Multifunctional flexible alicyclic epoxy resin and preparation method thereof

By introducing a flexible chain-end toughening structure into alicyclic epoxy resin, the problems of material brittleness and processing difficulties are solved, high toughness and stability are improved, and it is suitable for encapsulation glue of OLED devices.

CN118812464APending Publication Date: 2024-10-22JIANGSU TETRA NEW MATERIAL TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410890097.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing alicyclic epoxy resins in packaging materials have problems such as high brittleness, difficult processing and unstable performance, making it difficult to meet the high toughness, heat resistance and flexibility requirements of OLED equipment.

Method used

Using multifunctional flexible alicyclic epoxy resin and its preparation method, an ester intermediate with multiple double bonds is generated through the reaction of ethoxylated polyol and 3-cyclohexenecarboxylic acid, and is epoxidized. Introducing a flexible chain end toughening structure to improve the toughness and stability of the polymer chain.

Benefits of technology

It effectively reduces the brittleness of the material, improves the toughness and stability, significantly improves the flexibility of the system, and is suitable for high-demand OLED encapsulants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118812464A_ABST
    Figure CN118812464A_ABST
Patent Text Reader

Abstract

The invention discloses multifunctional flexible alicyclic epoxy resin and a preparation method thereof. The preparation method comprises the following steps: step one, enabling ethoxylated polyol to react with 3-cyclohexenecarboxylic acid in a reactor; 2, generating an ester intermediate with a plurality of double bonds in the step 1; 3, double bonds in the intermediate molecules obtained in the step 2 are epoxidized, and the multifunctional alicyclic epoxy resin is obtained. The preparation method has the beneficial effects that a method for toughening by introducing a flexible chain end is adopted, and a flexible chain segment is introduced into a macromolecular chain, so that the brittleness is reduced, and the toughness is improved; the toughening structure and the epoxy structure are connected through chemical bonding force, and after macromolecules are generated, the toughening structure can stably stay in a cured material and does not dissociate to the surface of a product, so that the toughness of the system is stable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of epoxy resin preparation, in particular to multifunctional flexible alicyclic epoxy resin and a preparation method thereof. Background Art

[0002] Organic light-emitting displays (OLEDs) have the advantages of high brightness, good color performance, wide viewing angle, and fast driving, and have been widely used in the display industry. However, since OLEDs use polymer or small molecule organic materials to emit light under the action of an electric field, when they are exposed to an environment containing oxygen and water vapor, the luminescent materials will be corroded to form black spots, which directly affects the use of OLED devices. In order to prevent the luminescent materials from being corroded, they must be encapsulated inside the device. OLED electronic devices have gone through the process of traditional cover-type encapsulation to flexible thin film encapsulation. Conventional encapsulation of traditional glass or metal cover plates is relatively expensive, which also limits the development of large display devices.

[0003] Cycloaliphatic epoxy resins have excellent processability, dielectric properties, thermal stability and adhesion, which makes them have good application prospects in the field of electronic packaging. In particular, the application of folding screens, curved screens and scroll screen displays in recent years has made the research and application of electronic devices develop towards thinness and flexibility, and has also put forward higher requirements for the properties of thin film packaging materials such as high temperature resistance, thermal shock resistance, flexibility, high tear resistance, gas permeability, and light transmittance. Due to the rigid structure and high cross-linking density of cycloaliphatic epoxy resins, the cured packaging materials are brittle. Therefore, it is necessary to strengthen and toughen the cycloaliphatic epoxy resins.

[0004] In the past few decades, people have made great efforts in toughening epoxy resins, but there are still many problems. For example, rubber elastomers and core-shell polymers reduce the modulus and heat resistance of epoxy resins while toughening; liquid crystal polymers can not only significantly improve toughness but also maintain modulus and heat resistance, but their weak solubility, compatibility and poor fluidity in epoxy resins make them difficult to process; nanomaterials will agglomerate during toughening and are difficult to disperse evenly in the matrix, resulting in unstable product performance, etc. In view of some drawbacks and shortcomings in the toughening design of epoxy resins, seeking composite materials with better comprehensive performance has become the main aspect of epoxy resin toughening research. Summary of the invention

[0005] The purpose of the present invention is to solve the above problems and to design a multifunctional flexible alicyclic epoxy resin and a preparation method thereof.

