Degradable modified PS plastic bowl and preparation method thereof

By melt-blending flame-retardant polylactic acid, PS-trimellitic anhydride copolymer and degradable polyurethane and molding them, the problem of poor degradability and insufficient mechanical properties of PS plastic in daily necessities was solved, and the production of modified PS plastic bowls was realized. High biodegradability and flame retardant properties.

CN118812973AInactive Publication Date: 2024-10-22WUXI FANGCHENG PACKAGING TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411305767.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing PS plastics have problems with poor degradability, insufficient mechanical properties and insufficient flame retardant properties when used in daily necessities.

Method used

Flame-retardant polylactic acid, PS-trimellitic anhydride copolymer and degradable polyurethane are used for melt blending, and a degradable modified PS plastic bowl is prepared through molding. The reaction of hexachlorocyclotriphosphazene and ethylenediamine is used to form a stable plastic bowl. The phosphate bond, combined with the amino reaction of TAIC, improves the cross-linking density and flame retardant properties.

Benefits of technology

The biodegradability, mechanical properties and flame retardant properties of the modified PS plastic bowl are improved, achieving easy degradation and high stability in the natural environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a degradable modified PS (polystyrene) plastic bowl and a preparation method thereof, belongs to the technical field of high polymer materials, and is used for solving the technical problems that in the prior art, when PS is applied to manufacturing of daily supplies such as plastic bowls, the degradability is poor, and the mechanical property and flame retardant property of the PS are poor. The preparation method comprises the following steps: adding flame-retardant polylactic acid, a PS-trimellitic anhydride copolymer and degradable polyurethane into a torque rheometer, carrying out melt blending to obtain a blend, carrying out compression molding on the blend, and carrying out pressure-maintaining cooling to obtain the degradable modified PS plastic bowl. Trimellitic anhydride is used for improving the degradability of polystyrene, and a soft segment chain, a hard segment chain and a small molecule chain extender which are easy to degrade are used for designing degradable polyurethane, so that the modified PS plastic bowl which is easy to degrade and good in mechanical property and flame retardant property is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a degradable modified PS plastic bowl and a preparation method thereof. Background Art

[0002] Plastic products represented by PS are widely used due to their low cost, chemical stability, good ductility and corrosion resistance. However, most plastics are abandoned or landfilled in the natural environment. These plastic products that enter the environment will decompose into smaller plastic particles under physical, chemical and biological effects, and continue to accumulate in sediments, soil and other media. Therefore, they are regarded as a potential persistent organic pollutant. Modifying PS plastics to prepare degradable modified PS plastics has positive practical significance and has attracted widespread attention. In addition, the poor flame retardancy and mechanical properties of PS plastics are also technical problems that need to be solved urgently.

[0003] Patent application CN105255094A discloses a method for preparing a composite recycled PS / ABS / PP cross-linked modified flame retardant plastic. Waste ABS, PS, PP plastics, modified graphene and related additives such as toughening agents are mixed to obtain a premix; the premix is ​​melt-extruded, stretched, cooled, dried and granulated to obtain a composite recycled PS / ABS / PP cross-linked modified flame retardant plastic. The above-mentioned prior art uses graphene as a flame retardant to improve the flame retardant properties of the material; and uses waste nitrile rubber as a toughening agent to improve the mechanical properties of the material. However, as an inorganic material, graphene has poor compatibility with plastics and cannot be evenly distributed; in addition, the degradation of nitrile rubber is slow, which reduces the degradability of recycled plastics.

[0004] Patent application CN1147529A discloses a formula and production process of a filled modified reinforced PE / PP / PS composite material. Mica is modified with potassium hydrogen fluoride, asbestos is modified with sulfonyl azide silane coupling agent, and calcium carbonate is modified with aluminate coupling agent. The three modified fillers are then blended with three matrix resins of polyethylene, polypropylene and PS, and related additives to prepare a PE / PP / PS composite material with high hardness and high rigidity. However, the composite material prepared by the above prior art using three matrix resins of polyethylene, polypropylene and PS still has the technical problem of poor degradability.

