Medical rubber composition and medical rubber product
By blending an acid absorbing agent with a specific BET specific surface area into halogenated butyl rubber, the problems of rising agent pH and equipment corrosion are solved, and the excellent performance of non-leaching medical rubber products is achieved.
Patent Information
- Application Number
- CN202410183853.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-21
- Filing Date
- 2024-02-19
- Publication Date
- 2024-10-22
AI Technical Summary
When medical rubber products molded using halogenated butyl rubber are in contact with chemicals, as the storage time increases, the pH value of the chemicals will rise, and halogen gas will cause equipment corrosion.
An acid absorber is compounded in halogenated butyl rubber. The BET specific surface area of the acid absorber is set to 150m2/g~200m2/g. The compounding amount relative to the base polymer is 1 to 3 parts by mass. Inhibits corrosion of halogen gas and maintains pH value of chemicals.
It effectively inhibits equipment corrosion caused by halogen gas, prevents the acid absorbing agent from dissolving into the agent, maintains the pH stability of the agent, and obtains excellent non-leaching medical rubber products.
Smart Images

Figure CN118812967A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a medical rubber composition and a medical rubber product, and more particularly, to a technology for improving the non-eluting property of a medical rubber product. Background Art
[0002] Medical rubber products used in containers for pharmaceuticals require high quality characteristics and physical properties. For example, the quality characteristics required for medical rubber plugs that seal or plug the opening of vials that store antibiotics and other preparations should be based on the 17th revised edition of the Japanese Pharmacopoeia's test for infusion rubber plugs. In addition, for medical rubber plugs that seal the opening of vials, multiple items such as gas permeation resistance, non-dissolution, high cleanliness, chemical resistance, needle resistance, self-sealing, and high sliding properties are essential.
[0003] Halogenated butyl rubber is used in medical rubber products such as medical rubber stoppers because of its excellent gas (air, water vapor) permeability resistance. Halogenated butyl rubber generates halogen gas during the kneading and molding process, which may cause equipment corrosion. In order to absorb acid from the halogen gas, it is known to mix an acid acceptor into the halogenated butyl rubber.
[0004] For example, Patent Document 1 discloses a medical rubber composition comprising (a) a base polymer containing a halogenated butyl rubber and (b) a liquid polymer, and further comprising hydrotalcite and magnesium oxide as an acid absorbent.
[0005] Patent document 2 discloses a precursor material for a silicone rubber topcoat-loaded sliding rubber material, which comprises: a rubber product, the rubber product containing a rubber component selected from at least any one of butyl rubber, halogenated butyl rubber and chloroprene rubber, a filler, a vulcanizing agent and a vulcanization aid, and further containing an acid absorber selected from magnesium oxide, zinc oxide and natural or synthetic hydrotalcite; and an interface modification layer, the interface modification layer covering the rubber product, containing an amino-modified polysiloxane compound and / or obtained by reacting the amino-modified polysiloxane compound with the surface molecules of the rubber product. [Prior art literature] [Patent Document]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2021-80370 [Patent Document 2] Japanese Patent Publication No. 2021-53988 Summary of the invention [Problems to be solved by the invention]
[0007] When a medical rubber product obtained by molding a medical rubber composition using a halogenated butyl rubber is stored in contact with a drug (e.g., saline), there is a problem that the pH of the drug (e.g., saline) increases with the storage time.
[0008] The present invention has been made in view of the above circumstances, and an object thereof is to provide a medical rubber composition comprising a halogenated butyl rubber and an acid absorbent, which can suppress corrosion of equipment caused by halogen gas while maintaining the pH of the drug. Another object of the present invention is to provide a medical rubber product having excellent non-eluting properties. [Methods used to solve the problem]
[0009] The medical rubber composition of the present invention is characterized by comprising a base polymer containing a halogenated butyl rubber and an acid scavenger, wherein the amount of the acid scavenger blended is 1 to 3 parts by mass relative to 100 parts by mass of the base polymer, and the BET specific surface area of the acid scavenger is 150 m 2 / g~200m 2 / g.