[0006] The technical solution of the present invention to achieve the above-mentioned purpose is to provide a multifunctional flexible alicyclic epoxy resin and a preparation method thereof. 1. The multifunctional flexible alicyclic epoxy resin is characterized in that it comprises compound I, compound II, and compound III, and the structural formulas of compound I, compound II, and compound III are as follows:

[0007]

[0008] As a further description of the technical solution, in the compound I, n is 4 on average.

[0009] As a further description of the technical solution, in the compound II, n is 6 on average.

[0010] As a further description of the technical solution, in the compound III, n is 6 on average.

[0011] The preparation method of a multifunctional flexible alicyclic epoxy resin comprises the following steps:

[0012] Step 1: reacting 3-cyclohexenecarboxylic acid with ethoxylated polyol in a reactor;

[0013] Step 2: generating an ester intermediate with multiple double bonds by step 1;

[0014] Step 3: epoxidizing the double bonds in the intermediate molecule obtained in step 2 to obtain a multifunctional alicyclic epoxy resin.

[0015] As a further description of the technical solution, the preparation method of compound I is as follows: 200 g of pentaerythritol ethoxylate, 140.4 g of 3-cyclohexenecarboxylic acid, 1.6 g of methanesulfonic acid and 600 g of toluene are added to a 2000 ml dry three-necked round-bottom flask with a condensing reflux device, the flask is placed in an oil bath, the temperature is raised to 120° C., and the reaction is stirred for 6 hours;

[0016] Detect the acid value of the reaction solution. After the reaction is qualified, add 200g of 5% sodium hydroxide solution to wash for 10min; separate the lower aqueous phase, and wash the organic phase with 200g of deionized water again;

[0017] The washed organic phase was desolventized to obtain 308.6g of light yellow liquid; the light yellow liquid obtained above, 600g of ethyl acetate and 16.7g of anhydrous sodium acetate were added to a 2000mL three-necked round-bottom flask, placed in a water bath, cooled to 15°C, and 190g of 23% peracetic acid solution prepared in advance was added dropwise; during the addition, the reaction temperature was maintained at 20-25°C; after the addition was completed, the reaction was kept at 25±3°C for 10h; after the reaction was completed, the aqueous phase was separated, and the organic phase was washed with 200g of deionized water, 200g of 10% liquid alkali and 200g of deionized water respectively. The organic phase with qualified aqueous phase was desolventized to obtain 285.7g of compound I product; it was a colorless and transparent liquid with an epoxy equivalent of 370 and a viscosity (25°C) of 1620cps.

[0018] As a further description of the technical solution, the preparation method of compound II is as follows: 200 g of triethoxylated trimethylolpropane, 82 g of 3-cyclohexenecarboxylic acid, 0.9 g of methanesulfonic acid and 600 g of toluene are added to a 2000 ml dry three-necked round-bottom flask with a condensing reflux device, the flask is placed in an oil bath, the temperature is raised to 120° C., and the reaction is stirred for 22 hours;

[0019] Detect the acid value of the reaction solution. After the reaction is qualified, add 200g of 5% sodium hydroxide solution to wash for 10min; separate the lower aqueous phase, and wash the organic phase with 200g of deionized water again;

[0020] After washing the organic phase, 263.8 g of light yellow liquid was obtained after desolventizing. The light yellow liquid obtained above, 600 g of ethyl acetate and 9.7 g of anhydrous sodium acetate were added to a 2000 mL three-necked round-bottom flask, placed in a water bath, cooled to 15°C, and 112.4 g of 23% peracetic acid solution prepared in advance was added dropwise; during the addition, the reaction temperature was maintained at 20-25°C; after the addition was completed, the temperature was kept at 25±3°C for 9 hours; after the reaction was completed, the aqueous phase was separated, and the organic phase was washed with 200 g of deionized water, 200 g of 10% liquid alkali and 200 g of deionized water respectively; the organic phase with qualified aqueous phase was desolventized to obtain 196.9 g of compound II product; it was a light yellow transparent liquid with an epoxy equivalent of 678 and a viscosity (25°C) of 358 cps.

