Foaming sole material with low damping G value and preparation method thereof

By adding 2-ethylhexyl acrylate/isfuric acid monoester copolymer rubber and high styrene directional hydrogenated SEBS to EVA materials, combined with microcapsule expansion agent and AC foaming agent, a circular closed cell structure is formed , solves the problem of insufficient shock-absorbing G value in the existing technology, realizes a foam sole material with low shock-absorbing G value and high rebound rate, and improves the shock-absorbing performance and user experience of sports shoes.

CN118812944AActive Publication Date: 2024-10-22ANTA (CHINA) CO LTD

Patent Information

Application Number
CN202410907095.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-22
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

The existing EVA series shock-absorbing sole foam materials have failed to achieve the technical level of shock-absorbing G value below 9.5, and there are still large impact forces and fatigue problems during exercise.

Method used

EVA materials are used to prepare foam sole materials with a low shock-absorbing G value, and are combined with 2-ethylhexyl acrylate/ethylhexanoic acid monoester copolymer rubber, directional hydrogenated SEBS, microcapsule expansion agents and reinforcing fillers to form a special The circular closed cell structure, combined with the use of AC foaming agent, enables the material to achieve large deformation and good resilience during impact.

Benefits of technology

It has realized a foam material with a shock-absorbing G value of ≤8.0 and a rebound rate of ≥60%, which can significantly reduce the impact force and improve the sports experience. It has broken the shock-absorbing G value limit in the industry and has excellent shock-absorbing performance and rebound performance. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004932456800000091
    Figure BDA0004932456800000091
  • Figure BDA0004932456800000101
    Figure BDA0004932456800000101
  • Figure BDA0004932456800000111
    Figure BDA0004932456800000111
Patent Text Reader

Abstract

The invention provides a foaming sole material with a low damping G value and a preparation method of the foaming sole material. The foaming sole material is prepared by foaming an EVA (Ethylene Vinyl Acetate) material; the EVA materials comprise 40 to 55 parts of EVA, 5 to 15 parts of acrylic acid-2-ethylhexyl acrylate / itaconic acid monoester copolymer rubber, 10 to 20 parts of directionally hydrogenated SEBS, 5 to 10 parts of POE, 5 to 10 parts of EPDM, 5 to 10 parts of OBC, 4 to 8 parts of a reinforcing filler, 3 to 5 parts of a microcapsule expanding agent, 0.5 to 0.8 part of a cross-linking agent, 2 to 3 parts of an AC foaming agent, 1 to 1.5 parts of zinc oxide, 0.5 to 1.2 parts of stearic acid and 0.5 to 1.3 parts of stearate. The foaming sole material is internally provided with the special circular closed foam holes, the circular foam holes generate large deformation in the exercise process, so that impact force is greatly reduced, high resilience is achieved, and the extreme experience of consumers in the exercise process is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of shoe materials, and in particular relates to a foamed sole material with a low shock-absorbing G value and a preparation method thereof. Background Art

[0002] The shock absorption system is the most important part of sports shoes. During exercise, the human body will constantly bear a lot of gravity. When the foot lands, it will also generate a considerable impact force. What has a greater impact on the human body is the recoil force from the ground after the foot lands. A pair of shoes with shock absorption function can prevent sports injuries, especially shin pain, fractures and joint pain; reduce fatigue, quickly restore physical strength, and are not easy to cause sore feet, that is, relatively improve sports performance. With the diversification and high-end production of footwear, the increasing updating of shoe materials, and the continuous advancement of shoemaking technology, the performance indicators of footwear are increasing. During exercise, with different movement speeds, the foot is usually subjected to a recoil force of 1.3-3 times the gravity. The faster the movement speed, the heavier the runner's weight, the greater the loading rate of the force, and the greater the recoil force. Therefore, it is imperative to develop a foam sole material with a low shock absorption G value (the lower the G value, the better the shock absorption performance).

[0003] In the prior art, there are methods to improve the shock absorption performance to a certain extent through structural or formula design. For example, Chinese patent document 201910697047.0 mentions a shock-absorbing sole, whose internal shock-absorbing structure includes multiple layers of stacked bubble sheets and hot-melt adhesive films between them. This technology is a shock-absorbing sole with improved structural design, but the shock absorption G value of its sole is 10.7 before fatigue and 11.8 after fatigue, and the shock absorption level still needs to be improved. For example, Chinese patent document 201910832129.1 mentions a high-shock-absorbing macroporous foamed midsole material, which is made by foaming EVA composite material; the EVA composite material includes the following components in parts by mass: 40 to 70 parts of ethylene-vinyl acetate copolymer; 10 to 30 parts of α-olefin thermoplastic elastomer; 10 to 30 parts of styrene copolymer; 0.4 to 0.6 parts of cross-linking agent; 2 to 4 parts of dinitrosopentamethylenetetramine; 2 to 4 parts of urea ester. The foam midsole material is a shock-absorbing sole designed with 2-5mm large foam holes, and its shock absorption G value is ≥ 9.5. It can be seen that the existing EVA series shock-absorbing sole foam materials have not yet achieved a technical level of shock absorption G value lower than 9.5 or even lower. Summary of the invention

[0004] In view of this, the present invention provides a foamed sole material with a low shock absorption G value and a preparation method thereof. The foamed sole material provided by the present invention has a lower shock absorption G value, which is beneficial to reducing impact force in shoe applications and has higher rebound, thereby improving the consumer's experience during exercise.