[0010] The present inventors studied the reason why the pH of the drug increases with the storage time of a medical rubber product obtained by molding a conventional medical rubber composition in which an acid absorber is blended with a halogenated butyl rubber, and found that the acid absorber dissolves into the drug and affects the pH. Then, by setting the BET specific surface area of the acid absorber to 150 m 2 / g~200m 2 / g, and the compounding amount of the acid scavenger is set to 1 to 3 parts by mass based on 100 parts by mass of the base polymer, so that the medical rubber composition obtained can suppress the corrosion of equipment caused by halogen gas while maintaining the pH of the drug, thereby completing the present invention. [Effects of the Invention]
[0011] According to the present invention, a medical rubber composition can be obtained that can suppress corrosion of equipment caused by halogen gas and can maintain the pH of a drug. In addition, according to the present invention, a medical rubber product having excellent non-eluting properties can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] [ Figure 1 ]An explanatory diagram of an embodiment (stopper) of the medical rubber product of the present invention. [ Figure 2 ]An explanatory diagram of one embodiment (rubber stopper) of the medical rubber product of the present invention. [ Figure 3]An explanatory diagram of one embodiment of the medical rubber product of the present invention (rubber stopper for vials). [ Figure 4 ]An explanatory diagram of one embodiment of the medical rubber product of the present invention (a rubber stopper for a vacuum blood collection tube). [reference numerals] 10: syringe, 11: syringe barrel, 12: plunger, 13: stopper, 15: fitting recess, 18: head, 20: rubber stopper, 21: top plate, 21b: flange, 22: stopper leg, 23: puncture portion, 24: medical container, 24a: upper edge, 24b: opening, 25: cap, 26: nylon film layer, 27: incision, 50: vacuum blood collection tube, 51: bottom tube, 53: rubber stopper DETAILED DESCRIPTION
[0013] <Medical rubber composition> The medical rubber composition of the present invention comprises a base polymer containing a halogenated butyl rubber and an acid scavenger, wherein the amount of the acid scavenger blended is 1 to 3 parts by mass relative to 100 parts by mass of the base polymer, and the BET specific surface area of the acid scavenger is 150 m 2 / g~200m 2 / g.
[0014] (Base polymer) First, the base polymer containing halogenated butyl rubber used in the present invention is described. As halogenated butyl rubber, for example, chlorinated butyl rubber, brominated butyl rubber, bromide of copolymer of isobutylene and p-methylstyrene, etc. can be cited. As the halogenated butyl rubber, chlorinated butyl rubber or brominated butyl rubber is preferred. The chlorinated butyl rubber or brominated butyl rubber is obtained, for example, by allowing chlorine or bromine to react with the isoprene structure part in butyl rubber, specifically, with the double bond and / or the carbon atom adjacent to the double bond, to generate an addition or substitution reaction. It should be noted that butyl rubber is a copolymer obtained by polymerizing isobutylene with a small amount of isoprene.
[0015] The halogen content in the halogenated butyl rubber is preferably 0.5 mass % or more, more preferably 1 mass % or more, further preferably 1.5 mass % or more, and is preferably 5 mass % or less, more preferably 4 mass % or less, further preferably 3 mass % or less.
[0016] As a specific example of the chlorinated butyl rubber, for example, CHLOROBUTYL 1066 manufactured by Japan Butyl Company [stabilizer: NS, halogen content: 1.26%, Mooney viscosity: 38 ML] can be cited. 1+8(125°C, specific gravity: 0.92]; at least one of LANXESS X_BUTYL CB1240 manufactured by LANXESS.
[0017] As a specific example of the brominated butyl rubber, for example, BROMOBUTYL 2255 [stabilizer: NS, halogen content: 2.0%, Mooney viscosity: 46 ML] manufactured by Nippon Butyl Corporation can be cited. 1+8 (125°C, specific gravity: 0.93]; at least one of LANXESS X_BUTYL BB 2030 manufactured by LANXESS, etc.
[0018] In the present invention, as the halogenated butyl rubber, chlorinated butyl rubber or brominated butyl rubber is preferably used.
[0019] The substrate polymer may contain other rubber components except halogenated butyl rubber. As other rubber components, for example, butyl rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, natural rubber, chloroprene rubber, nitrile rubber such as acrylonitrile rubber, hydrogenated nitrile rubber, norbornene rubber, ethylene propylene rubber, ethylene-propylene-diene rubber, acrylic rubber, ethylene-acrylate rubber, fluororubber, chlorosulfonated polyethylene rubber, epichlorohydrin rubber, silicone rubber, urethane rubber, polysulfide rubber, phosphazene rubber or 1,2-polybutadiene etc. can be listed. These can be used alone or in combination of two or more.
[0020] When other rubber components are used, the content of halogenated butyl rubber in the base polymer is preferably 90% by mass or more, more preferably 95% by mass or more, and further preferably 98% by mass or more. In addition, it is also a preferred embodiment that the base polymer consists only of halogenated butyl rubber.
[0021] (Acid Absorber) Next, the acid absorber used in the present invention is described. The acid absorber is compounded to absorb the halogen gas (e.g., hydrogen chloride gas, hydrogen bromide gas) generated when the halogenated butyl rubber is crosslinked. The acid absorber is not particularly limited as long as it can be compounded in the medical rubber composition, and examples thereof include metal oxides, metal hydroxides, hydrotalcites, and the like.