[0005] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a degradable modified PS plastic bowl, which is used to solve the technical problems in the prior art that when PS plastic is used in the manufacture of daily necessities, the PS plastic has poor degradability and poor mechanical properties and flame retardant properties.

[0007] The purpose of the present invention can be achieved through the following technical solutions: A method for preparing a degradable modified PS plastic bowl comprises the following steps: According to weight parts, 10-20 parts of flame-retardant polylactic acid, 100 parts of PS-trimellitic anhydride copolymer and 5-10 parts of degradable polyurethane are added to a torque rheometer, melt-blended to obtain a blend; the blend is compression-molded in a mold, cooled under pressure, and a degradable modified PS plastic bowl is obtained.

[0008] The method for preparing the flame retardant polylactic acid comprises the following steps: S1, hexachlorocyclotriphosphazene and ethanol are evenly mixed to obtain an ethanol solution of hexachlorocyclotriphosphazene; S2, anhydrous potassium carbonate and ethylenediamine are evenly mixed to obtain a mixed solid-liquid; an ethanol solution of hexachlorocyclotriphosphazene is added dropwise to the mixed solid-liquid at 5-10°C, and after the addition is completed, the temperature is raised to 20°C, and the reaction is continued for 2-3 hours to obtain a reaction liquid; the reaction liquid is heated to 80-90°C, the solvent is removed by reaction, and a solid is obtained; the solid is washed with deionized water and vacuum dried to obtain a solid intermediate A; S3, mixing TAIC and solid intermediate A, and then adding polylactic acid to blend to obtain a blend; adding the blend to a torque rheometer, blending at 190-200° C. for 5-10 minutes to obtain flame-retardant polylactic acid.

[0009] The reaction mechanism of hexachlorocyclotriphosphazene and ethylenediamine is as follows:

[0010] Reaction principle of solid intermediate A and TAIC:

[0011] Hexachlorocyclotriphosphazene has an active phosphorus-chlorine bond, which can react with ethylenediamine to remove hydrogen chloride to obtain a stable phosphate bond, thereby obtaining a solid intermediate A. The solid intermediate A and the amino group of TAIC undergo an addition reaction to form a CN single bond, thereby obtaining a flame-retardant polylactic acid with a certain crosslinking density.

[0012] Furthermore, in step S1, the usage ratio of hexachlorocyclotriphosphazene and ethanol is 35-45 g:200 mL; in step S2, the usage ratio of anhydrous potassium carbonate and ethylenediamine is 10 g:35-50 mL; in step S2, the vacuum drying temperature is 70-80° C. and the vacuum drying time is 30-60 min.

[0013] Furthermore, in step S3, the usage ratio of TAIC, intermediate A and polylactic acid is 5-10g:30-40g:200-300g; the mixing speed is 100r / min, and the mixing time is 5min; the blending speed is 100r / min, and the blending time is 5-10min.

[0014] Furthermore, the preparation method of the PS-trimellitic anhydride copolymer comprises the following steps: PS, trimellitic anhydride and DMF are mixed evenly, and then an initiator BPO is added, and the temperature is raised to 120-140°C, and the reaction is carried out for 3 hours to obtain a mixed solid-liquid; the mixed solid-liquid is then heated to 155-160°C, and the DMF solvent is distilled off to obtain a solid; the solid is washed with deionized water and then vacuum dried to obtain a PS-trimellitic anhydride copolymer.

[0015] The invention uses PS and trimellitic anhydride as reactants, uses DMF as solvent, and generates copolymerization reaction under the action of an initiator to obtain a PS-trimellitic anhydride copolymer.

[0016] Furthermore, the usage ratio of PS, trimellitic anhydride, DMF and initiator BPO is 8-10g:10-15g:100mL:0.3g; the vacuum drying temperature is 70-80°C, and the vacuum drying time is 30min.