[0021] As a further description of the technical solution, the preparation method of compound III is as follows: 200 g of triethoxylated glycerol, 83.3 g of 3-cyclohexenecarboxylic acid, 0.9 g of methanesulfonic acid and 600 g of toluene are added to a 2000 ml dry three-necked round-bottom flask with a condensing reflux device, the flask is placed in an oil bath, the temperature is raised to 120° C., and the reaction is stirred for 21 hours;

[0022] Detect the acid value of the reaction solution. After the reaction is qualified, add 200g of 5% sodium hydroxide solution to wash for 10min; separate the lower aqueous phase, and wash the organic phase with 200g of deionized water again;

[0023] After washing the organic phase, 262.9 g of yellow liquid was obtained after desolventizing. The light yellow liquid obtained above, 600 g of ethyl acetate and 9.9 g of anhydrous sodium acetate were added to a 2000 mL three-necked round-bottom flask, placed in a water bath, cooled to 15°C, and 114.3 g of 23% peracetic acid solution prepared in advance was added dropwise; during the addition, the reaction temperature was maintained at 20-25°C; after the addition was completed, the temperature was kept at 25±3°C for 9 hours; after the reaction was completed, the aqueous phase was separated, and the organic phase was washed with 200 g of deionized water, 200 g of 10% liquid alkali and 200 g of deionized water respectively; the organic phase with qualified aqueous phase was desolventized to obtain 220.5 g of compound III product; it was a yellow transparent liquid with an epoxy equivalent of 682 and a viscosity (25°C) of 613 cps.

[0024] Its beneficial effect lies in that the present invention adopts a method of introducing flexible chain ends for toughening, so that flexible chain segments are introduced into the polymer chain, thereby reducing brittleness and improving toughness; the toughening structure is connected to the epoxy structure by chemical bonding force, and after the polymer is generated, the toughening structure can stay stably in the solidified material and will not be free to the surface of the product, thereby making the toughness of the system stable; the alicyclic epoxy resin of the present technical solution is used as an active toughening resin in combination with other alicyclic epoxy resins, which can effectively improve the flexibility of the resin composition, which is a better choice for OLED encapsulation adhesives with special requirements for toughness. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is the reaction equation diagram of compound Ⅰ;

[0026] Figure 2 It is the reaction equation diagram of compound II;

[0027] Figure 3 It is the reaction equation diagram of compound III;

[0028] Figure 4 This is the GPC test chart of compound Ⅰ;

[0029] Figure 5 This is the GPC test chart of compound II;

[0030] Figure 6 This is the GPC detection chart of compound III. DETAILED DESCRIPTION

[0031] The present invention will be described in detail below in conjunction with the accompanying drawings. Figure 1-Figure 6As shown, the multifunctional flexible alicyclic epoxy resin includes compound I, compound II, and compound III. The structural formulas of compound I, compound II, and compound III are as follows:

[0032]

[0033]

[0034] In the compound I, n is 4 on average.

[0035] In the compound II, n is 6 on average.

[0036] In said compound III, n is 6 on average.

[0037] The preparation method of the multifunctional flexible alicyclic epoxy resin is described below, comprising the following steps:

[0038] Step 1: reacting 3-cyclohexenecarboxylic acid with ethoxylated polyol in a reactor;

[0039] Step 2: generating an ester intermediate with multiple double bonds by step 1;

[0040] Step 3: epoxidizing the double bonds in the intermediate molecule obtained in step 2 to obtain a multifunctional alicyclic epoxy resin.