[0022] Specific examples of the metal oxides include magnesium oxide (MgO), zinc oxide (ZnO), calcium oxide (CaO), aluminum oxide (Al2O3), etc. Specific examples of the metal hydroxides include magnesium hydroxide (Mg(OH)2), zinc hydroxide (Zn(OH)2), calcium hydroxide (Ca(OH)2), aluminum hydroxide (Al(OH)3), etc. Specific examples of the hydrotalcites include Mg(OH)2, 4.5 Al2(OH) 13 CO3·3.5H2O、Mg 4.5 Al2(OH) 13 CO3、Mg4Al2(OH) 12 CO3·3.5H2O、Mg6Al2(OH) 16 CO3·4H2O、Mg5Al2(OH) 14 CO3·4H2O、Mg3Al2(OH) 10 Mg-Al hydrotalcites such as CO3·1.7H2O, etc. Any natural or synthetic hydrotalcites can be used. These acid scavengers can be used alone or in combination of two or more.
[0023] In the present invention, the acid scavenger is preferably a metal oxide and / or a metal hydroxide, more preferably at least one selected from MgO, ZnO, Ca(OH)2, and Al(OH)3, and particularly preferably MgO and ZnO.
[0024] Specific examples of magnesium oxide used as the acid absorbent include commercially available products such as "STARMAG R" manufactured by Kojima Chemical Industries, Ltd.
[0025] The BET specific surface area of the acid scavenger used in the present invention is preferably 150 m 2 / g or more, more preferably 160m 2 / g or more, more preferably 170m 2 / g or more, preferably 200m 2 / g or less, more preferably 190m 2 / g or less, more preferably 180m 2 / g or less. When the BET specific surface area of the acid absorbing agent is within the above range, the halogen gas generated during processing is appropriately absorbed by the acid absorbing agent. It should be noted that the BET specific surface area of the acid absorbing agent is a value measured by a gas phase adsorption method using nitrogen as an adsorbed gas. For example, it can be measured according to the measurement method described in JIS Z 8830:2013 "Measurement method for specific surface area of powder (solid) based on gas adsorption".
[0026] The maximum particle size of the acid scavenger used in the present invention is preferably less than 20 μm, more preferably less than 18 μm, and further preferably less than 15 μm. When the maximum particle size of the acid scavenger is less than 20 μm, the undesirable situation that the raw material itself becomes a white spot foreign body can be reduced, and the appearance of the product becomes better. It should be noted that the maximum particle size of the acid scavenger can be measured, for example, by a laser diffraction / scattering method (ultrasonic treatment method).
[0027] The average particle size of the acid scavenger used in the present invention is preferably 2.0 μm or more, more preferably 3.0 μm or more, and preferably 5.0 μm or less, more preferably 4.0 μm or less. When the average particle size of the acid scavenger is within the above range, when the acid scavenger is dispersed in the base polymer, there is no situation where the acid scavenger aggregates and forms white spots, and the acid scavenger can be dispersed more uniformly. It should be noted that the average particle size of the acid scavenger can be measured, for example, by a laser diffraction / scattering method (ultrasonic treatment method). It should be noted that the average particle size is based on volume-based D 50 The value is the average particle size (μm).
[0028] The amount of the acid absorber in the medical rubber composition of the present invention is preferably 1.0 parts by mass or more, more preferably 1.2 parts by mass or more, and further preferably 1.5 parts by mass or more, relative to 100 parts by mass of the base polymer, and further preferably 3.0 parts by mass or less, more preferably 2.5 parts by mass or less, and further preferably 2.0 parts by mass or less. When the content of the acid absorber is 1.0 parts by mass or more, the acid absorption effect on the halogen gas generated in the mixing or molding process of the rubber becomes higher, and the corrosion caused by the halogen gas of the equipment used in these processes can be suppressed. In addition, when the content of the acid absorber is 3.0 parts by mass or less, the dissolution of the acid absorber from the medical rubber product into the drug is suppressed, and the processability (appropriateness of the Mooney viscosity) during molding is also better.
