaction time is 1 to 5 hours.

7. The photosensitive resin composition according to claim 4, It is characterized in that The polyimide precursor is 100 parts by mass as a measurement basis; Photoinitiator 0.01 to 30 parts by weight; 1 to 100 parts by weight of a photopolymerizable compound containing an unsaturated bond; Silane coupling agent 0.01 to 1 parts by mass; The polyimide precursor is selected from at least one of polyamic acid, polyamide ester and polyimide; The photoinitiator is selected from at least one of benzophenone compounds, benzylidene compounds, coumarin compounds, anthraquinone compounds, benzoin compounds, thioxanthone compounds, thiol compounds, glycine compounds, oxime compounds, α-aminoalkylphenone compounds, 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, and phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide; The silane coupling agent is selected from at least one of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, bis(γ-aminopropyl)tetramethylsiloxane, bis(γ-aminobutyl)tetramethylsiloxane, bis(γ-aminopropyl)tetraphenylsiloxane, bis(γ-aminopropyl)tetraphenylpolysiloxane, bis(γ-aminopropyl)tetraphenylsiloxane, bis(γ-aminobutyl)tetraphenylpolysiloxane, 3-(2,3-epoxypropyloxy)propyltriethoxysilane and vinyltriethoxysilane.

8. The photosensitive resin composition according to claim 4, It is characterized in that The photosensitive resin composition further contains epoxy compounds and / or photopolymerizable compounds of other structures; Preferably, based on 100 parts by mass of the polyimide precursor: 1 to 100 parts by mass of other photopolymerizable compounds and / or epoxy compounds; Preferably, the epoxy compound of other structures is selected from at least one of bisphenol A epoxy compounds, novolac epoxy compounds, biphenol epoxy compounds, bisphenol F glycidyl ether epoxy compounds, cyclic aliphatic epoxy compounds, heterocyclic epoxy compounds, and aromatic epoxy compounds; The photopolymerizable compound of other structures is selected from diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane diacrylate, trimethylolpropane dimethacrylate, trimethylolpropane trimethacrylate, styrene, α-methylstyrene, 1,2-dihydronaphthalene, 1,3-diisopropenylbenzene, 3-methylstyrene, 4-methylstyrene, p-vinylbenzene, 2-vinylnaphthalene, butyl acrylate, butyl methacrylate Ester, isobutyl acrylate, hexyl acrylate, isooctyl acrylate, isobornyl acrylate, isobornyl methacrylate, cyclohexyl methacrylate, 1,3-butanediol diacrylate, 1,3-butanediol dimethacrylate, neopentyl glycol diacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, 1,10-decanediol dimethacrylate, tricyclodecane dimethanol diacrylate, pentaerythritol Pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, dipentaerythritol hexaacrylate, dipentaerythritol hexamethacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 1,3-diacryloxy-2-hydroxypropane, 1,3-dimethacryloxy-2-hydroxypropane, methylenebisacrylamide, N,N-dimethylacrylamide, N-hydroxymethylacrylamide, 2,2,6,6-tetramethylpiperidinyl methacrylate, N-methyl-2,2,6, At least one of 6-tetramethylpiperidinyl acrylate, N-methyl-2,2,6,6-tetramethylpiperidinyl methacrylate, N-methyl-2,2,6,6-tetramethylpiperidinyl acrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, propoxylated bisphenol A diacrylate, propoxylated bisphenol A methacrylate, propoxylated ethoxylated bisphenol A diacrylate, propoxyethoxylated bisphenol A dimethacrylate, N-vinyl caprolactam, polyethylene glycol diacrylate, and 2-isocyanatoethyl methacrylate; Preferably, the photosensitive resin composition further contains a solvent; Preferably, based on 100 parts by mass of the polyimide precursor: 50 to 1000 parts by weight of solvent; Preferably, the solvent is selected from at least one of N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, N-vinylpyrrolidone, N,N-diethylformamide, γ-butyrolactone, ethyl lactate, methyl monoglyme, methyl diglyme, methyl triglyme, ethyl monoglyme, ethyl diglyme, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol dimethyl ether, and ethylene glycol diethyl ether.

9. The photosensitive resin composition according to claim 4, It is characterized in that The photosensitive resin composition is coated on a substrate, the substrate is heated to form a photosensitive resin layer, and the photosensitive resin layer is exposed, developed, and heated to form a cured film.

10. An electronic component or a semiconductor device, It is characterized in that The electronic component or semiconductor device is obtained by bonding a plurality of substrates or bonding a substrate to another member via the cured film of the photosensitive resin composition according to any one of claims 4 to 8.

Citation Information

Patent Citations

  • Photosensitive adhesive composition, photosensitive adhesive film, and semiconductor device using each

    CN102985505B

  • Resin composition containing polyimide precursor and method for manufacturing cured film using said resin composition

    CN105829968A

  • Photosensitive resin composition, method for manufacturing cured relief pattern, and semiconductor apparatus

    CN107850844A

  • Highly heat-resistant, negative-type photosensitive resin composition

    CN1668980B

  • Resin composition containing polyimide precursor, method for manufacturing cured film, and electronic component

    CN106462065A