[0041] The preparation of compound I, compound II and compound III will be described in detail below in conjunction with the examples;

[0042] The preparation method of compound I is as follows: 200 g of pentaerythritol ethoxylate, 140.4 g of 3-cyclohexenecarboxylic acid, 1.6 g of methanesulfonic acid and 600 g of toluene are added to a 2000 ml dry three-necked round-bottom flask with a condensing reflux device, the flask is placed in an oil bath, the temperature is raised to 120° C., and the reaction is stirred for 6 hours;

[0043] Detect the acid value of the reaction solution. After the reaction is qualified, add 200g of 5% sodium hydroxide solution to wash for 10min; separate the lower aqueous phase, and wash the organic phase with 200g of deionized water again;

[0044] The washed organic phase was desolventized to obtain 308.6g of light yellow liquid; the light yellow liquid obtained above, 600g of ethyl acetate and 16.7g of anhydrous sodium acetate were added to a 2000mL three-necked round-bottom flask, placed in a water bath, cooled to 15°C, and 190g of 23% peracetic acid solution prepared in advance was added dropwise; during the addition, the reaction temperature was maintained at 20-25°C; after the addition was completed, the reaction was kept at 25±3°C for 10h; after the reaction was completed, the aqueous phase was separated, and the organic phase was washed with 200g of deionized water, 200g of 10% liquid alkali and 200g of deionized water respectively. The organic phase with qualified aqueous phase was desolventized to obtain 285.7g of compound I product; it was a colorless and transparent liquid with an epoxy equivalent of 370 and a viscosity (25°C) of 1620cps; the reaction equation of compound I is as follows Figure 1 shown.

[0045] The preparation method of compound II is as follows: 200 g of triethoxylated trimethylolpropane, 82 g of 3-cyclohexenecarboxylic acid, 0.9 g of methanesulfonic acid and 600 g of toluene are added to a 2000 ml dry three-necked round-bottom flask with a condensing reflux device, the flask is placed in an oil bath, the temperature is raised to 120° C., and the reaction is stirred for 22 hours;

[0046] Detect the acid value of the reaction solution. After the reaction is qualified, add 200g of 5% sodium hydroxide solution to wash for 10min; separate the lower aqueous phase, and wash the organic phase with 200g of deionized water again;

[0047] The washed organic phase was desolventized to obtain 263.8g of light yellow liquid. The light yellow liquid obtained above, 600g of ethyl acetate and 9.7g of anhydrous sodium acetate were added to a 2000mL three-necked round-bottom flask, placed in a water bath, cooled to 15°C, and 112.4g of 23% peracetic acid solution prepared in advance was added dropwise; during the addition, the reaction temperature was maintained at 20-25°C; after the addition was completed, the reaction was kept at 25±3°C for 9h; after the reaction was completed, the aqueous phase was separated, and the organic phase was washed with 200g of deionized water, 200g of 10% liquid alkali and 200g of deionized water respectively; the organic phase with qualified aqueous phase was desolventized to obtain 196.9g of compound II product; it was a light yellow transparent liquid with an epoxy equivalent of 678 and a viscosity (25°C) of 358cps; the reaction equation of compound II is as follows Figure 2 shown.

[0048] The preparation method of compound III is as follows: 200 g of triethoxylated glycerol, 83.3 g of 3-cyclohexenecarboxylic acid, 0.9 g of methanesulfonic acid and 600 g of toluene are added to a 2000 ml dry three-necked round-bottom flask equipped with a condensation reflux device, the flask is placed in an oil bath, the temperature is raised to 120° C., and the reaction is stirred for 21 hours;

[0049] Detect the acid value of the reaction solution. After the reaction is qualified, add 200g of 5% sodium hydroxide solution to wash for 10min; separate the lower aqueous phase, and wash the organic phase with 200g of deionized water again;

[0050] The washed organic phase was desolventized to obtain 262.9 g of yellow liquid. The light yellow liquid obtained above, 600 g of ethyl acetate and 9.9 g of anhydrous sodium acetate were added to a 2000 mL three-necked round-bottom flask, placed in a water bath, cooled to 15°C, and 114.3 g of a 23% peracetic acid solution prepared in advance was added dropwise; during the addition, the reaction temperature was maintained at 20-25°C; after the addition was completed, the reaction was kept at 25±3°C for 9 hours; after the reaction was completed, the aqueous phase was separated, and the organic phase was washed with 200 g of deionized water, 200 g of 10% liquid alkali and 200 g of deionized water respectively; the organic phase with qualified aqueous phase was desolventized to obtain 220.5 g of compound III product; it was a yellow transparent liquid with an epoxy equivalent of 682 and a viscosity (25°C) of 613 cps; the reaction equation of compound III is as follows Figure 3 shown.

