Rubber sealing gasket as well as preparation method and application thereof
By using a specific ratio of carbon black and plasticizer in the rubber sealing gasket, the problem of swelling and extraction of the rubber sealing gasket in the propellant in the aerosol valve is solved, the sealing performance is improved, and the risk of leakage is reduced. Meets the requirements for use of aerosol valve systems.
Patent Information
- Application Number
- CN202310429227.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-22
AI Technical Summary
The rubber sealing gasket in the aerosol valve is prone to swelling and extraction when in contact with the propellant, leading to a decrease in sealing performance, increasing the risk of leakage, and affecting product safety.
A rubber sealing gasket formula with a specific ratio is used, including rubber, semi-reinforced carbon black, rapid extrusion carbon black, medium particle thermal cracking carbon black, liquid plasticizer and waxy plasticizer. Through compounding and Vulcanization treatment controls the amount of carbon black and plasticizer to improve the swelling rate and mechanical properties of the material in the propellant.
It significantly reduces the swelling rate of the rubber sealing gasket in the propellant, improves the sealing performance, reduces the risk of leakage, and meets the usage requirements of aerosol valve systems.
Smart Images

Figure BDA0004189839550000161 
Figure BDA0004189839550000171 
Figure BDA0004189839550000172
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber sealing materials, and in particular to a rubber sealing gasket and a preparation method and application thereof. Background Art
[0002] As an important part of the pressure packaging of aerosol products, aerosol valves will have a certain risk of leakage under the pressure in the can. Therefore, the leakage of propellants may cause safety hazards during the production, storage, transportation and use of aerosols. Usually, the aerosol valve is called the heart of the aerosol product, and the rubber gasket in the valve is called the heart of the valve. It can be seen that the rubber gasket is important to aerosol products. Through the analysis of the common valve structure of aerosols, it can be seen that there are three main ways for the valve to leak. The first is the radial fit between the inner gasket of the valve and the valve core; the second is the plane joint between the inner gasket and the top of the fixed cover; the third is the plane contact part between the fixed cover and the aerosol can. From the above, it can be seen that the rubber material of the inner gasket of the valve is closely related to the leakage of the propellant, which is directly related to the safety of aerosol products.
[0003] The elastomer seals used in aerosol valve systems are usually traditional chloroprene rubber, butyl rubber, or nitrile rubber, and the propellants are mostly liquefied petroleum gas LPG (a mixture of propane and butane) and DME (dimethyl ether). LPG and DME are gases at room temperature and pressure, but they are easily liquefied when pressurized and cooled. Rubber sealing gaskets are prone to swelling and extraction when in contact with propellants. Swelling refers to the propellant entering the interior of the sealing material, which increases the volume of the sealing material, causing the valve stem of the valve to tend to become sticky, pause or drag during operation, making the operation of the valve difficult; extraction refers to the propellant entering the interior of the sealing material dissolving the plasticizer components contained in the sealing material and then releasing them to the outside of the sealing material. Since the extracted plasticizer components cannot return to the interior of the sealing material, the sealing material will lose its flexibility and its volume will decrease, leaving a gap in the installation part sealed by the sealing material, and gas or liquid may leak. Therefore, how to reduce swelling and extraction phenomena so that the rubber gasket can meet the swelling rate requirements in the propellant has become a difficult problem to be solved urgently in the field. Summary of the invention
[0004] The object of the present invention is to provide a rubber sealing gasket and a preparation method and application thereof. The rubber sealing gasket provided by the present invention has a low swelling rate in the propellant and can meet the swelling rate requirement in the propellant.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The invention provides a rubber sealing gasket, which is prepared from the following raw materials in percentage by mass: 30-60wt% of rubber, 10-25wt% of semi-reinforced carbon black, 15-35wt% of fast extrusion carbon black, 3-15wt% of medium-particle thermal cracking carbon black, 0.6-6.0wt% of liquid plasticizer, 0.3-0.8wt% of waxy plasticizer, 2.0-3.2wt% of vulcanization accelerating agent, 0.1-1.8wt% of vulcanization accelerator, 0.5-1.5wt% of antioxidant and 0.3-1.0wt% of vulcanizing agent.
[0007] Preferably, it is prepared from raw materials including the following mass percentages: 43.4-57.4wt% of nitrile rubber, 10-18wt% of semi-reinforced carbon black, 15-25wt% of quick extrusion carbon black, 3-8wt% of medium particle thermal cracking carbon black, 2-5wt% of inorganic salt filler, 0.6-1.0wt% of liquid plasticizer, 0.3-0.6wt% of waxy plasticizer, 2.0-3.2wt% of vulcanization accelerator, 0.3-1.8wt% of vulcanization accelerator, 0.5-1.5wt% of antioxidant and 0.3-1.0wt% of vulcanizing agent;
[0008] Alternatively, the method is prepared from the following raw materials in percentage by weight: 44-59 wt% of chloroprene rubber, 10-18 wt% of semi-reinforced carbon black, 15-25 wt% of quick extrusion carbon black, 3-10 wt% of medium particle thermal cracking carbon black, 2.0 wt% of acid absorbent, 2.5-6.0 wt% of liquid plasticizer, 0.3-0.8 wt% of waxy plasticizer, 2.0-3.2 wt% of vulcanization accelerator, 0.1-1.8 wt% of vulcanization accelerator, 0.5-1.5 wt% of antioxidant and 0.3-1.0 wt% of vulcanizing agent;
[0009] Alternatively, the method is prepared from raw materials comprising the following weight percentages: 33-53wt% of butyl rubber, 15-25wt% of semi-reinforcing carbon black, 20-35wt% of quick extrusion carbon black, 3-15wt% of medium particle thermal cracking carbon black, 1.0-2.0wt% of liquid plasticizer, 0.3-0.8wt% of waxy plasticizer, 2.0-3.2wt% of vulcanization accelerating agent, 0.3-1.8wt% of vulcanization accelerator, 0.5-1.5wt% of antioxidant and 0.3-1.0wt% of vulcanizing agent.
[0010] Preferably, the semi-reinforcing carbon black is one of carbon black N754, carbon black N762, carbon black N765, carbon black N770, carbon black N772, carbon black N774 and carbon black N787.
[0011] Preferably, the fast extrusion carbon black is one of carbon black N539, carbon black N542, carbon black N550 and carbon black N568.
[0012] Preferably, the medium particle thermal cracking carbon black is carbon black N990.
[0013] Preferably, the inorganic salt filler is at least one of calcium carbonate, talc and kaolin.
[0014] Preferably, the liquid plasticizer is at least one of white oil, paraffin oil, adipic acid esters and phthalic acid esters; and the waxy plasticizer is at least one of vaseline and fatty acid metal salts.
[0015] Preferably, the vulcanization accelerating aids are zinc oxide and stearic acid, and the mass ratio of zinc oxide to stearic acid is 5:1.
[0016] The present invention also provides a method for preparing the rubber sealing gasket described in the above technical solution, comprising the following steps:
[0017] (1) plasticizing the rubber to obtain plasticized rubber;
[0018] (2) mixing the plasticized rubber obtained in step (1) with semi-reinforcing carbon black, fast extrusion carbon black, medium-particle thermal cracking carbon black, liquid plasticizer, waxy plasticizer, vulcanization accelerator, antioxidant, vulcanization accelerator and vulcanizing agent, and mixing, extruding and calendering in sequence to obtain a film;
[0019] (3) vulcanizing the rubber obtained in step (2) to obtain a rubber sealing gasket;
[0020] When the raw materials include an inorganic salt filler, the inorganic salt filler is added in step (2);
[0021] When the raw material includes an acid absorbent, the acid absorbent is added in step (2).
[0022] The present invention also provides the use of the rubber sealing gasket described in the above technical solution or the rubber sealing gasket prepared by the preparation method in an aerosol valve.