[0005] The invention provides a foamed sole material with a low shock-absorbing G value. The foamed sole material is prepared by foaming an EVA material. The EVA material comprises, by weight, 40-55 parts of EVA, 5-15 parts of 2-ethylhexyl acrylate / isobutyric acid monoester copolymer rubber, 10-20 parts of directional hydrogenated SEBS, 5-10 parts of POE, 5-10 parts of EPDM, 5-10 parts of OBC, 4-8 parts of reinforcing filler, 3-5 parts of microcapsule expansion agent, 0.5-0.8 parts of crosslinking agent, 2-3 parts of AC foaming agent, 1-1.5 parts of zinc oxide, 0.5-1.2 parts of stearic acid and 0.5-1.3 parts of stearate. The reinforcing filler is activated sepiolite fiber powder.

[0006] Preferably, the styrene unit structure content of the directionally hydrogenated SEBS is 35-40%, and the degree of hydrogenation is 50-80%.

[0007] Preferably, the reinforcing filler is activated sepiolite fiber powder treated with acid, anhydride or coupling agent.

[0008] Preferably, the reinforcing filler is sepiolite fiber powder activated by a titanate coupling agent, and the activation degree is greater than 80%.

[0009] Preferably, the initial decomposition temperature of the microcapsule expansion agent is 118-128°C, and the maximum decomposition temperature is 172-187°C.

[0010] Preferably, the vinyl acetate unit structure content of the EVA is 18-30%.

[0011] Preferably, the crystallinity of the POE, EPDM and OBC is respectively less than 18%;

[0012] The cross-linking agent is dicumyl peroxide and / or 1,4-di-tert-butyl peroxycumene; and the stearate is zinc stearate.

[0013] Preferably, the shock absorption G value of the foam sole material is not greater than 8, and the rebound rate is above 60%.

[0014] The present invention provides a method for preparing the foamed sole material as described above, comprising the following steps:

[0015] The EVA material is mixed and granulated in sequence, and then foamed and formed at least once to obtain a foamed sole material with a low shock-absorbing G value that can be used for sports shoes.

[0016] Preferably, the mixing temperature is 80-110°C; the granulation temperature is 80-95°C.

[0017] The test method of shock absorption G value known in the art includes: applying pressure quickly through the falling object, the pressure and displacement sensors continuously measure the entire loading and unloading compression cycle, and calculating the displacement change through the pressure record. The impact speed of the object depends on the height of the fall, the maximum pressure and displacement depend on the shock absorption performance of the shoe, and the maximum energy applied depends on the height of the fall and the shock absorption performance of the shoe. The test standard of shock absorption G value includes: fixing the mass of the falling object to 8.5±0.1kg and the height to 50±2.5mm to obtain the maximum impact energy of 5±0.5J, so that the G value is only related to the shock absorption performance of the sole, and its formula is:

[0018] G=-F / mg=2+2H / D+2U F / mgD;

[0019] F: impact force; F = -F M , F M =2mg+2mgH / D+2U F / D, the larger the deformation D value, the higher the F M The smaller.

[0020] Therefore, the shock absorption G value is related to the displacement change after the impact. The greater the displacement deformation, the more the pressure is dispersed, and the lower the G value.

[0021] In order to obtain smaller force and larger deformation, the present invention provides a foamed sole material formed by foaming EVA-based materials, which is specifically prepared by mixing 2-ethylhexyl acrylate / isobutyric acid monoester copolymer rubber, directional hydrogenated SEBS, microcapsule expansion agent and reinforcing filler, and then blending and foaming with polymers such as EVA, POE, OBC, EPDM, etc., to obtain a foamed material with a shock-absorbing G value of ≤8.0 and a rebound rate of ≥60%. The foamed sole material uses a microcapsule expansion agent and an AC foaming agent to obtain a special circular closed pore inside. The circular pores undergo a large deformation during exercise, thereby greatly reducing the impact force, which is beneficial to the health of consumers, and has a high rebound, which enhances the ultimate experience of consumers during exercise. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a morphology of the internal cells of the foamed sole sample of Example 3;

[0023] Figure 2 This is a picture of the internal pore morphology of the foamed sole of Comparative Example 6. DETAILED DESCRIPTION

[0024] The technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, rather than all the embodiments. Based on the embodiment in the present invention, all other embodiments obtained by ordinary technicians in the art without making creative work are within the scope of protection of the present invention. Unless otherwise specified, the various reagents and raw materials used in the present invention are all commodities that can be purchased from the market or products that can be prepared by recognized methods.