[0051] The application of the multifunctional flexible alicyclic epoxy resin of the present invention is described below: Compound I, Compound II and Compound III are respectively mixed with TTA21 (3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexylcarboxylate) in proportion, and then an active diluent and a cationic initiator are added to measure the curing speed and the hardness and toughness of the cured product; the raw material ratio and the test results are shown in Table 1.

[0052] The test data show that the surface dry energy of compound I, compound II and is relatively high, indicating that their curing speed is relatively slow; for photocurable adhesives and photocurable inks, they cannot be used alone as a base resin; however, after compounding with TTA21, the flexibility of the cured product is significantly improved; judging from the curing speed and cured product hardness data, the performance of compound I is better than that of compound II and compound III.

[0053] In general, the use of compound I, compound II and compound III as active toughening resins in combination with other alicyclic epoxy resins can effectively improve the flexibility of the resin composition, which is undoubtedly a better choice for OLED encapsulation adhesives with special requirements for toughness.

[0054] Table 1 Compound photocuring performance data table

[0055]

[0056] The present invention adopts a method of introducing flexible chain ends for toughening, so that flexible chain segments are introduced into the polymer chain, thereby reducing brittleness and improving toughness; the toughening structure is connected to the epoxy structure by chemical bonding force, and after the polymer is generated, the toughening structure can stay stably in the solidified material and will not be free to the surface of the product, thereby making the toughness of the system stable; the alicyclic epoxy resin of the present technical solution is used as an active toughening resin in combination with other alicyclic epoxy resins, which can effectively improve the flexibility of the resin composition, which is a better choice for OLED encapsulation adhesives with special requirements for toughness.

[0057] The above technical solutions only reflect the preferred technical solutions of the technical solutions of the present invention. Some changes that may be made to certain parts thereof by technicians in this technical field all reflect the principles of the present invention and fall within the protection scope of the present invention.

Claims

1. A multifunctional flexible alicyclic epoxy resin, characterized in that: Including compound I, compound II, compound III, the structural formulas of compound I, compound II, and compound III are as follows:

2. The multifunctional flexible alicyclic epoxy resin according to claim 1, characterized in that: In the compound I, n is 4 on average.

3. The multifunctional flexible alicyclic epoxy resin according to claim 1, characterized in that: In the compound II, n is 6 on average.

4. The multifunctional flexible alicyclic epoxy resin according to claim 1, characterized in that: In the compound III, n is 6 on average.

5. A method for preparing a multifunctional flexible alicyclic epoxy resin as claimed in claim 1, characterized in that: The following steps are involved: Step 1: reacting 3-cyclohexenecarboxylic acid with ethoxylated polyol in a reactor; Step 2: generating an ester intermediate with multiple double bonds by step 1; Step 3: epoxidizing the double bonds in the intermediate molecule obtained in step 2 to obtain a multifunctional alicyclic epoxy resin.

6. The method for preparing a multifunctional flexible alicyclic epoxy resin according to claim 5, characterized in that: The preparation method of compound I is as follows: 200 g of pentaerythritol ethoxylate, 140.4 g of 3-cyclohexenecarboxylic acid, 1.6 g of methanesulfonic acid and 600 g of toluene are added to a 2000 ml dry three-necked round-bottom flask with a condensing reflux device, the flask is placed in an oil bath, the temperature is raised to 120° C., and the reaction is stirred for 6 hours; Detect the acid value of the reaction solution. After the reaction is qualified, add 200g of 5% sodium hydroxide solution to wash for 10min; separate the lower aqueous phase, and wash the organic phase with 200g of deionized water again; The washed organic phase was desolventized to obtain 308.6g of light yellow liquid; the light yellow liquid obtained above, 600g of ethyl acetate and 16.7g of anhydrous sodium acetate were added to a 2000mL three-necked round-bottom flask, placed in a water bath, cooled to 15°C, and 190g of 23% peracetic acid solution prepared in advance was added dropwise; during the addition, the reaction temperature was maintained at 20-25°C; after the addition was completed, the reaction was kept at 25±3°C for 10h; after the reaction was completed, the aqueous phase was separated, and the organic phase was washed with 200g of deionized water, 200g of 10% liquid alkali and 200g of deionized water respectively. The organic phase with qualified aqueous phase was desolventized to obtain 285.7g of compound I product; it was a colorless and transparent liquid with an epoxy equivalent of 370 and a viscosity (25°C) of 1620cps.