[0023] The invention provides a rubber sealing gasket, which is prepared from the following raw materials in mass percentage: 30-60wt% of rubber, 10-25wt% of semi-reinforcing carbon black, 15-35wt% of fast extrusion carbon black, 3-15wt% of medium-particle thermal cracking carbon black, 0.6-6.0wt% of liquid plasticizer, 0.3-0.8wt% of waxy plasticizer, 2.0-3.2wt% of vulcanization accelerator, 0.1-1.8wt% of vulcanization accelerator, 0.5-1.5wt% of antioxidant and 0.3-1.0wt% of vulcanizing agent. The invention uses semi-reinforcing carbon black, fast extrusion carbon black and medium-particle thermal cracking carbon black as reinforcing agents, and controls the quality of the three kinds of carbon black to improve the swelling rate of the material in the propellant; the plasticizer uses a liquid plasticizer and a waxy plasticizer in combination, and controls the amount of the plasticizer, so that the rubber sealing gasket can meet the swelling rate requirement in the propellant. Experimental results show that the LPG thickness swelling rate of the nitrile rubber sealing gasket provided by the present invention is 2.0-10.0%, and the DME thickness swelling rate is 18.0-29.0%; the LPG thickness swelling rate of the chloroprene rubber sealing gasket is 1.0-6.0%, and the DME thickness swelling rate is 9.90-16.0%; the LPG thickness swelling rate of the butyl rubber sealing gasket is 10.0-23.0%, and the DME thickness swelling rate is 5.0-12.0%. DETAILED DESCRIPTION
[0024] The invention provides a rubber sealing gasket, which is prepared from the following raw materials in percentage by mass: 30-60wt% of rubber, 10-25wt% of semi-reinforced carbon black, 15-35wt% of fast extrusion carbon black, 3-15wt% of medium-particle thermal cracking carbon black, 0.6-6.0wt% of liquid plasticizer, 0.3-0.8wt% of waxy plasticizer, 2.0-3.2wt% of vulcanization accelerating agent, 0.1-1.8wt% of vulcanization accelerator, 0.5-1.5wt% of antioxidant and 0.3-1.0wt% of vulcanizing agent.
[0025] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention include 30-60wt% of rubber, preferably 33-59wt%, more preferably 43.4-57.4wt%, and more preferably 44-53wt%. In the present invention, the rubber is preferably nitrile rubber, chloroprene rubber or butyl rubber. The present invention has no particular limitation on the source of the rubber, and commercial products well known to those skilled in the art can be used. In the present invention, the rubber is a matrix material.
[0026] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention also include 10-25wt% of semi-reinforcing carbon black, further preferably 15-25wt%, and more preferably 15-20wt%. In the present invention, the semi-reinforcing carbon black is preferably one of carbon black N754, carbon black N762, carbon black N765, carbon black N770, carbon black N772, carbon black N774 and carbon black N787; the particle size of the semi-reinforcing carbon black is preferably 60-100nm. The present invention does not specifically limit the source of the semi-reinforcing carbon black, and commercial products familiar to those skilled in the art can be used. In the present invention, the semi-reinforcing carbon black mainly improves the strength of the material, and cooperates with fast-extrusion carbon black and medium-particle thermal cracking carbon black to improve the swelling rate of the material in propellants and organic solvents.
[0027] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention also include 15-35wt% of fast-extruded carbon black, further preferably 20-35wt%, and more preferably 25-30wt%. In the present invention, the fast-extruded carbon black is preferably one of carbon black N539, carbon black N542, carbon black N550 and carbon black N568; the particle size of the fast-extruded carbon black is preferably 40-50nm. The present invention does not specifically limit the source of the fast-extruded carbon black, and commercially available products familiar to those skilled in the art can be used. In the present invention, the fast-extruded carbon black improves the processing properties of the material while increasing the strength of the material, and improves the swelling rate of the material in the propellant and organic solvent in combination with semi-reinforcing carbon black and medium-particle thermal cracking carbon black.
[0028] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket described in the present invention also include 3-15wt% of medium-particle thermal cracking carbon black, further preferably 3-10wt%, and more preferably 5-8wt%. In the present invention, the medium-particle thermal cracking carbon black is preferably carbon black N990; the average particle size of the medium-particle thermal cracking carbon black is preferably 280nm. The present invention does not specifically limit the source of the medium-particle thermal cracking carbon black, and commercially available products familiar to those skilled in the art can be used. In the present invention, the medium-particle thermal cracking carbon black has good oil extraction resistance and improves the swelling rate of the material in organic solvents.
[0029] In the present invention, based on the mass ratio of the rubber sealing gasket being 100%, the total mass of the semi-reinforced carbon black, the fast extrusion carbon black and the medium particle thermal cracking carbon black is preferably 28 to 75 wt %, more preferably 30 to 53 wt %, and more preferably 40 to 51 wt %. By controlling the total mass of the carbon black, the present invention can further improve the swelling rate and mechanical properties of the rubber sealing gasket in the propellant and the organic solvent.
[0030] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention also include 0.6-6.0wt% of liquid plasticizer, more preferably 1.0-5.0wt%, and more preferably 2-2.5wt%. In the present invention, the liquid plasticizer is preferably at least one of white oil, paraffin oil, adipic acid esters and phthalates. The present invention has no special limitation on the source of the liquid plasticizer, and commercially available products familiar to those skilled in the art can be used. In the present invention, the compounding of the liquid plasticizer and the waxy plasticizer can adjust the swelling rate and hardness of the rubber sealing gasket in different organic solvents and propellants, and can also improve the processing performance.
[0031] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention also include 0.3-0.8wt% of waxy plasticizer, and more preferably 0.5-0.6wt%. In the present invention, the waxy plasticizer is preferably at least one of vaseline and fatty acid metal salt. The present invention has no special limitation on the source of the waxy plasticizer, and commercial products well known to those skilled in the art can be used. In the present invention, the compounding of the waxy plasticizer and the liquid plasticizer can adjust the swelling rate and hardness of the rubber sealing gasket in different organic solvents and propellants, and can also improve the processing performance.
[0032] In the present invention, the ratio of the total mass of the semi-reinforcing carbon black, the fast extrusion carbon black and the medium particle thermal cracking carbon black to the total mass of the liquid plasticizer and the waxy plasticizer is preferably (8-35): 1, more preferably (15-22): 1, and more preferably (18-20): 1. The present invention can achieve an ideal swelling rate of the rubber sealing gasket in the propellant and various organic solvents by controlling the total mass ratio of the semi-reinforcing carbon black, the fast extrusion carbon black and the medium particle thermal cracking carbon black to the total mass of the liquid plasticizer and the waxy plasticizer.
[0033] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention also include 2.0-3.2wt% of a vulcanization accelerator, more preferably 2.4-3.0wt%, and more preferably 2.6-3.0.wt%. In the present invention, the vulcanization accelerator is preferably zinc oxide and stearic acid, and the mass ratio of zinc oxide to stearic acid is preferably 5:1. The present invention has no special limitation on the source of the vulcanization accelerator, and commercial products well known to those skilled in the art can be used. In the present invention, the vulcanization accelerator has the function of activating the vulcanization accelerator.
[0034] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention also include 0.1-1.8wt% of a vulcanization accelerator, preferably 0.3-1.8wt%, and more preferably 0.8-1.5wt%. In the present invention, the vulcanization accelerator is preferably at least one of a thiuram accelerator, a sulfonamide accelerator, a thiazole accelerator, and a thiourea accelerator. The present invention does not specifically limit the source of the vulcanization accelerator, and commercially available products familiar to those skilled in the art can be used. In the present invention, the vulcanization accelerator can promote vulcanization, shorten the vulcanization time, reduce the vulcanization temperature, reduce the amount of vulcanizing agent, and improve the physical and mechanical properties of the rubber sealing gasket.
[0035] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention also include 0.5-1.5wt% of an antioxidant, preferably 1.0-1.5wt%, and more preferably 1.2-1.4wt%. In the present invention, the antioxidant is preferably an amine antioxidant and / or a phenol antioxidant. The present invention has no special limitation on the source of the antioxidant, and commercial products well known to those skilled in the art can be used. In the present invention, the antioxidant can improve the aging resistance of the rubber sealing gasket.