[0017] Furthermore, the degradable polyurethane is prepared by the following steps: A1. Mix sorbitol and polyol vegetable oil, raise the temperature to 80-100° C., then add toluene diisocyanate, stir to obtain a mixed solid-liquid; add a catalyst to the mixed solid-liquid, and react at a constant temperature of 80° C. for 3-5 hours to obtain a polymer; A2. Add 10-20 g of a small molecule chain extender to the polymer, stir at a constant temperature of 50-60° C. for 10-20 min to obtain a sample; cast the sample in a polytetrafluoroethylene mold, and cure at 70° C. for 5-7 days to obtain a degradable polyurethane.

[0018] The present invention uses sorbitol and castor oil containing polyols as soft forging chains, and toluene diisocyanate and small molecular diols as hard segment chains, so as to prepare a degradable polyurethane that is easily degradable and pollution-free to the environment. Specifically, sorbitol and castor oil are physically blended according to a certain mass ratio, and the -NCO in toluene diisocyanate reacts with the -OH group in sorbitol and castor oil to produce carbamate to form a prepolymer; then a small molecular diol with active hydrogen is used as a chain extender to extend the chain with the remaining isocyanate in the reaction to form a polymer, so as to prepare a degradable polyurethane; then the chain extender and the prepolymer are reacted to prepare a cross-linked polyurethane. The incompatibility between the soft and hard segments in the polyurethane and the strong polarity of the polyurethane molecules allow the intermolecular interaction to form a crystalline region and produce microphase separation, so that it can serve as a mechanical property reinforcement component of the prepared composite material.

[0019] Furthermore, in step A1, the polyol vegetable oil is any one of castor oil, soybean oil or palm oil and a combination thereof, and the catalyst is dibutyltin dilaurate; the dosage ratio of sorbitol, polyol vegetable oil, toluene diisocyanate and catalyst is 18-25g:5-10mL:17g:0.3-0.5g; the stirring speed is 5-10min and the stirring time is 100r / min; in step A2, the small molecule chain extender is any one of ethylene glycol, 1,3-butanediol, 1,4-butanediol or 1,6-propylene glycol and a combination thereof.

[0020] Furthermore, the temperature of melt blending is 180-200°C, the rotation speed is 50r / min, the melt blending time is 10-20min; the molding time is 8-10min, the molding pressure is 10MPa; and the pressure holding cooling time is 10min.

[0021] As another aspect of the present invention, a method for preparing a degradable modified PS plastic bowl provides a degradable modified PS plastic bowl.

[0022] The present invention has the following beneficial effects: 1. The degradable modified PS plastic bowl prepared by the present invention is obtained by melt blending and compression molding of flame-retardant polylactic acid, PS-trimellitic anhydride copolymer and degradable polyurethane. Polylactic acid is a degradable thermoplastic polymer. After use, polylactic acid can be hydrolyzed into lactic acid; PS itself has poor degradability. When trimellitic anhydride and PS are blended, trimellitic anhydride has a strong electron-withdrawing group, so it has positive polarity. PS gives electrons due to the conjugation effect of the benzene ring and has negative polarity; PS and trimellitic anhydride copolymerize to form a stable state of attraction between positive and negative electrodes, thereby accelerating the biodegradability of PS-trimellitic anhydride copolymer; polyurethane is difficult to degrade in the natural environment, and environmentally friendly sorbitol and castor oil are used as the soft segment chain of the degradable polyurethane, small molecular weight toluene diisocyanate is used as the hard segment chain, and diol is used as a small molecule chain extender, thereby reducing the molecular weight of the degradable polyurethane and improving the degradability of the degradable polyurethane. The three components are melt-blended and then compression-molded to prepare an easily degradable modified PS plastic bowl.