7. The method for preparing a multifunctional flexible alicyclic epoxy resin according to claim 5, characterized in that: The preparation method of compound II is as follows: 200 g of triethoxylated trimethylolpropane, 82 g of 3-cyclohexenecarboxylic acid, 0.9 g of methanesulfonic acid and 600 g of toluene are added to a 2000 ml dry three-necked round-bottom flask with a condensing reflux device, the flask is placed in an oil bath, the temperature is raised to 120° C., and the reaction is stirred for 22 hours; Detect the acid value of the reaction solution. After the reaction is qualified, add 200g of 5% sodium hydroxide solution to wash for 10 minutes; separate the lower aqueous phase, and wash the organic phase with 200g of deionized water again; After washing the organic phase, 263.8 g of light yellow liquid was obtained after desolventizing. The light yellow liquid obtained above, 600 g of ethyl acetate and 9.7 g of anhydrous sodium acetate were added to a 2000 mL three-necked round-bottom flask, placed in a water bath, cooled to 15°C, and 112.4 g of 23% peracetic acid solution prepared in advance was added dropwise; during the addition, the reaction temperature was maintained at 20-25°C; after the addition was completed, the temperature was kept at 25±3°C for 9 hours; after the reaction was completed, the aqueous phase was separated, and the organic phase was washed with 200 g of deionized water, 200 g of 10% liquid alkali and 200 g of deionized water respectively; the organic phase with qualified aqueous phase was desolventized to obtain 196.9 g of compound II product; it was a light yellow transparent liquid with an epoxy equivalent of 678 and a viscosity (25°C) of 358 cps.

8. The method for preparing a multifunctional flexible alicyclic epoxy resin according to claim 5, characterized in that: The preparation method of compound III is as follows: 200 g of triethoxylated glycerol, 83.3 g of 3-cyclohexenecarboxylic acid, 0.9 g of methanesulfonic acid and 600 g of toluene are added to a 2000 ml dry three-necked round-bottom flask equipped with a condensation reflux device, the flask is placed in an oil bath, the temperature is raised to 120° C., and the reaction is stirred for 21 hours; Detect the acid value of the reaction solution. After the reaction is qualified, add 200g of 5% sodium hydroxide solution to wash for 10 minutes; separate the lower aqueous phase, and wash the organic phase with 200g of deionized water again; After washing the organic phase, 262.9 g of yellow liquid was obtained after desolventizing. The light yellow liquid obtained above, 600 g of ethyl acetate and 9.9 g of anhydrous sodium acetate were added to a 2000 mL three-necked round-bottom flask, placed in a water bath, cooled to 15°C, and 114.3 g of 23% peracetic acid solution prepared in advance was added dropwise; during the addition, the reaction temperature was maintained at 20-25°C; after the addition was completed, the temperature was kept at 25±3°C for 9 hours; after the reaction was completed, the aqueous phase was separated, and the organic phase was washed with 200 g of deionized water, 200 g of 10% liquid alkali and 200 g of deionized water respectively; the organic phase with qualified aqueous phase was desolventized to obtain 220.5 g of compound III product; it was a yellow transparent liquid with an epoxy equivalent of 682 and a viscosity (25°C) of 613 cps.

Citation Information

Cited By

  • A crack-resistant, high-temperature resistant epoxy potting compound, its preparation method and application

    CN122668682A

  • Anti-cracking, high-temperature-resistant epoxy potting adhesive, preparation method and application thereof

    CN122668682B