[0036] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention also include 0.3-1.0wt% of a vulcanizing agent, preferably 0.3-0.6wt%, and more preferably 0.4-0.5wt%. In the present invention, the vulcanizing agent is preferably sulfur or a sulfur-containing compound. The present invention has no special limitation on the source of the vulcanizing agent, and commercial products well known to those skilled in the art can be used. In the present invention, the vulcanizing agent is used for vulcanization, which can improve the mechanical properties of the rubber sealing gasket.
[0037] In the present invention, the rubber sealing gasket is preferably prepared from raw materials including the following mass percentages: 43.4-57.4wt% of nitrile rubber, 10-18wt% of semi-reinforced carbon black, 15-25wt% of fast extrusion carbon black, 3-8wt% of medium particle thermal cracking carbon black, 2-5wt% of inorganic salt filler, 0.6-1.0wt% of liquid plasticizer, 0.3-0.6wt% of waxy plasticizer, 2.0-3.2wt% of vulcanization accelerator, 0.3-1.8wt% of vulcanization accelerator, 0.5-1.5wt% of antioxidant and 0.3-1.0wt% of vulcanizing agent;
[0038] Alternatively, it is preferably prepared from the following raw materials in percentage by weight: 44-59wt% of chloroprene rubber, 10-18wt% of semi-reinforced carbon black, 15-25wt% of fast extrusion carbon black, 3-10wt% of medium particle thermal cracking carbon black, 2.0wt% of acid absorbent, 2.5-6.0wt% of liquid plasticizer, 0.3-0.8wt% of waxy plasticizer, 2.0-3.2wt% of vulcanization accelerator, 0.1-1.8wt% of vulcanization accelerator, 0.5-1.5wt% of antioxidant and 0.3-1.0wt% of vulcanizing agent;
[0039] Alternatively, it is preferably prepared from raw materials including the following mass percentages: 33-53wt% of butyl rubber, 15-25wt% of semi-reinforcing carbon black, 20-35wt% of quick extrusion carbon black, 3-15wt% of medium particle thermal cracking carbon black, 1.0-2.0wt% of liquid plasticizer, 0.3-0.8wt% of waxy plasticizer, 2.0-3.2wt% of vulcanization accelerator, 0.3-1.8wt% of vulcanization accelerator, 0.5-1.5wt% of antioxidant and 0.3-1.0wt% of vulcanizing agent.
[0040] In one technical solution of the present invention, the rubber sealing gasket is preferably prepared from raw materials including the following mass percentages: 43.4-57.4wt% of nitrile rubber, 10-18wt% of semi-reinforced carbon black, 15-25wt% of fast extrusion carbon black, 3-8wt% of medium particle thermal cracking carbon black, 2-5wt% of inorganic salt filler, 0.6-1.0wt% of liquid plasticizer, 0.3-0.6wt% of waxy plasticizer, 2.0-3.2wt% of vulcanization accelerator, 0.3-1.8wt% of vulcanization accelerator, 0.5-1.5wt% of antioxidant and 0.3-1.0wt% of vulcanizer.
[0041] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably include 43.4-57.4wt% of nitrile rubber, more preferably 48.4-55wt%, and more preferably 48.4-50wt%. In the present invention, the nitrile rubber is a butadiene-acrylonitrile copolymer, which is a copolymer formed by polymerization of acrylonitrile and butadiene monomers. Due to the presence of cyano groups in the molecular chain structure, the oil resistance (such as resistance to mineral oil, liquid fuel, animal and vegetable oils and solvents) is better than that of natural rubber, chloroprene rubber and styrene-butadiene rubber. Compared with other rubbers, it has a wider range of use temperature, and the long-term use temperature is 120°C. At the same time, it has good low temperature resistance, the lowest glass transition temperature can reach -55°C, good chemical resistance stability, good processing performance, and as the acrylonitrile content in its structure increases, its relative density increases, the vulcanization speed increases, and the tensile strength performance increases. Due to the strong polar CN group, it has excellent stability to non-polar aliphatic hydrocarbon oils and gasoline.
[0042] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 10-18 wt % of semi-reinforcing carbon black, more preferably 12-18 wt %, and even more preferably 15-16 wt %.
[0043] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably also include 15-25wt% of quick-extrusion carbon black, more preferably 18-24wt%, and even more preferably 20-22wt%.
[0044] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably also include 3-8wt% of medium-particle thermal cracking carbon black, more preferably 5-8wt%, and even more preferably 6-8wt%.
[0045] In the present invention, based on the mass ratio of the rubber sealing gasket being 100%, the total mass of the semi-reinforced carbon black, the fast extrusion carbon black and the medium particle thermal cracking carbon black is preferably 28 to 51 wt %, more preferably 30 to 47 wt %, and more preferably 35 to 43 wt %. By controlling the total mass of the carbon black, the present invention can further improve the swelling rate and mechanical properties of the rubber sealing gasket in the propellant and the organic solvent.
[0046] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably also include 2-5wt% of inorganic salt filler, more preferably 2-4wt%, and more preferably 3wt%. In the present invention, the inorganic salt filler is preferably at least one of calcium carbonate, talcum powder and kaolin; the particle size of the calcium carbonate is preferably 1250-3000 mesh; the particle size of the talcum powder is preferably 800-1250; the particle size of the kaolin is preferably 325-2500 mesh. The present invention does not specifically limit the source of the inorganic salt filler, and commercial products well known to those skilled in the art can be used. In the present invention, the inorganic salt filler is used to provide mechanical properties of the rubber sealing gasket.
[0047] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 0.6-1.0 wt % of a liquid plasticizer, and more preferably 0.8-0.9 wt %.
[0048] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 0.3-0.6 wt %, more preferably 0.4-0.5 wt % of a waxy plasticizer.
[0049] In the present invention, the total mass of the liquid plasticizer and the waxy plasticizer is preferably less than 1.6wt% based on the mass ratio of the rubber sealing gasket as 100%. The present invention can avoid too little plasticizer, which reduces the dissolution of the projectile and the organic solvent, resulting in excessive swelling rate, and the aerosol valve is easy to stick, pause, or drag during operation, making the operation of the valve difficult, and the fluidity of the rubber is poor, which is not conducive to mass production; it can also avoid too much plasticizer, which increases the dissolution of the projectile and the organic solvent, resulting in large volume shrinkage and easy leakage.
[0050] In the present invention, the ratio of the total mass of the semi-reinforcing carbon black, the fast extrusion carbon black and the medium particle thermal cracking carbon black to the total mass of the liquid plasticizer and the waxy plasticizer is preferably (22-35): 1, and more preferably (25-30): 1. The present invention can achieve an ideal swelling rate of the rubber sealing gasket in the propellant and various organic solvents by controlling the ratio of the total mass of the semi-reinforcing carbon black, the fast extrusion carbon black and the medium particle thermal cracking carbon black to the total mass of the liquid plasticizer and the waxy plasticizer.
[0051] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 2.0 to 3.2 wt % of a vulcanization accelerator, more preferably 2.4 to 3.0 wt %, and even more preferably 2.6 to 3.0 wt %.
[0052] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 0.3-1.8wt% of a vulcanization accelerator, more preferably 0.5-1.6wt%, and even more preferably 0.8-1.5wt%.
[0053] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 0.5-1.5wt% of an antioxidant, more preferably 1.0-1.5wt%, and even more preferably 1.2-1.4wt%.
[0054] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 0.3-1.0 wt % of a vulcanizing agent, more preferably 0.3-0.6 wt %, and even more preferably 0.4-0.5 wt %.
[0055] The rubber sealing gasket prepared by the nitrile rubber of the present invention has a Shore hardness of 60-80, preferably 63-68; the thickness swelling rate of LPG is 2.0-10.0%, preferably 3.0-8.0%; the thickness swelling rate of DME is 18.0-29.0%, preferably 18.4-27.5%, and is suitable for use in aerosol valve systems in the field of daily chemicals.