[0029] The molar ratio of the halogen contained in the halogenated butyl rubber to the acid absorbent (halogen / acid absorbent) is preferably 1.0 or less, more preferably 0.8 or less, further preferably 0.7 or less, and preferably 0.3 or more, more preferably 0.4 or more, and further preferably 0.5 or more. When the molar ratio (halogen / acid absorbent) is 1.0 or less, the acid absorption effect of the halogen gas generated in the mixing or forming process of the rubber is further increased, and the corrosion caused by the halogen gas of the equipment used in these processes can be further suppressed. In addition, when the molar ratio (halogen / acid absorbent) is 0.3 or more, the dissolution of the acid absorbent from the medical rubber product into the medicament is further suppressed, and the processability (appropriateness of the Mooney viscosity) during forming is also better. It should be noted that the molar ratio (halogen / acid absorbent) can be calculated by the following formula. Molar ratio (halogen / acid scavenger) = {(mass fraction of halogenated butyl rubber × halogen content in halogenated butyl rubber) / molecular weight of halogen} / {mass fraction of acid scavenger / molecular weight of acid scavenger}
[0030] (Vulcanizing agent) The medical rubber composition of the present invention preferably further contains a vulcanizing agent. The vulcanizing agent is compounded in order to vulcanize the halogenated butyl rubber component contained in the substrate polymer. As the vulcanizing agent, there is no particular limitation as long as it is a vulcanizing agent that can vulcanize the halogenated butyl rubber. As the vulcanizing agent, for example, sulfur, organic peroxides, triazine derivatives, etc. can be cited, and these can be used alone or in combination of two or more.
[0031] Examples of the sulfur include powdered sulfur, finely powdered sulfur, precipitated sulfur, colloidal sulfur, and sulfur chloride.
[0032] As the organic peroxide, dialkyl peroxide, peroxyester, peroxyketal, hydroperoxide, etc. can be cited. As the dialkyl peroxide, for example, di(2-tert-butylperoxyisopropyl)benzene, diisopropylbenzene peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, tert-butylisopropylbenzene peroxide, di-tert-hexyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, etc. can be cited. As the peroxyester, for example, tert-butyl peroxymaleate, tert-butylperoxy-3,3,5-trimethylcyclohexanoate, tert-butyl peroxylaurate, tert-butyl peroxyisopropylmonocarbonate, tert-hexyl peroxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, tert-butyl peroxyacetate, tert-butyl peroxybenzoate, etc. can be cited. Examples of peroxyketals include 1,1-di(tert-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(tert-hexylperoxy)cyclohexane, 1,1-di(tert-butylperoxy)-2-methylcyclohexane, 1,1-di(tert-butylperoxy)cyclohexane, 2,2-di(tert-butylperoxy)butane, 4,4-di(tert-butylperoxy)valerate, and 2,2-di(4,4-di(tert-butylperoxy)cyclohexyl)propane. Examples of hydroperoxides include p-menthane hydroperoxide and diisopropylbenzene hydroperoxide.
[0033] As the triazine derivative, for example, there can be mentioned a compound represented by the general formula (1).
Chemical formula 1
[0034] In the general formula (1), examples of the alkyl group include alkyl groups having 1 to 12 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl, n-hexyl, 1,1-dimethylpropyl, octyl, isooctyl, 2-ethylhexyl, decyl, and dodecyl. Examples of the alkenyl group include alkenyl groups having 1 to 12 carbon atoms, such as vinyl, allyl, 1-propenyl, isopropenyl, 2-butenyl, 1,3-butadienyl, and 2-pentenyl. Examples of the aryl group include monocyclic or condensed polycyclic aromatic hydrocarbon groups, such as aryl groups having 6 to 14 carbon atoms, such as phenyl, naphthyl, anthracenyl, phenanthryl, and acenaphthylenyl groups. Examples of the aralkyl group include aralkyl groups having 7 to 19 carbon atoms, such as benzyl, phenethyl, diphenylmethyl, 1-naphthylmethyl, 2-naphthylmethyl, 2,2-diphenylethyl, 3-phenylpropyl, 4-phenylbutyl, 5-phenylpentyl, 2-biphenylmethyl, 3-biphenylmethyl, or 4-biphenylmethyl. Examples of the alkylaryl group include alkylaryl groups having 7 to 19 carbon atoms, such as tolyl, xylyl, or octylphenyl. Examples of the cycloalkyl group include cycloalkyl groups having 3 to 9 carbon atoms, such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, or cyclononyl.
[0035] Specific examples of the triazine derivative represented by the general formula (1) include 2,4,6-trimercapto-s-triazine, 2-methylamino-4,6-dimercapto-s-triazine, 2-(n-butylamino)-4,6-dimercapto-s-triazine, 2-octylamino-4,6-dimercapto-s-triazine, 2-propylamino-4,6-dimercapto-s-triazine, 2-diallylamino-4,6-dimercapto-s-triazine, 2-dimethylamino-4,6-dimercapto-s-triazine, , 2-dibutylamino-4,6-dimercapto-s-triazine, 2-di(isobutylamino)-4,6-dimercapto-s-triazine, 2-dipropylamino-4,6-dimercapto-s-triazine, 2-di(2-ethylhexyl)amino-4,6-dimercapto-s-triazine, 2-dioleylamino-4,6-dimercapto-s-triazine, 2-laurylamino-4,6-dimercapto-s-triazine or 2-anilino-4,6-dimercapto-s-triazine, or their sodium salts or disodium salts.