[0025] The invention provides a foamed sole material with a low shock-absorbing G value. The foamed sole material is prepared by foaming an EVA material. The EVA material comprises, by weight, 40-55 parts of EVA, 5-15 parts of 2-ethylhexyl acrylate / isobutyric acid monoester copolymer rubber, 10-20 parts of directional hydrogenated SEBS, 5-10 parts of POE, 5-10 parts of EPDM, 5-10 parts of OBC, 4-8 parts of reinforcing filler, 3-5 parts of microcapsule expansion agent, 0.5-0.8 parts of crosslinking agent, 2-3 parts of AC foaming agent, 1-1.5 parts of zinc oxide, 0.5-1.2 parts of stearic acid and 0.5-1.3 parts of stearate.

[0026] The present invention provides a foaming material for a shoe sole, which has a lower shock-absorbing G value and a higher rebound, is beneficial for reducing impact force in shoe applications, and can enhance the experience of consumers during exercise.

[0027] The foamed sole material described in the embodiment of the present invention is made by foaming EVA-type materials. The EVA-type materials are raw material compositions comprising polymers such as EVA, crosslinking agents, foaming agents, and additives. The EVA is the main component, and specifically includes the following components in parts by weight: 40-55 parts of EVA, 5-10 parts of POE, 5-10 parts of EPDM, 5-10 parts of OBC, 5-15 parts of 2-ethylhexyl acrylate / isobutyric acid monoester copolymer rubber, and 10-20 parts of directional hydrogenated SEBS.

[0028] Wherein, EVA is the English abbreviation of ethylene-vinyl acetate copolymer, which is a polymer resin copolymerized by ethylene and vinyl acetate VA, and generally has good elasticity. The EVA described in the embodiment of the present invention includes EVA with VA = 18%-30% (mass percentage), and the preferred commercially available varieties are: EVA 7470M (Formosa Plastics Corporation); its weight parts can be 40 parts, 45 parts, 50 parts, etc.

[0029] The full name of POE in English is Polyolefin elastomer, which is mainly a random polyethylene octene elastomer; it preferably includes a polyolefin elastomer grade with a crystallinity of ≤18%, and further preferred commercial varieties include: POE 8180 (Dow Company). In an embodiment of the present invention, the weight parts of the POE can be 5 parts, 8 parts, 10 parts, etc. The olefin block copolymer OBC includes a grade with a crystallinity of ≤15%, and its crystallinity can be 10-15%. The preferred varieties include OBC 9107 (Dow Company, hardness 60A). In an embodiment of the present invention, the weight parts of the OBC can be 5 parts, 8 parts, 10 parts, etc.

[0030] In addition, the embodiment of the present invention preferably uses 5 to 7 parts by weight of EPDM. EPDM is the abbreviation of ethylene propylene diene monomer rubber, which is a terpolymer of ethylene, propylene and non-conjugated dienes. In the embodiment of the present invention, the EPDM mainly includes grades with a crystallinity of ≤5%, and the preferred commercial varieties are: EPDM5565 (Dow), with a crystallinity of 1%.

[0031] In some embodiments of the present invention, the EVA material formula includes, by weight, 5, 10 or 15 parts of 2-ethylhexyl acrylate / isobutyric acid monoester copolymer rubber, and 10, 15 or 20 parts of directional hydrogenated SEBS. The main monomer of the 2-ethylhexyl acrylate / isobutyric acid monoester copolymer rubber is 2-ethylhexyl acrylate, the vulcanizing monomer is isobutyric acid monoester, and the content of the vulcanizing monomer is preferably 4-5% of the copolymer elastomer, and the preferred commercial varieties are ACM-2212 (Jiujiang Duwei Rubber Technology Co., Ltd.), Mooney viscosity 40±5ML (1+4) 100°C. At the same time, the embodiment of the present invention adopts directional hydrogenated SEBS with high styrene content, which preferably includes a block copolymer of styrene-butadiene-styrene with a styrene mass content of 35-40% and a hydrogenation degree of 50-80%, and the preferred commercial varieties are SEBS-Q5583, purchased from Zhejiang Zhongli Synthetic Materials Technology Co., Ltd. The degree of hydrogenation refers to the mass percentage of partially hydrogenated butadiene in the material.