[0056] In another technical solution of the present invention, the rubber sealing gasket is preferably prepared from raw materials including the following mass percentages: 44-59wt% of chloroprene rubber, 10-18wt% of semi-reinforced carbon black, 15-25wt% of fast extrusion carbon black, 3-10wt% of medium particle thermal cracking carbon black, 2.0wt% of acid absorbent, 2.5-6.0wt% of liquid plasticizer, 0.3-0.8wt% of waxy plasticizer, 2.0-3.2wt% of vulcanization accelerator, 0.1-1.8wt% of vulcanization accelerator, 0.5-1.5wt% of antioxidant and 0.3-1.0wt% of vulcanizer.
[0057] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably include 44-59wt% of chloroprene rubber, and more preferably 50-55wt%. In the present invention, the chloroprene rubber is a chloroprene polymer, which is obtained by α-polymerization reaction of chloroprene monomer as the main raw material, and has good physical and mechanical properties, oil resistance, heat resistance, flame resistance, sunlight resistance, ozone resistance, acid and alkali resistance, chemical reagent resistance, and oil resistance is second only to nitrile rubber.
[0058] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 10 to 18 wt % of semi-reinforcing carbon black, and more preferably 12 to 15 wt %.
[0059] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably also include 15-25wt% of quick-extrusion carbon black, more preferably 16-23wt%, and even more preferably 20-22wt%.
[0060] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably also include 3-10wt% of medium-particle thermal cracking carbon black, more preferably 3-8wt%, and even more preferably 3-7wt%.
[0061] In the present invention, based on the mass ratio of the rubber sealing gasket being 100%, the total mass of the semi-reinforced carbon black, the fast extrusion carbon black and the medium particle thermal cracking carbon black is preferably 30 to 53 wt%, more preferably 31 to 46 wt%, and more preferably 35 to 40 wt%. By controlling the total mass of the carbon black, the present invention can further improve the swelling rate and mechanical properties of the rubber sealing gasket in the propellant and the organic solvent.
[0062] Based on the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably also include 2.0wt% of an acid absorbent; the acid absorbent is preferably magnesium oxide. The present invention has no special limitation on the source of the acid absorbent, and commercial products well known to those skilled in the art can be used. In the present invention, chloroprene rubber is easily dehalogenated to form acid during high-temperature vulcanization, and the addition of an acid absorbent can absorb the acid generated by vulcanization.
[0063] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 2.5-6.0wt% of liquid plasticizer, more preferably 2.8-5.0wt%, and even more preferably 3.0-4.5wt%.
[0064] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 0.3 to 0.8 wt %, more preferably 0.3 to 0.5 wt % of a waxy plasticizer.
[0065] In the present invention, the ratio of the total mass of the semi-reinforcing carbon black, fast extrusion carbon black and medium particle thermal cracking carbon black to the total mass of the liquid plasticizer and the waxy plasticizer is preferably (8-15):1, more preferably (10-12):1.
[0066] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 2.0-3.2 wt % of a vulcanization accelerator, more preferably 2.6-3.2 wt %, and even more preferably 2.6-3.0 wt %.
[0067] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 0.1 to 1.8 wt % of a vulcanization accelerator, more preferably 0.2 to 1.0 wt %, and even more preferably 0.2 to 0.6 wt %.
[0068] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 0.5-1.5wt% of an antioxidant, more preferably 0.8-1.2wt%, and even more preferably 1.0-1.1wt%.
[0069] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 0.3-1.0 wt % of a vulcanizing agent, more preferably 0.3-0.6 wt %, and even more preferably 0.3-0.5 wt %.
[0070] The rubber sealing gasket prepared by using chloroprene rubber has a Shore hardness of 65-82, preferably 70-76; the thickness swelling rate of LPG is 1.0-6.0%, preferably 2.0-3.5%; the thickness swelling rate of DME is 9.90-16.0%, preferably 10.0-13.5%, and is suitable for use in aerosol valve systems in the field of daily chemicals.
[0071] In another technical solution of the present invention, the rubber sealing gasket is preferably prepared from raw materials including the following mass percentages: 33-53wt% of butyl rubber, 15-25wt% of semi-reinforced carbon black, 20-35wt% of fast extrusion carbon black, 3-15wt% of medium particle thermal cracking carbon black, 1.0-2.0wt% of liquid plasticizer, 0.3-0.8wt% of waxy plasticizer, 2.0-3.2wt% of vulcanization accelerator, 0.3-1.8wt% of vulcanization accelerator, 0.5-1.5wt% of antioxidant and 0.3-1.0wt% of vulcanizer.
[0072] Based on the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably include 33-53wt% of butyl rubber, and more preferably 40-50wt%. In the present invention, the butyl rubber is an isobutylene-isoprene copolymer, which is obtained by cationic polymerization of isobutylene monomer and a small amount of isoprene monomer at low temperature, has good chemical stability and thermal stability, is resistant to aging and chemicals, and has shock absorption and electrical insulation properties, good resistance to sunlight and ozone, can be exposed to animal oil or vegetable oil or oxidizable chemicals, and is most prominent in air tightness and water tightness.
[0073] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 15 to 25 wt % of semi-reinforcing carbon black, and more preferably 24 to 25 wt %.
[0074] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably also include 20-35wt% of quick-extrusion carbon black, more preferably 18-30wt%, and even more preferably 20-30wt%.
[0075] Taking the mass ratio of the rubber sealing gasket as 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably also include 3-15wt% of medium-particle thermal cracking carbon black, more preferably 5-10wt%, and even more preferably 8-9wt%.
[0076] In the present invention, based on the mass ratio of the rubber sealing gasket being 100%, the total mass of the semi-reinforced carbon black, the fast extrusion carbon black and the medium particle thermal cracking carbon black is preferably 40 to 75 wt%, more preferably 45 to 60 wt%, and more preferably 50 to 58 wt%. By controlling the total mass of the carbon black, the present invention can further improve the swelling rate and mechanical properties of the rubber sealing gasket in the propellant and the organic solvent.
[0077] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 1.0 to 2.0 wt % of a liquid plasticizer, and more preferably 1.2 to 1.4 wt %.
[0078] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 0.3 to 0.8 wt %, more preferably 0.3 to 0.5 wt % of a waxy plasticizer.
[0079] In the present invention, based on the mass ratio of the rubber sealing gasket being 100%, the total mass of the liquid plasticizer and the waxy plasticizer is preferably less than 2.3 wt %.
[0080] In the present invention, the ratio of the total mass of the semi-reinforcing carbon black, fast extrusion carbon black and medium particle thermal cracking carbon black to the total mass of the liquid plasticizer and the waxy plasticizer is preferably (20-35):1, more preferably (25-30):1.
[0081] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 2.0 to 3.2 wt % of a vulcanization accelerator, more preferably 2.0 to 2.6 wt %, and even more preferably 2.2 to 2.5 wt %.
[0082] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 0.3-1.8 wt % of a vulcanization accelerator, more preferably 0.3-1.0 wt %, and even more preferably 0.5-1.0 wt %.
[0083] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 0.5-1.5wt% of an antioxidant, more preferably 0.6-1.0wt%, and even more preferably 0.7-0.9wt%.
[0084] Based on the mass ratio of the rubber sealing gasket being 100%, the raw materials for preparing the rubber sealing gasket of the present invention preferably further include 0.3-1.0 wt % of a vulcanizing agent, more preferably 0.3-0.7 wt %, and even more preferably 0.3-0.5 wt %.
[0085] The rubber sealing gasket prepared by butyl rubber of the present invention has a Shore hardness of 65-80, preferably 68-78; the thickness swelling rate of LPG is 10.0-23.0%, preferably 15.0-18.0%; the thickness swelling rate of DME is 5.0-12.0%, preferably 5.0-9.5%, and is suitable for use in aerosol valve systems in the field of daily chemicals.
[0086] The present invention uses a compound of semi-reinforced carbon black, fast extrusion carbon black and medium-particle thermal cracking carbon black as reinforcing agents, and controls the quality of the three types of carbon black to improve the swelling rate of the material in the propellant; the plasticizer uses a liquid plasticizer and a waxy plasticizer in combination, and controls the amount of the plasticizer, so that the rubber sealing gasket can meet the swelling rate requirements in the propellant.