[0036] In the present invention, as the vulcanizing agent, sulfur or a triazine derivative is preferably used.
[0037] The content of the vulcanizing agent in the medical rubber composition of the present invention is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and further preferably 0.3 parts by mass or more, relative to 100 parts by mass of the base polymer, and is preferably 5.0 parts by mass or less, more preferably 3.0 parts by mass or less, and further preferably 1.0 parts by mass or less. When the content of the vulcanizing agent is within the above range, a rubber having good rubber properties (hardness, tensile strength, compression set (Compression set: Cset)) and good processability (less scorching) can be obtained.
[0038] The medical rubber composition of the present invention preferably does not contain a vulcanization accelerator. This is because the following situation may occur: the vulcanization accelerator may remain in the rubber product of the final product and dissolve into the medicine in the syringe or vial. Examples of the vulcanization accelerator include guanidine accelerators (e.g., diphenylguanidine), thiuram accelerators (e.g., tetramethylthiuram disulfide, tetramethylthiuram monosulfide), dithiocarbamate accelerators (e.g., zinc dimethyldithiocarbamate), thiazole accelerators (e.g., 2-mercaptobenzothiazole, dibenzothiazole disulfide), and sulfenamide accelerators (N-cyclohexyl-2-benzothiazolesulfenamide, N-tert-butyl-2-benzothiazolesulfenamide).
[0039] (Bulking Agent) The medical rubber composition of the present invention may further contain a filler. As the filler, for example, inorganic fillers such as clay and talc, olefin resins, styrene elastomers, or ultra-high molecular weight polyethylene (UHMWPE) resin powders can be cited. Among these, as the filler, an inorganic filler is preferred, and clay or talc is more preferred. The filler serves to adjust the rubber hardness of the medical rubber product, and also serves as an extender to reduce the production cost of the medical rubber product.
[0040] Examples of the clay include calcined clay and kaolin clay. Specific examples of the clay include SILLITIN (registered trademark) Z manufactured by HOFFMANN MINERAL, SATINTONE (registered trademark) W manufactured by ENGELHARD, NN kaolin clay manufactured by Tsuchiya Kaolin Industry Co., Ltd., and PoleStar 200R manufactured by Imerys Specialities Japan.
[0041] Specific examples of the talc include High Toron A manufactured by Takehara Chemical Industry Co., Ltd., MICRO ACE (registered trademark) K-1 manufactured by Nippon Talc Co., Ltd., and ImerFlex T20 (registered trademark) manufactured by Imerys Specialities Japan Co., Ltd.
[0042] The content of the filler in the medical rubber composition of the present invention is preferably appropriately set according to the rubber hardness of the target medical rubber product, etc. For example, the content of the filler in the medical rubber composition of the present invention is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and further preferably 20 parts by mass or more, and is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and further preferably 100 parts by mass or less, relative to 100 parts by mass of the base polymer.
[0043] (Other ingredients) The medical rubber composition of the present invention may further contain, in addition to the above components, titanium oxide, a colorant such as carbon black, stearic acid, a lubricant such as low-density polyethylene (LDPE), a processing aid, polyethylene glycol as a crosslinking activator, and the like in appropriate proportions.
[0044] The medical rubber composition of the present invention is obtained by kneading a base polymer, an acid scavenger, and other compounding materials added as needed. The kneading can be performed using, for example, an open roll, a closed kneader, etc. The kneaded product is preferably formed into a strip, a sheet, a granule, etc., and more preferably formed into a sheet.
[0045] The Mooney viscosity (ML) of the medical rubber composition of the present invention is 1+4 The Mooney viscosity (ML) is preferably 60 or more, more preferably 62 or more, and is preferably 75 or less, more preferably 70 or less. 1+4 When the (100° C.) is within the above range, the kneading properties of the rubber composition for medical use become better and the processability is further improved.
[0046] <Medical rubber products> The present invention includes a medical rubber product obtained by molding the medical rubber composition of the present invention. The medical rubber product of the present invention can be manufactured by a conventional manufacturing method. For example, by press-molding a medical rubber composition formed into a strip, a sheet, a granular shape, etc., a medical rubber product of a desired shape can be obtained. During the pressing, a crosslinking reaction (vulcanization reaction) of the medical rubber composition is carried out. The molding temperature is, for example, preferably above 130°C, more preferably above 140°C, and preferably below 200°C, more preferably below 190°C. The molding time is preferably above 2 minutes, more preferably above 3 minutes, and preferably below 60 minutes, more preferably below 30 minutes. The molding pressure is preferably above 0.1MPa, more preferably above 0.2MPa, and preferably below 10MPa, more preferably below 8MPa.