[0032] The embodiment of the present invention selects to add materials with high shock absorption performance in the formula design. Specifically, it can be known from the group contribution theory that the polymer material with large side group volume, large number, large polarity, many intermolecular hydrogen bonds and strong intermolecular force on the molecular chain has large internal rotation activation energy and intermolecular force, large internal friction resistance of segment movement, and thus large hysteresis, large internal friction and good shock absorption performance. On the basis of the above-mentioned EVA and other matrices, the present invention adds an appropriate amount of 2-ethylhexyl acrylate / isobutyric acid monoester copolymer rubber and directional hydrogenated SEBS with high styrene content. The 2-ethylhexyl acrylate / isobutyric acid monoester copolymer rubber molecular chain contains polar carboxyl and ester bonds, many intermolecular hydrogen bonds, and large force, so the internal friction is large and the shock absorption performance is good; and the molecular structure of the directional hydrogenated SEBS with high styrene content, in addition to the flexible and highly elastic butadiene segment, also has styrene with large side group volume on the molecular chain, and as the styrene content increases, the side group internal friction effect on the overall molecular structure is more obvious, so the shock absorption performance is better. Furthermore, the directional hydrogenated SEBS with a high styrene content has better flexibility and adhesion than the fully hydrogenated SEBS with a high styrene content.

[0033] In addition to the above-mentioned polymer matrix components, the EVA-based materials include: 3-5 parts by weight of microcapsule expansion agent, 0.5-0.8 parts by weight of cross-linking agent, and 2-3 parts by weight of AC foaming agent. The AC foaming agent is azodicarbonamide, and the specific commercially available varieties are AC3000H. Preferably, the initial decomposition temperature of the microcapsule expansion agent is 118-128°C, and the maximum decomposition temperature is 172-187°C; the grade with a particle size of 18-24μm can be selected, and the preferred variety is 909DU80 (Akzo Nobel). The cross-linking agent is preferably a peroxide cross-linking agent, and more preferably one of diisopropylbenzene peroxide and 1,4-di-tert-butylperoxyisopropylbenzene, and the specific varieties are DCP and BIBP.

[0034] The embodiment of the present invention can use a low-temperature microcapsule expansion agent and an AC foaming agent to obtain a foamed sole material with special circular closed pores inside. The chemical foaming of the foamed sole of a general sports shoe uses an AC foaming agent of azodicarbonamide, which decomposes at high temperature to produce nitrogen and a small amount of carbon dioxide, and is simultaneously added with an appropriate amount of a cross-linking agent to form a network structure in the microstructure of the material, thereby locking the gas inside the material to form a foamed material. However, the interior of the foamed material prepared by the AC foaming agent is a closed-cell microporous structure that cannot be seen by the naked eye, and the deformation is small under the same stress. In an embodiment of the present invention, a low-temperature microcapsule expansion agent is compounded with an AC foaming agent. During the foaming process, the low-temperature microcapsule expansion agent is first expanded into an elliptical or spherical shape by heat. As the temperature further increases, the microcapsule expansion agent, the AC foaming agent and the cross-linking agent act synchronously, and the polymer matrix wraps the elliptical or spherical pores to form a three-dimensional network shell-core structure. The core structure is deformed by force, and the shell structure has mechanical properties such as high elasticity. This special shell-core structure is conducive to the foaming material to produce a large deformation when loaded with force, and has excellent recovery performance after the force is unloaded.

[0035] In parts by weight, some preferred embodiments of the present invention include: 4-8 parts of activated sepiolite fiber powder, 1-1.5 parts of zinc oxide, 0.5-1.2 parts of stearic acid, and 0.5-1.3 parts of stearate; further including: 1.2 parts of zinc oxide, 1.0 parts of stearic acid, and 1.0 parts of zinc stearate.

[0036] As for the reinforcing filler, the present invention gives priority to high-strength activated sepiolite fiber powder, which is beneficial to improving the reinforcing performance. As a natural mineral fiber, sepiolite fiber is a fibrous variant of sepiolite mineral, called α-sepiolite. As a layered chain silicate mineral, sepiolite has a layer of magnesium oxygen octahedron sandwiched between two layers of silicon oxygen tetrahedron in the structure, forming a 2:1 type layered structural unit, and its tetrahedral layer is continuous, and the direction of active oxygen in the layer is periodically reversed; the octahedral layer forms a channel arranged alternately in the upper and lower layers. The Si-OH in the structure of sepiolite fiber can directly react with organic matter to generate organic mineral derivatives, and the activation reagent for activating and modifying sepiolite fiber can be anhydride, coupling agent, etc. After the sepiolite fiber powder is activated by anhydride, the activity of the functional groups on the surface of the sepiolite fiber is improved, and the specific surface area is increased, thereby achieving a better reinforcement effect, which can significantly enhance the tensile strength, bending strength and impact strength of the composite material.