[0087] The rubber types adopted in the present invention are nitrile rubber (NBR), chloroprene rubber and butyl rubber. Because different rubber types have different properties, the raw material ratio of other auxiliary materials is optimized and adjusted. No matter which type of rubber raw material is adopted, the prepared sealing gasket product can meet the technical requirements; by setting a reasonable type and ratio of plasticizer, the processing performance and flexibility of the rubber material are improved while the extraction limit in the propellant and organic solvent is met; by setting a reasonable type and ratio of reinforcing agent carbon black, the strength of the rubber material is improved while the swelling rate requirement in the propellant and organic solvent is met.
[0088] The present invention also provides a method for preparing the rubber sealing gasket described in the above technical solution, comprising the following steps:
[0089] (1) plasticizing the rubber to obtain plasticized rubber;
[0090] (2) mixing the plasticized rubber obtained in step (1) with semi-reinforcing carbon black, fast extrusion carbon black, medium-particle thermal cracking carbon black, liquid plasticizer, waxy plasticizer, vulcanization accelerator, antioxidant, vulcanization accelerator and vulcanizing agent, and then extruding and calendering in sequence to obtain a film;
[0091] (3) vulcanizing the rubber obtained in step (2) to obtain a rubber sealing gasket.
[0092] The present invention plasticizes rubber to obtain plasticized rubber.
[0093] In the present invention, the plasticizing is preferably carried out in an internal mixer; the plasticizing time is preferably 1 to 15 minutes. The present invention has no special limitation on the type of the internal mixer, and the equipment well known to those skilled in the art can be used. The present invention has no special limitation on the temperature of the plasticizing, and the temperature well known to those skilled in the art can be used.
[0094] After obtaining the plasticized rubber, the invention mixes the plasticized rubber with semi-reinforced carbon black, fast extrusion carbon black, medium-particle thermal cracking carbon black, liquid plasticizer, waxy plasticizer, vulcanization accelerator, antioxidant, vulcanization accelerator and vulcanizing agent, and then sequentially extrude and calender to obtain a film.
[0095] In the present invention, the operation of mixing the plasticized rubber with semi-reinforcing carbon black, fast extrusion carbon black, medium-particle thermal cracking carbon black, liquid plasticizer, waxy plasticizer, vulcanization accelerator, antioxidant, vulcanization accelerator and vulcanizing agent is preferably to mix the plasticized rubber with semi-reinforcing carbon black, fast extrusion carbon black, medium-particle thermal cracking carbon black, liquid plasticizer, waxy plasticizer and antioxidant in one stage, and then pound the rubber and let it stand in sequence, and then add the vulcanization accelerator, vulcanization accelerator and vulcanizing agent for two-stage mixing.
[0096] In the present invention, the time of the mixing stage is preferably 10 minutes; the temperature of the mixing stage is preferably 80 to 110°C, more preferably 90 to 100°C.
[0097] In the present invention, the tamping of the rubber is preferably performed on an open mill. The present invention has no particular limitation on the type of the open mill, and an instrument well known to those skilled in the art can be used. The present invention has no particular limitation on the operation of tamping the rubber, and an operation well known to those skilled in the art can be used.
[0098] In the present invention, the standing time is preferably 30 minutes.
[0099] In the present invention, the temperature of the second stage mixing is preferably 50-60°C; the time of the second stage mixing is preferably 5 minutes; and the second stage mixing is preferably performed on an open mill. The present invention has no special limitation on the model of the open mill, and any equipment well known to those skilled in the art can be used.
[0100] In the present invention, the extrusion is preferably carried out in an extruder, and the temperature of the extruder is preferably 70-90° C. The present invention has no particular limitation on the type of the extruder, and any equipment well known to those skilled in the art can be used.
[0101] In the present invention, the calendering is preferably carried out in a calendering machine. The present invention has no special limitation on the type of the calendering machine, and the equipment well known to those skilled in the art can be used. The present invention has no special limitation on the operation of the calendering, and the operation well known to those skilled in the art can be used.
[0102] After calendering, the present invention preferably trims the calendered product to obtain a film. The present invention has no special limitation on the trimming operation, and the operation well known to those skilled in the art can be used.
[0103] After obtaining the film, the present invention vulcanizes the film to obtain a rubber sealing gasket.
[0104] In the present invention, the vulcanization is preferably carried out in a plate vulcanizer; the vulcanization temperature is preferably 160-175°C; the vulcanization time is preferably 3-6 minutes; and the vulcanization pressure is preferably 17-20 MPa. The present invention has no particular limitation on the type of the plate vulcanizer, and any instrument or equipment familiar to those skilled in the art may be used.
[0105] After the vulcanization is completed, the present invention preferably punches the product obtained by the vulcanization to obtain a rubber sealing gasket. The present invention has no special limitation on the punching operation, which can be adjusted according to actual needs.
[0106] In the present invention, when the raw materials include an inorganic salt filler, the inorganic salt filler is preferably added during kneading; when the raw materials include an acid absorbent, the acid absorbent is preferably added during kneading.
[0107] The preparation method provided by the invention has simple process and is suitable for industrial production.
[0108] The present invention also provides the use of the rubber sealing gasket described in the above technical solution or the rubber sealing gasket prepared by the preparation method in an aerosol valve.
[0109] The present invention has no special limitation on the application operation of the rubber sealing gasket in the aerosol valve, and the application operation well known to those skilled in the art can be adopted.
[0110] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0111] Example 1
[0112] The rubber sealing gasket is prepared from the following raw materials in percentage by weight: 48.4 wt% of nitrile rubber, 14 wt% of semi-reinforced carbon black N774 with a particle size of 60 to 100 nm, 20 wt% of fast extrusion carbon black N550 with a particle size of 40 to 50 nm, 7 wt% of medium-particle thermal cracking carbon black N990 with an average particle size of 280 nm, 3.0 wt% of light calcium carbonate with a particle size of 1250 to 3000 meshes, and 0.9 wt% of dioctyl adipate (DOA). %, vaseline 0.5wt%, vulcanization accelerator 3.0wt%, vulcanization accelerator 1.4wt%, antioxidant 1.4wt% and sulfur 0.4wt%; wherein the vulcanization accelerator is 2.5wt% of zinc oxide and 0.5wt% of stearic acid; the vulcanization accelerator is 0.9wt% of vulcanization accelerator TMTD and 0.5wt% of vulcanization accelerator CZ; the antioxidant is 0.9wt% of antioxidant 224 and 0.5wt% of antioxidant MB.
[0113] Example 2
[0114] The rubber sealing gasket is prepared from the following raw materials in percentage by weight: 43.4wt% of nitrile rubber, 16wt% of semi-reinforced carbon black N774 with a particle size of 60-100nm, 22wt% of fast extrusion carbon black N550 with a particle size of 40-50nm, 8wt% of medium-particle thermal cracking carbon black N990 with an average particle size of 280nm, 3.0wt% of light calcium carbonate with a particle size of 1250-3000 mesh, 0.9wt% of dioctyl adipate (DOA), and 1.3wt% of nitrile rubber. %, vaseline 0.5wt%, vulcanization accelerator 3.0wt%, vulcanization accelerator 1.4wt%, antioxidant 1.4wt% and sulfur 0.4wt%; wherein the vulcanization accelerator is 2.5wt% of zinc oxide and 0.5wt% of stearic acid; the vulcanization accelerator is 0.9wt% of vulcanization accelerator TMTD and 0.5wt% of vulcanization accelerator CZ; the antioxidant is 0.9wt% of antioxidant 224 and 0.5wt% of antioxidant MB.