[0023] 2. The polylactic acid, PS and polyurethane used in the present invention are all flammable plastics. In order to improve the flammability of the prepared plastic bowls, the present invention designs a flame retardant small molecule and polylactic acid for compounding to obtain flame retardant polylactic acid; hexachlorocyclotriphosphazene has high nitrogen and phosphorus elements and is itself an efficient flame retardant small molecule; however, the phosphorus-chlorine bond of hexachlorocyclotriphosphazene is too active and cannot be used as a stable flame retardant small molecule and polylactic acid for compounding; the present invention reacts ethylenediamine and hexachlorocyclotriphosphazene, which not only realizes the halogen-free flame retardant small molecule, but also can further improve the stability of the flame retardant small molecule. Under the high temperature conditions of melt blending, the residual amino groups of the flame retardant small molecules can undergo a dehydration reaction with trimellitic anhydride and a dehydration reaction with the excess hydroxyl groups of the degradable polyurethane, which can improve the complex strength between the three matrix plastics and improve the stability of the prepared modified PS plastic bowl.

[0024] 3. As separate matrix resins, polylactic acid, PS and polyurethane all have technical problems of low elongation at break and poor mechanical properties. By melt blending the three and melt cross-linking the matrix components, the prepared composite material has higher mechanical properties. For polylactic acid, the composite flame retardant small molecules are cross-linked with a cross-linking agent. By increasing the cross-linking density of the flame retardant small molecules, not only the stability of the flame retardant small molecules is increased by increasing the molecular weight, but also the mechanical properties of polylactic acid itself are improved. In addition, under the high temperature conditions of melt blending, the carbonyl functional group in the cross-linking agent TAIC can react with the excess hydroxyl groups in the polyurethane to increase the cross-linking density between the components, thereby helping to improve the mechanical properties of the modified PS plastic bowl. DETAILED DESCRIPTION

[0025] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1 This embodiment provides a method for preparing a flame retardant polylactic acid, comprising the following steps: S1, 35g of hexachlorocyclotriphosphazene and 200mL of ethanol were mixed evenly to obtain an ethanol solution of hexachlorocyclotriphosphazene. 10g of anhydrous potassium carbonate and 35mL of ethylenediamine were added to a 500mL three-necked flask, and the mixture was shaken to obtain a mixed solid-liquid mixture; a thermometer was connected to one end of the three-necked flask, and a constant pressure dropping funnel was set at the other end, and then the three-necked flask was transferred to a water bath, and all the ethanol solution of hexachlorocyclotriphosphazene was added thereto through a constant pressure dropping funnel at 5°C. After the addition was completed, the temperature was raised to 20°C, and the reaction was continued for 3h to obtain a reaction solution; the reaction solution was heated to 80°C, and the solvent was removed by reaction to obtain a solid; the solid was washed three times with deionized water, and then vacuum dried at 70-80°C for 30-60min to obtain a solid intermediate A.

[0027] S2. 5 g of TAIC and 30 g of solid intermediate A were blended at 100 r / min for 5 min, and then 200 g of polylactic acid was added and blended at 100 r / min for 5 min to obtain a blend; the blend was transferred to a torque rheometer and blended at 190° C. for 5 min to obtain a flame retardant polylactic acid.

[0028] Example 2 This embodiment provides a method for preparing a flame retardant polylactic acid, comprising the following steps: S1, 40g of hexachlorocyclotriphosphazene and 200mL of ethanol were mixed evenly to obtain an ethanol solution of hexachlorocyclotriphosphazene. 10g of anhydrous potassium carbonate and 45mL of ethylenediamine were added to a 500mL three-necked flask, and the mixture was shaken to obtain a mixed solid-liquid mixture; a thermometer was connected to one end of the three-necked flask, and a constant pressure dropping funnel was set at the other end, and then the three-necked flask was transferred to a water bath, and all the ethanol solution of hexachlorocyclotriphosphazene was added thereto through a constant pressure dropping funnel at 8°C. After the addition was completed, the temperature was raised to 20°C, and the reaction was continued for 2.5h to obtain a reaction solution; the reaction solution was heated to 85°C, and the solvent was removed by reaction to obtain a solid; the solid was washed three times with deionized water, and then vacuum dried at 73°C for 50min to obtain a solid intermediate A.