[0037] Further preferably, the reinforcing filler includes titanate coupling agent activated sepiolite fiber powder, and the activation degree is greater than 80%; the present invention can use commercially available reinforcing fillers, such as Hongsheng Chemical Co., Ltd., 1000 mesh activated sepiolite fiber powder. The activation degree is the degree of activation; in order to improve the dispersion performance of sepiolite and strengthen the interface bonding between sepiolite and polymer materials, coupling agents, surface treatment agents or acids are usually used to activate and modify the surface of sepiolite. The principle of modification is mainly to utilize the acid active centers and active Si-OH groups on the surface of sepiolite; activation modification can not only reduce the surface energy, but also change the polarity of sepiolite. In addition, the preferred varieties of zinc oxide are ZnO 997, which can play a role of lubrication and activation with stearates.

[0038] The embodiment of the present invention also provides a method for preparing the foamed sole material as described above, comprising the following steps:

[0039] The EVA material is mixed and granulated in sequence, and then foamed and formed at least once to obtain a foamed sole material with a low shock-absorbing G value that can be used for sports shoes.

[0040] The embodiment of the present invention is applicable to preparation by one-shot injection molding (IP process) or two-shot compression molding (MD process); wherein the implementation steps of the IP process include: weighing → mixing → granulation → foaming → baking, and the specific contents are as follows:

[0041] Weighing materials: According to the dosage of the formula, BIBP, AC foaming agent, and microcapsule expansion agent can be weighed as the first group; stearic acid, zinc stearate, and zinc oxide can be weighed as the second group; activated sepiolite fiber can be weighed as the third group, and the remaining materials can be weighed as the fourth group.

[0042] Mixing: First, pour the fourth group of materials into the internal mixer and turn on the machine. Mix for 10-15 minutes. It is preferred to pour in the third group of materials when the temperature rises to between 80-85°C; pour in the second group of materials when the temperature rises to 90-95°C; pour in the first group of materials when the temperature rises to 90-105°C. After mixing for 3-5 minutes, pour out the mixed materials.

[0043] Granulation: Pour the mixed material into the granulator, and adjust the temperatures of the first, second, third and fourth zones to 80, 85, 90 and 95°C respectively. In addition, it is preferred to adjust the screw speed to 40-50 rpm and the cutting speed to 15-20 rpm.

[0044] Foaming: Pour the prepared pellets into the injection foaming machine, and adjust the temperature of the first, second, third and fourth feeding zones to 80, 85, 90 and 95°C respectively. It is preferred to adjust the upper and lower mold temperatures to 170-175°C and 170-175°C respectively. Set the material amount according to the mold usage, and the crosslinking vulcanization time can be 480-600 seconds.

[0045] Baking: The temperature of the first, second, third and fourth zones of the oven can be adjusted to 80, 90, 95 and 100°C respectively, and the rotation speed is preferably 60-70 revolutions per minute; the foamed foam material is fed into the oven port, the oven length is preferably 30-40 meters, and the baking time from beginning to end is preferably 30-40 minutes.

[0046] In some other embodiments, the MD process implementation steps include: weighing → mixing → granulation → small foaming → secondary compression molding; the specific contents of this implementation step are as follows:

[0047] Weighing materials: According to the dosage of the formula, BIBP, AC foaming agent, and microcapsule expansion agent can be weighed as the first group; stearic acid, zinc stearate, and zinc oxide can be weighed as the second group; activated sepiolite fiber can be weighed as the third group, and the remaining materials can be weighed as the fourth group.

[0048] Mixing: First, pour the fourth group of materials into the internal mixer, turn on the machine, and mix for 10-15 minutes. It is preferred that the third group of materials be poured in when the temperature rises to between 80-85°C; the second group of materials be poured in when the temperature rises to 90-95°C; the first group of materials be poured in when the temperature rises to 90-105°C. Pour the mixed materials out after mixing for 3 to 5 minutes.

[0049] Granulation: Pour the mixed material into the granulator, and the temperatures of the first, second, third and fourth zones are preferably adjusted to 80, 85, 90 and 95° C., respectively. In addition, the screw speed is preferably adjusted to 40-50 rpm, and the cutting speed is preferably adjusted to 15-20 rpm.

[0050] Small foaming: Pour the prepared pellets into a flat-plate molded small foaming mold to complete the first foaming. The foaming temperature is preferably 175°C; the foaming time can be 550-600 seconds.

[0051] Molding: After the semi-finished product with small foams is cooled for 24 hours, it is pressed into a flat-plate molding mold to complete the molding of the finished product; the hot pressing temperature is preferably 175°C; the hot pressing time can be 400-420 seconds; the sole after hot pressing is quickly placed in the mold for cooling, the cooling water temperature can be 25°C, and the cooling time can be 400-420 seconds.