[0115] Example 3
[0116] The rubber sealing gasket is prepared from the following raw materials in percentage by mass: 57.4wt% of nitrile rubber, 10wt% of semi-reinforced carbon black N774 with a particle size of 60-100nm, 16wt% of fast extrusion carbon black N550 with a particle size of 40-50nm, 6wt% of medium-particle thermal cracking carbon black N990 with an average particle size of 280nm, 3.0wt% of light calcium carbonate with a particle size of 1250-3000 mesh, 0.9wt% of dioctyl adipate (DOA), 0.5wt% of vaseline, 3.0wt% of vulcanization accelerator, 1.4wt% of vulcanization accelerator, 1.4wt% of antioxidant and 0.4wt% of sulfur; wherein the vulcanization accelerator is 2.5wt% of zinc oxide and 0.5wt% of stearic acid; the vulcanization accelerator is 0.9wt% of vulcanization accelerator TMTD and 0.5wt% of vulcanization accelerator CZ; the antioxidant is 0.9wt% of antioxidant 224 and 0.5wt% of antioxidant MB.
[0117] The preparation method of the rubber sealing gasket described in Examples 1 to 3 comprises the following steps:
[0118] (1) placing the nitrile rubber in an internal mixer and plasticizing for 1 min to obtain a plasticized rubber;
[0119] (2) adding semi-reinforced carbon black, quick-extrusion carbon black, medium-particle thermal cracking carbon black, light calcium carbonate, dioctyl adipate, vaseline and antioxidant to the plasticized rubber and mixing them at 80° C. for 10 min, then transferring the mixed rubber to an open mixing mill, tamping the rubber and leaving it for 30 min, then adding a vulcanization accelerator, a vulcanizing accelerator and a vulcanizing agent on the open mixing mill and mixing them at 50° C. for 5 min, then extruding the mixture through an extruder and using a three-roll calender to form a sheet, and then cutting the mixture into a film through a trimmer; wherein the temperature of the extruder is 70° C.;
[0120] (3) placing the rubber sheet on a flat vulcanizer for vulcanization, and then placing it in a punching machine for punching to obtain a rubber sealing gasket; wherein the vulcanization temperature is 160° C., the time is 5 minutes, and the pressure is 18 MPa.
[0121] Comparative Example
[0122] European rubber gaskets.
[0123] The rubber sealing gaskets prepared in Examples 1 to 3 were subjected to performance tests, wherein the tensile strength and elongation were tested in accordance with GB / T 528-2009, and the hardness was tested in accordance with GB / T 531.1-2008, and the results are shown in Table 1; the thickness swelling rate was measured after the initial thickness of the sample was measured, and the sample to be tested was immersed in a propellant and various organic solvents under the condition of 50°C±1, and the thickness was measured again after the constant temperature for 3 days, 21 days, and 8 weeks, and the swelling change rate was calculated, and the results are shown in Tables 2 to 4.
[0124] Table 1 Physical properties of rubber sealing gaskets
[0125] Example 1 Example 2 Example 3 Tensile strength(MPa) 12.8 13.7 12.3 100% tensile strength (MPa) 4.1 5.7 3.0 Elongation(%) 330 250 400 Hardness(Shore A) 70 80 64
[0126] Table 2 Thickness swelling rate of rubber sealing gasket after swelling in propellant and organic solvent for 3 days (%)
[0127]
[0128]
[0129] Table 3 Thickness swelling rate of rubber sealing gasket after swelling in propellant and organic solvent for 3 weeks (%)
[0130] Test items Example 1 Example 2 Example 3 Comparative Example LPG 4.39 4.95 3.20 7.36 DME 26.14 26.50 24.95 26.95 Xylene / Toluene 42.73 42.16 43.00 40.58 Ethyl acetate 39.65 40.79 39.29 38.76 n-Hexane 4.01 6.06 3.76 7.35 Isopropyl alcohol 4.87 4.04 5.06 6.78 Dichloromethane 71.92 72.58 71.65 72.39 Pure water 2.29 3.64 4.76 2.94 Anhydrous ethanol 4.50 4.64 4.96 6.48 Ethanol / pure water 3.47 5.34 5.04 7.09
[0131] Table 4 Thickness swelling rate of rubber sealing gasket after swelling in propellant and organic solvent for 8 weeks (%)
[0132]
[0133]
[0134] As can be seen from Tables 1 to 4, in order to achieve a suitable thickness swelling rate of the nitrile rubber gasket in various organic solvents, especially in the propellant LPG, the thickness swelling rate ranges from 3.0 to 8.0%, and in the propellant DME, the thickness swelling rate ranges from 18.4 to 27.5%, the amount of carbon black and plasticizer added as the main auxiliary materials in the material is adjusted, and it is found that the amount of carbon black and plasticizer is the key factor affecting the change of the swelling rate of organic solvents and propellants. When the total amount of carbon black added is between 30 and 47wt%, the total amount of plasticizer added is less than 1.7wt%, and the ratio of the total amount of carbon black to the total amount of plasticizer is 22 to 35:1, the ideal swelling rate can be achieved in the propellant and various organic solvents.
[0135] Example 4
[0136] The rubber sealing gasket is prepared from the following raw materials in percentage by mass: 50wt% of chloroprene rubber, 14wt% of semi-reinforced carbon black N774 with a particle size of 60-100nm, 20wt% of fast extrusion carbon black N550 with a particle size of 40-50nm, 6wt% of medium-particle thermal cracking carbon black N990 with an average particle size of 280nm, 3.0wt% of dioctyl adipate (DOA), 0.5wt% of vaseline, 3.0wt% of vulcanization accelerator, 0.2wt% of vulcanization accelerator, 1.0wt% of antioxidant 224, 0.3wt% of vulcanizing agent and 2.0wt% of acid absorbent magnesium oxide; wherein the vulcanization accelerator is 2.5wt% of zinc oxide and 0.5wt% of stearic acid; the vulcanization accelerator is TMTD; and the vulcanizing agent is AN-22.
[0137] Example 5
[0138] The rubber sealing gasket is prepared from the following raw materials in percentage by mass: 44wt% of chloroprene rubber, 16wt% of semi-reinforced carbon black N774 with a particle size of 60-100nm, 23wt% of fast extrusion carbon black N550 with a particle size of 40-50nm, 7wt% of medium-particle thermal cracking carbon black N990 with an average particle size of 280nm, 3.0wt% of dioctyl adipate (DOA), 0.5wt% of vaseline, 3.0wt% of vulcanization accelerator, 0.20wt% of vulcanization accelerator, 1.0wt% of antioxidant 224, 0.3wt% of vulcanizing agent and 2.0wt% of acid absorbent magnesium oxide; wherein the vulcanization accelerator is 2.5wt% of zinc oxide and 0.5wt% of stearic acid; the vulcanization accelerator is TMTD; and the vulcanizing agent is AN-22.
[0139] Example 6
[0140] The rubber sealing gasket is prepared from the following raw materials in percentage by mass: 59wt% of chloroprene rubber, 12wt% of semi-reinforced carbon black N774 with a particle size of 60-100nm, 16wt% of fast extrusion carbon black N550 with a particle size of 40-50nm, 3wt% of medium-particle thermal cracking carbon black N990 with an average particle size of 280nm, 3.0wt% of dioctyl adipate (DOA), 0.5wt% of vaseline, 3.0wt% of vulcanization accelerator, 0.2wt% of vulcanization accelerator, 1.0wt% of antioxidant 224, 0.3wt% of vulcanizing agent and 2.0wt% of acid absorbent magnesium oxide; wherein the vulcanization accelerator is 2.5wt% of zinc oxide and 0.5wt% of stearic acid; the vulcanization accelerator is TMTD; and the vulcanizing agent is AN-22.
[0141] The preparation method of the rubber sealing gasket described in Examples 4 to 6 comprises the following steps:
[0142] (1) placing the chloroprene rubber in an internal mixer and plasticizing for 1.5 min to obtain a plasticized rubber;
[0143] (2) adding semi-reinforced carbon black, quick-extrusion carbon black, medium-particle thermal cracking carbon black, magnesium oxide, dioctyl adipate, vaseline and antioxidant 224 to the plasticized rubber and mixing at 80°C for 10 minutes, then transferring the mixed rubber to an open mixing mill, tamping the rubber and leaving it for 30 minutes, then adding a vulcanization accelerator, a vulcanizing accelerator and a vulcanizing agent on the open mixing mill and mixing at 50°C for 5 minutes, extruding through an extruder and using a three-roll calender to form a sheet, and then cutting it into a film through a trimmer; wherein the temperature of the extruder is 70°C;
[0144] (3) placing the rubber sheet on a flat vulcanizer for vulcanization, and then placing it in a punching machine for punching to obtain a rubber sealing gasket; wherein the vulcanization temperature is 160° C., the time is 5 minutes, and the pressure is 18 MPa.