[0029] S2. 8 g of TAIC and 33 g of solid intermediate A were blended at 100 r / min for 5 min, and then 260 g of polylactic acid was added and blended at 100 r / min for 6 min to obtain a blend; the blend was transferred to a torque rheometer and blended at 195° C. for 6 min to obtain a flame retardant polylactic acid.

[0030] Example 3 This embodiment provides a method for preparing a flame retardant polylactic acid, comprising the following steps: S1, 45g of hexachlorocyclotriphosphazene and 200mL of ethanol were mixed evenly to obtain an ethanol solution of hexachlorocyclotriphosphazene. 10g of anhydrous potassium carbonate and 50mL of ethylenediamine were added to a 500mL three-necked flask, and the mixture was shaken to obtain a mixed solid-liquid mixture; a thermometer was connected to one end of the three-necked flask, and a constant pressure dropping funnel was set at the other end, and then the three-necked flask was transferred to a water bath, and all the ethanol solution of hexachlorocyclotriphosphazene was added thereto through a constant pressure dropping funnel at 10°C. After the addition was completed, the temperature was raised to 20°C, and the reaction was continued for 2h to obtain a reaction solution; the reaction solution was heated to 90°C, and the solvent was removed by reaction to obtain a solid; the solid was washed three times with deionized water, and then vacuum dried at 80°C for 60min to obtain a solid intermediate A.

[0031] S2. 10 g of TAIC and 40 g of solid intermediate A were blended at 100 r / min for 5 min, and then 300 g of polylactic acid was added and blended at 100 r / min for 10 min to obtain a blend; the blend was transferred to a torque rheometer and blended at 200° C. for 10 min to obtain a flame retardant polylactic acid.

[0032] Example 4 This embodiment provides a method for preparing a PS-trimellitic anhydride copolymer, comprising the following steps: One end of a 250mL three-necked flask was connected to an electric stirrer, one end was connected to a reflux device, and one end was connected to a thermometer, and then 8g of PS, 10g of trimellitic anhydride and 100mL of DMF were added and mixed evenly; then 0.3g of initiator BPO was added to the three-necked flask, and the three-necked flask was transferred to a water bath, heated to 120°C, and reacted for 3h to obtain a mixed solid-liquid; then the mixed solid-liquid was heated to 155°C, and the DMF solvent was distilled off to obtain a solid. The solid was washed with deionized water and then dried in a vacuum drying oven at 70°C for 30min to obtain a PS-trimellitic anhydride copolymer.

[0033] Example 5 This embodiment provides a method for preparing a PS-trimellitic anhydride copolymer, comprising the following steps: One end of a 250mL three-necked flask was connected to an electric stirrer, one end was connected to a reflux device, and one end was connected to a thermometer, and then 9g of PS, 12g of trimellitic anhydride and 100mL of DMF were added and mixed evenly; then 0.3g of initiator BPO was added to the three-necked flask, and the three-necked flask was transferred to a water bath, heated to 130°C, and reacted for 3h to obtain a mixed solid-liquid; then the mixed solid-liquid was heated to 158°C, and the DMF solvent was distilled off to obtain a solid. The solid was washed with deionized water and then dried in a vacuum drying oven at 6°C for 30min to obtain a PS-trimellitic anhydride copolymer.

[0034] Example 6 This embodiment provides a method for preparing a PS-trimellitic anhydride copolymer, comprising the following steps: One end of a 250mL three-necked flask was connected to an electric stirrer, one end was connected to a reflux device, and one end was connected to a thermometer, and then 10g of PS, 15g of trimellitic anhydride and 100mL of DMF were added and mixed evenly; then 0.3g of initiator BPO was added to the three-necked flask, and the three-necked flask was transferred to a water bath, heated to 140°C, and reacted for 3h to obtain a mixed solid-liquid; then the mixed solid-liquid was heated to 160°C, and the DMF solvent was distilled off to obtain a solid. The solid was washed with deionized water, and then dried in a vacuum drying oven at 80°C for 30min to obtain a PS-trimellitic anhydride copolymer.