[0052] In summary, the embodiment of the present invention not only prepares a low shock-absorbing G-value sole foam material by using 2-ethylhexyl acrylate / isobutyric acid monoester copolymer rubber, directional hydrogenated SEBS with high styrene content, sepiolite fiber, and low-temperature microcapsule expansion agent, but also scientifically matches low-crystallinity or high-flexibility polymers in the formula to improve the resilience of the foam material, and finally obtains a foam material with a shock-absorbing G value ≤ 8.0 and a rebound rate ≥ 60%. This shock-absorbing G value breaks through the industry limit and achieves the lowest shock-absorbing G value in the industry, which is a first in the industry.

[0053] In order to better illustrate the present invention, further examples are given below.

[0054] Embodiment 1:

[0055] According to the dosage of the formula in Table 1, BIBP, AC foaming agent, and microcapsule expansion agent are weighed as the first group; stearic acid, zinc stearate, and zinc oxide are weighed as the second group; activated sepiolite fiber is weighed as the third group, and the remaining materials are weighed as the fourth group.

[0056] First, pour the fourth group of materials into the internal mixer, turn on the machine, mix for 10-15 minutes, and when the temperature rises to between 80-85℃, pour in the third group of materials; when the temperature rises to 90-95℃, pour in the second group of materials; when the temperature rises to 90-100℃, pour in the first group of materials, mix for 5 minutes and pour out the mixed materials.

[0057] Pour the mixed material into the material making machine, adjust the temperature of the first, second, third and fourth zones to 80, 85, 90 and 95°C respectively; adjust the screw speed to 40-50 rpm, and adjust the cutting speed to 15-20 rpm.

[0058] Pour the prepared pellets into a flat-plate compression foaming mold to complete the first foaming at a foaming temperature of 175°C and a foaming time of 550-600 seconds.

[0059] The semi-finished product with small foams is left to cool. After 24 hours, the semi-finished product is pressed into a flat-plate molding mold to complete the molding of the finished product. The hot pressing temperature is 175°C and the hot pressing time is 400-420 seconds. The sole after hot pressing is quickly placed in the mold for cooling. The cooling water temperature is 25°C and the cooling time is 400-420 seconds.

[0060] Embodiment 2-7

[0061] According to the process steps of Example 1, the raw material formula is shown in Table 1.

[0062] Comparative Examples 1-7

[0063] The process steps of Example 1 are followed, except for the formulation design, see Table 2.

[0064] The mechanical property data of the sole samples of each embodiment and comparative example are also compared as follows.

[0065] Table 1 Formula of Examples 1-7 of the present invention

[0066]

[0067] Table 2 Formula of Comparative Examples 1-7 of the present invention

[0068]

[0069] Among them, the sources of raw materials are as follows:

[0070] ACM-2212: Mooney viscosity 40±5ML(1+4)100℃, Jiujiang Duwei Rubber Technology Co., Ltd.

[0071] SEBS-Q5583: styrene content 39%, hydrogenation degree 50%, hardness 85A, Zhejiang Zhongli Synthetic Materials Technology Co., Ltd.

[0072] Activated sepiolite fiber powder: mesh size 1000 mesh, Hongsheng Chemical Co., Ltd.

[0073] EVA7470M: hardness 82A, VA content 26%, crystallinity 24.8%, Formosa Plastics Corporation.

[0074] POE 8180: hardness 63A, crystallinity 16%, Dow.

[0075] EPDM5565: crystallinity 1%, Mooney viscosity 65ML (1+4) 100℃, Dow Chemical.

[0076] OBC 9107: crystallinity 10.6%, hardness 60A, Dow.

[0077] ZnO 997: Baishi brand zinc oxide, relative density 4.42~4.45, Quanzhou Xufeng Powder Raw Material Co., Ltd.

[0078] BIBP: Sinopec.

[0079] Stearic acid 1801: Dukuda, Indonesia.

[0080] Zinc stearate: Huzhou Linghu Xinwang Chemical Co., Ltd.

[0081] Foaming agent AC 3000H: Hangzhou Haihong Fine Chemical Co., Ltd.

[0082] Microcapsule expansion agent 909DU80: Akzo Nobel.

[0083] SOE L609: Hardness 76A, S content 33%, Asahi Kasei Corporation.

[0084] Talc: mesh size 2000, Quanzhou Xufeng Powder Raw Material Co., Ltd.