[0145] The rubber sealing gaskets prepared in Examples 4 to 6 were subjected to performance tests, wherein the tensile strength and elongation were tested in accordance with GB / T 528-2009, and the hardness was tested in accordance with GB / T 531.1-2008, and the results are shown in Table 5; the thickness swelling rate was measured after the initial thickness of the sample was measured, and then the sample to be tested was immersed in a propellant and various organic solvents at 50°C±1, and the thickness was measured again after the constant temperature for 3 days, 21 days, and 8 weeks, and the swelling change rate was calculated. The results are shown in Tables 6 to 8.
[0146] Table 5 Physical properties of rubber sealing gaskets
[0147] Example 4 Example 5 Example 6 Tensile strength(MPa) 16.4 17.4 17.1 100% tensile strength (MPa) 8.3 12.2 5.3 Elongation(%) 190 140 280 Hardness(Shore A) 74 82 68
[0148] Table 6 Thickness swelling rate of rubber sealing gasket after swelling in propellant and organic solvent for 3 days (%)
[0149]
[0150]
[0151] Table 7 Thickness swelling rate of rubber sealing gasket after swelling in propellant and organic solvent for 3 weeks (%)
[0152] Test items Example 4 Example 5 Example 6 Comparative Example LPG 3.03 2.03 2.03 3.18 DME 11.82 14.22 15.45 11.02 Xylene / Toluene 35.77 38.60 47.35 36.08 Ethyl acetate 16.02 19.11 20.45 11.86 n-Hexane 4.46 4.46 4.49 7.03 Isopropyl alcohol -0.78 -0.97 -1.56 -2.05 Dichloromethane 34.30 40.65 49.86 31.48 Pure water 5.78 11.26 14.03 3.28 Anhydrous ethanol -0.77 -1.54 -2.21 -2.09 Ethanol / pure water 6.20 10.43 13.87 3.55
[0153] Table 8 Thickness swelling rate of rubber sealing gasket after swelling in propellant and organic solvent for 8 weeks (%)
[0154]
[0155]
[0156] As can be seen from Tables 5 to 8, in order to achieve a suitable thickness swelling ratio of the chloroprene rubber gasket in various organic solvents, especially in the propellant LPG, the thickness swelling ratio ranges from 1.0 to 6.0%, and in the propellant DME, the thickness swelling ratio ranges from 9.90 to 16.0%, the amount of carbon black and plasticizer added as the main auxiliary materials in the material is adjusted, and it is found that the amount of carbon black and plasticizer is the key factor affecting the change of the swelling ratio of the organic solvent and the propellant. When the total amount of carbon black added is between 31 and 46wt%, the total amount of plasticizer added is less than or equal to 3.5wt%, and the ratio of the total amount of carbon black to the total amount of plasticizer is (8 to 15): 1, the ideal swelling ratio can be achieved in the propellant and various organic solvents.
[0157] Example 7
[0158] The rubber sealing gasket is prepared from the following raw materials in percentage by mass: 40wt% of butyl rubber, 20wt% of semi-reinforced carbon black N774 with a particle size of 60-100nm, 25wt% of fast extrusion carbon black N550 with a particle size of 40-50nm, 8wt% of medium-particle thermal cracking carbon black N990 with an average particle size of 280nm, 1.5wt% of white oil, 0.5wt% of vaseline, 2.4wt% of vulcanization accelerator, 0.8wt% of vulcanization accelerator, 0.8wt% of antioxidant and 1.0wt% of sulfur; wherein the vulcanization accelerator is 2.0wt% of zinc oxide and 0.4wt% of stearic acid; the vulcanization accelerator is 0.24wt% of vulcanization accelerator TMTD, 0.16wt% of vulcanization accelerator DPTT and 0.4wt% of vulcanization accelerator MBTS; the antioxidant is 0.4wt% of 1076 and 0.4wt% of TNP.
[0159] Example 8
[0160] The rubber sealing gasket is prepared from the following raw materials in percentage by weight: 33wt% of butyl rubber, 20wt% of semi-reinforced carbon black N774 with a particle size of 60-100nm, 30wt% of fast extrusion carbon black N550 with a particle size of 40-50nm, 10wt% of medium-particle thermal cracking carbon black N990 with an average particle size of 280nm, 1.5wt% of white oil, 0.5wt% of vaseline, 2.4wt% of vulcanization accelerator, and 1.5wt% of sulfur. The composition comprises 0.8wt% of vulcanization accelerator, 0.8wt% of antioxidant and 1.0wt% of sulfur; wherein the vulcanization accelerating aids are 2.0wt% of zinc oxide and 0.4wt% of stearic acid; the vulcanization accelerators are 0.24wt% of vulcanization accelerator TMTD, 0.16wt% of vulcanization accelerator DPTT and 0.4wt% of vulcanization accelerator MBTS; the antioxidants are 0.4wt% of 1076 and 0.4wt% of TNP.
[0161] Example 9
[0162] The rubber sealing gasket is prepared from the following raw materials in percentage by mass: 53wt% of butyl rubber, 15wt% of semi-reinforced carbon black N774 with a particle size of 60-100nm, 20wt% of fast extrusion carbon black N550 with a particle size of 40-50nm, 5wt% of medium-particle thermal cracking carbon black N990 with an average particle size of 280nm, 1.5wt% of white oil, 0.5wt% of vaseline, 2.4wt% of vulcanization accelerator, The composition comprises 0.8wt% of vulcanizing agent, 0.8wt% of antioxidant and 1.0wt% of sulfur; wherein the vulcanization accelerating agent is 2.0wt% of zinc oxide and 0.4wt% of stearic acid; the vulcanization accelerator is 0.24wt% of vulcanization accelerator TMTD, 0.16wt% of vulcanization accelerator DPTT and 0.4wt% of vulcanization accelerator MBTS; the antioxidant is 0.4wt% of antioxidant 1076 and 0.4wt% of TNP.
[0163] The preparation method of the rubber sealing gasket described in Examples 7 to 9 comprises the following steps:
[0164] (1) placing butyl rubber in an internal mixer and plasticizing for 1 min to obtain plasticized rubber;
[0165] (2) adding semi-reinforced carbon black, quick-extrusion carbon black, medium-particle thermal cracking carbon black, white oil, vaseline and antioxidant to the plasticized rubber and mixing them at 80°C for 10 minutes, then transferring the mixed rubber to an open mixer, tamping the rubber and leaving it for 30 minutes, then adding a vulcanization accelerator, a vulcanizing accelerator and a vulcanizing agent on the open mixer and mixing them at 50°C for 5 minutes, then extruding them through an extruder and using a three-roll calender to form a sheet, and then cutting them into films through a trimmer; wherein the temperature of the extruder is 70°C;
[0166] (3) placing the rubber sheet on a flat vulcanizer for vulcanization, and then placing it in a punching machine for punching to obtain a rubber sealing gasket; wherein the vulcanization temperature is 170° C., the time is 5 minutes, and the pressure is 18 MPa.
[0167] The rubber sealing gaskets prepared in Examples 7 to 9 were subjected to performance tests, wherein the tensile strength and elongation were tested in accordance with GB / T 528-2009, and the hardness was tested in accordance with GB / T 531.1-2008, and the results are shown in Table 9; the thickness swelling rate was measured after the initial thickness of the sample was measured, and then the sample to be tested was immersed in a propellant and various organic solvents at 50°C±1, and the thickness was measured again after the constant temperature for 3 days, 21 days, and 8 weeks, and the swelling change rate was calculated. The results are shown in Tables 10 to 12.