[0047] Unnecessary parts are cut off from the molded product after press molding to form a specified shape. The obtained molded product is cleaned, sterilized, dried and packaged to manufacture medical rubber products.
[0048] In addition, for the medical rubber product of the present invention, a resin film can be laminated in the same manner as in the past to be integrated. As the resin film, for example, films of inactive resins such as polytetrafluoroethylene (PTFE), tetrafluoroethylene-ethylene copolymer (ETFE) and their modified products, and ultra-high density polyethylene (UHMWPE) can be listed.
[0049] The resin film may be press-molded in a state of being overlapped on the rubber composition in a sheet form, for example, and may be integrated with the medical rubber product formed by the press molding.
[0050] The medical rubber product of the present invention is particularly suitable for use as a medical rubber product that can come into contact with medicines, blood, etc. Specific examples of the medical rubber product of the present invention include rubber stoppers for containers of various medicines such as liquid preparations, powder preparations, and freeze-dried preparations, medical rubber stoppers such as rubber stoppers for vacuum blood collection tubes, and sliding or sealing parts such as stoppers for syringes.
[0051] Figure 1 This is a diagram showing a medical syringe using the medical rubber component product of the present invention, a so-called prefilled syringe, in an exploded state. Figure 1 In the figure, the syringe 11 and half of the stopper 13 are shown in cross-section. The prefilled syringe 10 includes: a cylindrical syringe 11; a plunger 12 combined with the syringe 11 and capable of reciprocating in the syringe 11; and a stopper 13 mounted on the front end of the plunger 12. The stopper 13 is formed from the medical rubber composition of the present invention. A laminate film for improving sliding properties may be laminated on the surface of the stopper 13.
[0052] The plunger 12 is composed of, for example, a resin plate having a cross-shaped cross section, and has a head 18 at its front end for mounting the stopper 13. The head 18 is formed integrally with the plunger 12, is made of resin, and is processed into an external thread shape. The stopper 13 is a roughly cylindrical shape with a short axis, and its front end surface is formed into, for example, a blunt-angled mountain shape protruding from the center of the axis. And a fitting recess 15 in the shape of an internal thread carved in the axial direction from the rear end surface is formed. The stopper 13 is mounted on the front end of the plunger 12 by screwing the head 18 of the plunger 12 into the fitting recess 15 of the stopper 13.
[0053] Figure 2 This is a schematic cross-sectional view of a specific example of a rubber stopper 20 as the medical rubber product of the present invention. Figure 3 The state where the opening 24 b of the container 24 filled with the medicine is sealed with the rubber stopper 20 is shown.
[0054] The rubber stopper 20 is composed of a top plate 21 and a stopper leg 22. The top plate 21 has a puncture portion 23 that can be punctured by an injection needle of a syringe, and a flange portion 21b that contacts the upper edge surface 24a of the container mouth of a medical container 24. The stopper leg 22 protrudes toward the lower surface of the top plate 21 and is embedded in the medical container mouth. In addition, the stopper leg 22 has a substantially cylindrical shape and is provided with a cutout 27. A nylon film layer 26 is provided on the top surface of the top plate 21 of the rubber stopper 20. By providing the nylon film layer 26 on the top surface of the rubber stopper 20, mechanical transportability during the manufacture of pharmaceuticals can be ensured. In addition, by providing the nylon film layer 26 on the top surface of the rubber stopper 20, the surface slipperiness of the top surface can be improved, and the generation of needle puncture fragments can be prevented when the injection needle punctures.
[0055] exist Figure 3 In the illustrated embodiment, a vial for storing a freeze-dried preparation is used as the container 24. When the liquid medicine stored in the container 24 is a liquid medicine for injection, the injection needle of the syringe pierces the piercing portion 23 of the top plate 21 so that the liquid medicine for injection is sucked into the syringe without opening the rubber stopper 20. In this way, the rubber stopper 20 is not opened to prevent foreign matter from mixing into the liquid medicine for injection in the container 24.
[0056] On the top plate 21, a metal or resin cover 25 is provided which can cover the opening 24b of the container 24 and the rubber stopper 20. The rubber stopper 20 (including the opening 24b) is sealed with the cover 25 to prevent bacteria from adhering to the puncture portion 23 where the injection needle of the syringe punctures, and to prevent bacteria from mixing into the injection liquid through the injection needle. As the type of cover 25, a flip-off cap, a pull-top cap, a clean cap, etc. can be used. In the case of using a large amount of injection liquid like a hospital, it is preferable to use a clean cap that can be opened with one hand and is easy to operate.