[0085] Table 3 Sole performance data of comparative examples of the present invention

[0086]

[0087] Table 4 Sole performance data of comparative examples of the present invention

[0088]

[0089] From the test results of Comparative Example 3 and Comparative Examples 1 and 2, and Comparative Example 6 and Example 3, it can be seen that the use of microcapsule expansion agent and AC foaming agent in combination has a lower shock absorption G value, a higher rebound rate and a lower compression deformation than the foamed sole material using AC foaming agent alone, which shows that the microcapsule expansion agent and AC foaming agent are conducive to forming a three-dimensional network shell-core structure in the foamed sole, and the core structure produces a large deformation under force, which is conducive to improving the shock absorption performance; at the same time, the shell structure has high elasticity and high mechanical properties, and can have excellent recovery performance after force unloading, so it is also conducive to improving the resilience and improving the compression deformation of the foamed sole.

[0090] From the test results of Comparative Example 8 and Example 3, it can be seen that: when using microcapsule expansion agent alone and microcapsule expansion agent + AC foaming agent in combination, the microcapsule expansion agent has a small amount of gas emission, so the amount added is large, and the amount added needs to reach 5 times that of AC foaming agent to achieve the same foaming ratio. On the one hand, using only microcapsule expansion agent will cause larger bubbles, and the interface strength between the holes will deteriorate, resulting in a significant decrease in performance such as rebound performance / compression deformation / tensile strength / delamination and tearing, and is not conducive to the recovery performance after force unloading. On the other hand, using expansion foaming agent alone requires adding more than 15 parts, and the price of expansion agent reaches 120 yuan / kg, which is 5-10 times that of other materials. Considering the mass production cost, it is not recommended to use it alone.

[0091] It can be seen from the test data of Comparative Examples 3, 4, 5 and Example 3 that adding 2-ethylhexyl acrylate / isobutyric acid monoester copolymer rubber or directional hydrogenated SEBS with high styrene content is beneficial to reducing the shock absorption G value, but when the two are used together, the shock absorption G value decreases more significantly. This shows that whether using a polymer with a polar molecular chain or a polymer with a large side group, the internal friction effect of the overall formula can be improved, the shock absorption G value can be reduced, and the shock absorption performance can be improved.

[0092] From the test data of Comparative Example 7 and Example 3, it can be seen that the foamed sole reinforced with activated sepiolite fiber has higher rebound rate, delamination tear strength and tensile strength, and lower shock absorption G value and compression deformation, which shows that the reinforcement effect of activated sepiolite fiber is better than that of talcum powder.

[0093] As can be seen from the test data of embodiment 1-example 7: adjusting 5-15 parts of 2-ethylhexyl acrylate / monoester of furan acid copolymer rubber, 10-20 parts of directional hydrogenated SEBS with high styrene content, 40-50 parts of EVA, 5-10 parts of POE, 5-10 parts of EPDM, 5-10 parts of OBC, 4-8 parts of activated sepiolite fiber powder, 2-5 parts of low-temperature microcapsule expansion agent, can obtain a shock-absorbing G value of 7-8, a rebound rate of ≥60%, and various mechanical properties meet the requirements of the foamed sole of the sports shoe sole. And along with the increase of the addition of 2-ethylhexyl acrylate / monoester of furan acid copolymer rubber, or the increase of the addition of directional hydrogenated SEBS with high styrene content, all help to reduce the shock-absorbing G value. And, increasing the addition of microcapsule foaming agent and sepiolite fiber simultaneously, also can improve shock-absorbing performance, compression deformation performance, and other mechanical properties only slightly decline.

[0094] according to Figure 1 and Figure 2 It can be seen from the internal cells of the foamed soles of Example 3 and Comparative Example 6 that the internal cells of the foamed soles using only the AC foaming agent are small, while the internal cells of the foamed soles using the microcapsule expansion agent and the AC foaming agent are round, and special cells with large deformation during loading and excellent recovery performance during unloading are prepared. These round cells are conducive to large deformation when subjected to force, and the dense parts between the cells contribute to mechanics, so that the round cells can be supported to recover after the force is unloaded.

[0095] Compared with the existing EVA shock-absorbing foam material, firstly, the low shock-absorbing G value foam sole material prepared by the method described in this patent has improved the internal friction effect of the overall formula, reduced the shock-absorbing G value, and improved the shock-absorbing performance by adding 2-ethylhexyl acrylate / monoisocyanate copolymer rubber containing polar acid bonds and ester bonds on the molecular chain and high styrene directional hydrogenated SEBS with large side group volume in the formula. Secondly, by selecting high-strength sepiolite fiber powder activated by titanate, the functional group activity on the surface of the activated sepiolite fiber powder is improved, the specific surface area is increased, and the dispersibility is better; at the same time, the titanate component is conducive to connecting polymers such as 2-ethylhexyl acrylate / monoisocyanate copolymer rubber, EVA, and activated sepiolite fiber powder, increasing the compatibility between the polymer matrix and the reinforcing filler, and the reinforcement effect is better than the talcum powder used in conventional EVA foam soles, which can significantly enhance the impact strength of the foam material. Therefore, it is innovative in formula matching.