[0168] Table 9 Physical properties of rubber sealing gaskets
[0169] Example 7 Example 8 Example 9 Tensile strength(MPa) 7.5 8.9 7.8 100% tensile strength (MPa) 3.8 5.2 2.7 Elongation(%) 360 170 540 Hardness(Shore A) 74 80 63
[0170] Table 10 Thickness swelling rate of rubber sealing gasket after swelling in propellant and organic solvent for 3 days (%)
[0171] Test items Example 7 Example 8 Example 9 Comparative Example LPG 17.11 18.78 10.88 21.07 DME 8.30 9.67 6.56 11.57 Xylene / Toluene 34.68 35.13 30.24 34.35 Ethyl acetate 2.91 4.22 0.89 4.42 n-Hexane 35.55 36.56 31.28 36.18 Isopropyl alcohol 0.37 1.19 0.80 0.63 Dichloromethane 22.18 20.98 18.88 20.35 Pure water 0.08 0.29 0.45 0.05 Anhydrous ethanol 0.00 0.39 0.63 0.00 Ethanol / pure water 0.28 0.46 0.15 0.08
[0172] Table 11 Thickness swelling rate of rubber sealing gasket after swelling in propellant and organic solvent for 3 weeks (%)
[0173] Test items Example 7 Example 8 Example 9 Comparative Example LPG 17.78 19.27 11.32 22.45 DME 8.09 10.13 6.83 10.78 Xylene / Toluene 35.57 36.58 31.45 35.64 Ethyl acetate 2.70 2.89 -0.19 3.27 n-Hexane 34.44 35.71 32.13 37.32 Isopropyl alcohol 0.09 0.06 -0.43 0.83 Dichloromethane 22.78 22.30 19.50 21.23 Pure water 0.47 0.67 1.89 0.31 Anhydrous ethanol 0.09 -0.29 2.22 0.59 Ethanol / pure water 0.75 1.45 0.54 0.63
[0174] Table 12 Thickness swelling rate of rubber sealing gasket after swelling in propellant and organic solvent for 8 weeks (%)
[0175]
[0176]
[0177] As can be seen from Tables 9 to 12, in order to achieve a suitable thickness swelling rate of the butyl rubber gasket in various organic solvents, especially in the propellant LPG, the thickness swelling rate ranges from 10.0 to 23.0%, and in the propellant DME, the thickness swelling rate ranges from 5.0 to 12.0%, the amount of carbon black and plasticizer added to the material is adjusted, and it is found that the amount of carbon black and plasticizer is the key factor affecting the change of the swelling rate of organic solvents and propellants. When the total amount of carbon black added is between 40 and 60wt%, the total amount of plasticizer added is less than 2.3wt%, and the ratio of the total amount of carbon black to the total amount of plasticizer is 24 to 30:1, the ideal swelling rate can be achieved in the propellant and various organic solvents. When the amount of plasticizer is small, the material hardness is too large, and the measured hardness is 80 degrees, which is not suitable for the automated assembly of aerosol valves and will also cause difficulties in the gasket processing technology; when the amount of plasticizer is large, the dissolution of propellants and organic solvents increases, resulting in large volume shrinkage and easy leakage. The rubber sealing gasket based on the technical solution of the present invention has an ideal swelling rate in propellants and organic solvents, good air tightness, and has the same performance as similar products in developed countries. It can replace imports and fill domestic gaps, and is suitable for use in aerosol valve systems in the field of daily chemicals.
[0178] It can be seen from the above embodiments and comparative examples that the rubber sealing gasket provided by the present invention can meet the swelling rate requirement in the propellant.
[0179] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A rubber sealing gasket, prepared from the following raw materials in percentage by mass: 30-60 wt% of rubber, 10-25 wt% of semi-reinforced carbon black, 15-35 wt% of quick-extrusion carbon black, 3-15 wt% of medium-particle thermal cracking carbon black, 0.6-6.0 wt% of liquid plasticizer, 0.3-0.8 wt% of waxy plasticizer, 2.0-3.2 wt% of vulcanization accelerator, 0.1-1.8 wt% of vulcanization accelerator, 0.5-1.5 wt% of antioxidant and 0.3-1.0 wt% of vulcanizing agent.
2. The rubber sealing gasket according to claim 1, characterized in that: The invention is prepared from the following raw materials in percentage by weight: 43.4-57.4 wt% of nitrile rubber, 10-18 wt% of semi-reinforced carbon black, 15-25 wt% of quick-extrusion carbon black, 3-8 wt% of medium-particle thermal cracking carbon black, 2-5 wt% of inorganic salt filler, 0.6-1.0 wt% of liquid plasticizer, 0.3-0.6 wt% of waxy plasticizer, 2.0-3.2 wt% of vulcanization accelerating agent, 0.3-1.8 wt% of vulcanization accelerator, 0.5-1.5 wt% of antioxidant and 0.3-1.0 wt% of vulcanizing agent; Alternatively, the method is prepared from the following raw materials in percentage by weight: 44-59 wt% of chloroprene rubber, 10-18 wt% of semi-reinforced carbon black, 15-25 wt% of quick extrusion carbon black, 3-10 wt% of medium particle thermal cracking carbon black, 2.0 wt% of acid absorbent, 2.5-6.0 wt% of liquid plasticizer, 0.3-0.8 wt% of waxy plasticizer, 2.0-3.2 wt% of vulcanization accelerator, 0.1-1.8 wt% of vulcanization accelerator, 0.5-1.5 wt% of antioxidant and 0.3-1.0 wt% of vulcanizing agent; Alternatively, the method is prepared from raw materials comprising the following weight percentages: 33-53wt% of butyl rubber, 15-25wt% of semi-reinforcing carbon black, 20-35wt% of quick extrusion carbon black, 3-15wt% of medium particle thermal cracking carbon black, 1.0-2.0wt% of liquid plasticizer, 0.3-0.8wt% of waxy plasticizer, 2.0-3.2wt% of vulcanization accelerating agent, 0.3-1.8wt% of vulcanization accelerator, 0.5-1.5wt% of antioxidant and 0.3-1.0wt% of vulcanizing agent.
3. The rubber sealing gasket according to claim 1 or 2, characterized in that: The semi-reinforcing carbon black is one of carbon black N754, carbon black N762, carbon black N765, carbon black N770, carbon black N772, carbon black N774 and carbon black N787.
4. The rubber sealing gasket according to claim 1 or 2, characterized in that: The fast extrusion carbon black is one of carbon black N539, carbon black N542, carbon black N550 and carbon black N568.
5. The rubber sealing gasket according to claim 1 or 2, characterized in that: The medium particle thermal cracking carbon black is carbon black N990.
6. The rubber sealing gasket according to claim 2, characterized in that: The inorganic salt filler is at least one of calcium carbonate, talc and kaolin.
7. The rubber sealing gasket according to claim 1 or 2, characterized in that: The liquid plasticizer is at least one of white oil, paraffin oil, adipic acid esters and phthalic acid esters; the waxy plasticizer is at least one of vaseline and fatty acid metal salts.
8. The rubber sealing gasket according to claim 1 or 2, characterized in that: The vulcanization accelerating aids are zinc oxide and stearic acid, and the mass ratio of zinc oxide to stearic acid is 5:
1.
9. The method for preparing the rubber sealing gasket according to any one of claims 1 to 8, comprising the following steps: (1) plasticizing the rubber to obtain plasticized rubber; (2) mixing the plasticized rubber obtained in step (1) with semi-reinforcing carbon black, fast extrusion carbon black, medium-particle thermal cracking carbon black, liquid plasticizer, waxy plasticizer, vulcanization accelerator, antioxidant, vulcanization accelerator and vulcanizing agent, and then extruding and calendering in sequence to obtain a film; (3) vulcanizing the rubber obtained in step (2) to obtain a rubber sealing gasket; When the raw materials include an inorganic salt filler, the inorganic salt filler is added in step (2); When the raw material includes an acid absorbent, the acid absorbent is added in step (2).
10. Use of the rubber sealing gasket according to any one of claims 1 to 8 or the rubber sealing gasket prepared by the preparation method according to claim 9 in an aerosol valve.