[0057] Figure 4 : is an explanatory diagram showing an example of a vacuum blood collection tube. The vacuum blood collection tube 50 includes a bottom tube 51 and a rubber stopper 53 that seals the opening of the bottom tube 51. Such a rubber stopper 53 is formed from the medical rubber composition of the present invention. It is designed to automatically collect blood by reducing the pressure inside the blood collection tube. Example
[0058] Hereinafter, the present invention will be described in detail by way of examples, but the present invention is not limited to the following examples, and any changes and embodiments that do not depart from the spirit and scope of the present invention are included in the scope of the present invention.
[0059] [Preparation of rubber composition for medical use] The medical rubber composition was prepared by kneading the materials shown in Table 1. The kneading was performed at 80° C. to 140° C. for 5 to 30 minutes using a closed type pressure kneader.
[0060] [Table 1]
[0061] The details of the compounding materials used are shown below. Bromobutyl rubber: BROMOBUTYL 2255 manufactured by Nippon Butyl Rubber Co., Ltd. [Bromine content: 2.0%] Acid absorbent 1: STARMAG (registered trademark) R (magnesium oxide, BET specific surface area 178 m2) manufactured by Kamishima Chemical Industry Co., Ltd.2 / g, maximum particle size 13μm, average particle size 3.5μm) Acid absorbent 2: MAGSARAT (registered trademark) 150ST (magnesium oxide, BET specific surface area 65 m2) manufactured by Kyowa Chemical Industry Co., Ltd. 2 / g, maximum particle size 20μm, average particle size 4.8μm) Acid absorbent 3: STARMAG (registered trademark) M (magnesium oxide, BET specific surface area 47 m2) manufactured by Kamishima Chemical Industry Co., Ltd. 2 / g, maximum particle size 262μm, average particle size 3.5μm) Sulfur: 5% oil-containing sulfur manufactured by Tsurumi Chemical Co., Ltd. Talc: ImerFlex T20 (registered trademark) manufactured by Imerys Specialities Titanium oxide: TIPAQUE (registered trademark) A-100 manufactured by Ishihara Industry Co., Ltd. Carbon black: Thermax MT manufactured by Cancarb Limited
[0062] [Evaluation method] (1) Mooney viscosity The Mooney viscosity of the medical rubber composition is measured according to the measurement method described in JIS K6300-1:2013 “Method for measuring viscosity and scorch time using a Mooney viscometer”.
[0063] (2) BET specific surface area of the acid scavenger (m 2 / g) The BET specific surface area was measured under the following conditions. Measuring device: Macsorp HM model (manufactured by MOUNTECH Co., Ltd.) Pretreatment conditions: 160°C, 1 hour Method for determining the amount of adsorbed gas: carrier gas method Analysis method of adsorption data: single point method
[0064] (3) Particle size of acid absorbent (μm) 50 mL of ethanol was collected in a 100 mL beaker, and about 0.2 g of the sample powder was added. The dispersion was prepared by ultrasonic treatment (UD-201 manufactured by TOMY Seiko Co., Ltd.) for 3 minutes. The prepared solution was measured using a laser diffraction method-particle size distribution meter (Microtrac HRA Model 9320-X100 manufactured by Nikkiso Co., Ltd.). From the obtained particle size distribution, the volume-based D 50 value and maximum particle size.
[0065] (4) Appearance inspection The medical rubber composition prepared above was press-molded under the conditions of 15 to 20 atmospheres and 165° C. to 190° C. for 7 to 20 minutes to prepare a slab (length 225 mm, width 60 mm, thickness 2 mm). The surface of the slab was visually observed to confirm white spots caused by the acid absorber, and the appearance was evaluated according to the following evaluation criteria. ○: No white spots caused by the acid absorber were observed. △: Only one white spot foreign matter caused by the acid absorber was confirmed. ×: Two or more white spots of foreign matter caused by the acid absorber were observed.
[0066] (5) Dissolution test The medical rubber composition prepared above was press-molded under the conditions of 15 to 20 atmospheres and 165° C. to 190° C. for 7 to 20 minutes to prepare a measurement sample for the elution test ( Thickness 2mm sample). The prepared test sample was washed three times with water or an alkaline aqueous solution such as an aqueous sodium carbonate solution using an autoclave: the prepared test sample was washed at 121°C for 30 minutes and then immersed in water. 200g of physiological saline was placed in a glass bottle, and the test solution immersed in the washed sample was stored in an oven at 40°C for a specified time (0 hours, 6 hours, 24 hours, 48 hours, 72 hours, 96 hours, 168 hours, 336 hours, 504 hours). In addition, a blank test solution in which only 200g of physiological saline was added to the glass bottle was also stored in an oven at 40°C for a specified time. After a certain period of time, the test solution and the blank test solution were taken out of the oven, cooled to room temperature, and then the pH of each was measured using a pH measuring device (LAQUAD-210P manufactured by Horiba, Ltd.), and the pH difference between them was calculated. The non-dissolution property of the acid absorber is evaluated using the maximum value (peak value) of the pH difference between the test solution and the blank test solution within the predetermined time according to the following evaluation criteria: The smaller the pH difference, the less dissolution of the acid absorber. ○: The maximum pH difference between the test solution and the blank test solution is less than 1.05. ×: The maximum pH difference between the test solution and the blank test solution is 1.05 or more.