[0096] Compared with the existing EVA shock-absorbing foam materials, the shock-absorbing G value of the patented invention can be achieved below 8.0, breaking the technical bottleneck of shock-absorbing G value ≥ 9.5 in the industry. At the same time, it can maintain high elasticity with a rebound rate of ≥ 60%, combining excellent shock-absorbing performance and rebound performance, which is a first in the industry.

[0097] By using a low-temperature microcapsule expansion agent and an AC foaming agent in combination, a special round closed cell with large deformation when loaded and excellent recovery performance when unloaded is obtained. During the foaming process, the low-temperature microcapsule expansion agent first expands into an elliptical or spherical shape when heated. As the temperature further increases, the microcapsule expansion agent, AC foaming agent and cross-linking agent act synchronously, and the polymer matrix wraps the round cells to form a three-dimensional network shell structure-core structure. The core structure deforms when subjected to force, and the shell structure has high elasticity and high mechanical properties. This special shell-core structure is conducive to the foaming material to produce a large deformation when subjected to force loading and excellent recovery performance after force unloading. Large deformation can effectively reduce the impact force, thereby obtaining a low shock absorption G value, and excellent recovery performance is conducive to improving the resilience and compression deformation of the foamed sole.

[0098] In general, the patent of this invention uses a two-pronged approach of formula matching and special cell structure design to finally obtain a foam material with a shock absorption G value ≤ 8.0 and a rebound rate ≥ 60%. This shock absorption G value breaks through the industry limit and achieves the lowest shock absorption G value in the industry while maintaining high elasticity. It has great market prospects in sports shoes such as running shoes and basketball shoes.

[0099] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A foam sole material with low shock absorption G value, characterized in that: The foamed sole material is made from EVA materials through foaming; in parts by weight, the EVA materials include: 40-55 parts of EVA, 5-15 parts of 2-ethylhexyl acrylate / isobutyric acid monoester copolymer rubber, 10-20 parts of directional hydrogenated SEBS, 5-10 parts of POE, 5-10 parts of EPDM, 5-10 parts of OBC, 4-8 parts of reinforcing filler, 3-5 parts of microcapsule expansion agent, 0.5-0.8 parts of crosslinking agent, 2-3 parts of AC foaming agent, 1-1.5 parts of zinc oxide, 0.5-1.2 parts of stearic acid, and 0.5-1.3 parts of stearate; the reinforcing filler is activated sepiolite fiber powder.

2. The foamed sole material according to claim 1, characterized in that: The styrene unit structure content of the directional hydrogenated SEBS is 35-40%, and the hydrogenation degree is 50-80%.

3. The foamed sole material according to claim 1, characterized in that: The reinforcing filler is activated sepiolite fiber powder treated with acid, anhydride or coupling agent.

4. The foamed sole material according to claim 3, characterized in that: The reinforcing filler is sepiolite fiber powder activated by a titanate coupling agent, and the activation degree is greater than 80%.

5. The foamed sole material according to claim 1, characterized in that: The initial decomposition temperature of the microcapsule expansion agent is 118-128°C, and the maximum decomposition temperature is 172-187°C.

6. The foamed sole material according to any one of claims 1 to 5, characterized in that: The vinyl acetate unit structure content of the EVA is 18-30%.

7. The foamed sole material according to claim 6, characterized in that: The crystallinity of the POE, EPDM and OBC is respectively less than 18%; The cross-linking agent is dicumyl peroxide and / or 1,4-di-tert-butyl peroxycumene; and the stearate is zinc stearate.

8. The foamed sole material according to any one of claims 1 to 5, characterized in that: The shock absorption G value of the foamed sole material is not greater than 8, and the rebound rate is above 60%.

9. The method for preparing the foamed sole material according to any one of claims 1 to 8, characterized in that: The following steps are involved: The EVA material is mixed and granulated in sequence, and then foamed and formed at least once to obtain a foamed sole material with a low shock-absorbing G value that can be used for sports shoes.

10. The preparation method according to claim 9, characterized in that: The mixing temperature is 80-110°C; the granulation temperature is 80-95°C.

Citation Information

Patent Citations

  • High-cushioning macroporous foaming insole material, preparation method thereof and sports shoes

    CN110483879A

  • Cushioning structure in sole, cushioning sole and preparation method of cushioning sole

    CN110313681A

  • Composite response foamed rubber-plastic sole, preparation method thereof and sports shoes

    CN112029186A

  • Master batch material, preparation method and application of foaming master batch, and preparation method of foaming shoes

    CN112159540A

  • Environment-friendly light absorbing and flushing foaming material with micro air bag structure as well as preparation method and application of environment-friendly light absorbing and flushing foaming material

    CN115477807A

Cited By

  • Integrally-formed multifunctional shoe sole and preparation method thereof

    CN119431940A