[0067] (6) Equipment corrosion After kneading the medical rubber composition at 80° C. to 140° C. for 5 to 30 minutes, the metal surface of the kneading machine was visually observed and the corrosion of the equipment was evaluated according to the following evaluation criteria. 0: The metal is not corroded and the surface gloss is maintained. △: The metal is slightly corroded and the surface gloss is reduced. ×: The metal is corroded and loses its surface gloss. With continued use, dirt adheres and the color turns brown.
[0068] The evaluation results of each item are shown in Table 1.
[0069] According to the results in Table 1, it is clear that the base polymer containing halogenated butyl rubber and the acid scavenger, the content of the acid scavenger is 1 to 3 parts by mass relative to 100 parts by mass of the base polymer, and the BET specific surface area of the acid scavenger is 150 m 2 / g~200m 2 The medical rubber composition of the present invention having an average molecular weight of 100 μg / cm2 can suppress the corrosion of equipment caused by halogen gas and reduce the elution of the acid absorbent into the drug solution (maintain the pH of the drug solution).
[0070] [Industrial Applicability]
[0071] The present invention can be applied to a medical rubber composition and a medical rubber product.
[0072] A preferred embodiment (1) of the present invention is a medical rubber composition, characterized in that it contains a base polymer containing a halogenated butyl rubber and an acid scavenger, wherein the amount of the acid scavenger blended is 1 to 3 parts by mass relative to 100 parts by mass of the base polymer, and the BET specific surface area of the acid scavenger is 150 m 2 / g~200m 2 / g.
[0073] A preferred embodiment (2) of the present invention is the medical rubber composition according to embodiment (1), wherein the halogenated butyl rubber is chlorinated butyl rubber or brominated butyl rubber.
[0074] A preferred embodiment (3) of the present invention is the medical rubber composition according to embodiment (1) or (2), wherein the acid scavenger contains magnesium oxide or zinc oxide.
[0075] A preferred embodiment (4) of the present invention is the rubber composition for medical use according to any one of embodiments (1) to (3), wherein the maximum particle size of the acid scavenger is less than 20 μm.
[0076] A preferred embodiment (5) of the present invention is the rubber composition for medical use according to any one of embodiments (1) to (4), wherein the rubber composition for medical use further contains a vulcanizing agent.
[0077] A preferred embodiment (6) of the present invention is the rubber composition for medical use according to any one of embodiments (1) to (5), wherein the rubber composition for medical use further contains a filler.
[0078] A preferred embodiment (7) of the present invention is the medical rubber composition according to any one of embodiments (1) to (6), wherein the Mooney viscosity (ML 1+4 (100℃)) is 60~75.
[0079] A preferred embodiment (8) of the present invention is a medical rubber product obtained by molding the medical rubber composition according to any one of embodiments (1) to (7).
[0080] A preferred embodiment (9) of the present invention is the medical rubber product according to embodiment (8), wherein the medical rubber product is a stopper for a syringe.
Claims
1. A medical rubber composition, characterized in that: Containing a base polymer comprising halogenated butyl rubber and an acid scavenger, The amount of the acid scavenger is 1 to 3 parts by mass relative to 100 parts by mass of the base polymer. The BET specific surface area of the acid scavenger is 150 m 2 / g~200m 2 / g.
2. The medical rubber composition according to claim 1, wherein The halogenated butyl rubber is chlorinated butyl rubber or brominated butyl rubber.
3. The medical rubber composition according to claim 1, wherein The acid scavenger comprises magnesium oxide or zinc oxide.
4. The medical rubber composition according to claim 1, wherein The maximum particle size of the acid scavenger is less than 20 μm.
5. The medical rubber composition according to claim 1, wherein The medical rubber composition further contains a vulcanizing agent.
6. The medical rubber composition according to claim 1, wherein The medical rubber composition further contains a filler.
7. The medical rubber composition according to claim 1, wherein The Mooney viscosity of the medical rubber composition at 100°C, ML 1+4 It is 60 to 75.
8. A medical rubber product, characterized in that: The rubber composition for medical use according to any one of claims 1 to 7 is obtained by molding.
9. The medical rubber product according to claim 8, wherein: The medical rubber product is a stopper for a syringe.
Citation Information
Patent Citations
Medical rubber composition and medical rubber component
JP2021080370A