[0035] Example 7 This embodiment provides a method for preparing a degradable polyurethane, comprising the following steps: 1. Add 18 g of sorbitol and 5 mL of palm oil into a 250 mL three-necked flask with a condensing device; then heat the three-necked flask to 80°C, add 17 g of toluene diisocyanate into the three-necked flask, stir at 100 r / min for 5 min to obtain a mixed solid-liquid; add 0.3 g of catalyst dibutyltin dilaurate into the mixed solid-liquid, react at a constant temperature of 80°C for 3 h to obtain a polymer.

[0036] 10 g of ethylene glycol was added to the polymer, and the mixture was stirred at a constant temperature of 50° C. for 10 minutes to obtain a sample; the sample was cast in a polytetrafluoroethylene mold, and cured at 70° C. for 5 days to obtain a degradable polyurethane.

[0037] Example 8 This embodiment provides a method for preparing a degradable polyurethane, comprising the following steps: 1. Add 22g of sorbitol and 6mL of castor oil into a 250mL three-necked flask with a condensing device; then heat the three-necked flask to 90°C, add 17g of toluene diisocyanate into the three-necked flask, stir at 100r / min for 6min to obtain a mixed solid-liquid; add 0.3g of catalyst dibutyltin dilaurate into the mixed solid-liquid, react at a constant temperature of 80°C for 3h to obtain a polymer.

[0038] 2. Add 15 g of 1,3-butanediol to the polymer, stir at a constant temperature of 53° C. for 15 minutes to obtain a sample; cast the sample in a polytetrafluoroethylene mold, and cure it at 70° C. for 5 days to obtain a degradable polyurethane.

[0039] Example 9 This embodiment provides a method for preparing a degradable polyurethane, comprising the following steps: 1. Add 25 g of sorbitol and 10 mL of soybean oil into a 250 mL three-necked flask with a condensing device; then heat the three-necked flask to 100 ° C, add 17 g of toluene diisocyanate into the three-necked flask, stir at 100 r / min for 10 min to obtain a mixed solid-liquid; add 0.5 g of catalyst dibutyltin dilaurate into the mixed solid-liquid, react at a constant temperature of 80 ° C for 5 h to obtain a polymer.

[0040] 2. Add 20 g of 1,6-propylene glycol to the polymer, stir at a constant temperature of 60° C. for 20 minutes to obtain a sample; cast the sample in a polytetrafluoroethylene mold, and cure it at 70° C. for 7 days to obtain a degradable polyurethane.

[0041] Example 10 This embodiment provides a method for preparing a degradable modified PS plastic bowl, comprising the following steps: According to parts by weight, 10 parts of the flame-retardant polylactic acid prepared in Example 1, 100 parts of the PS-trimellitic anhydride copolymer prepared in Example 4, and 5 parts of the degradable polyurethane prepared in Example 7 were added to a torque rheometer for melt blending to obtain a blend; wherein the melt blending temperature is 180°C, the rotation speed is 50r / min, and the melt blending time is 10min; the blend is compression molded in a mold, wherein the molding time is 8min, the molding pressure is 10MPa, and then the pressure is maintained and cooled for 10min to obtain a degradable modified PS plastic bowl.

[0042] Embodiment 11 This embodiment provides a method for preparing a degradable modified PS plastic bowl, comprising the following steps: According to parts by weight, 10 parts of the flame-retardant polylactic acid prepared in Example 2, 100 parts of the PS-trimellitic anhydride copolymer prepared in Example 5, and 5 parts of the degradable polyurethane prepared in Example 8 were added to a torque rheometer for melt blending to obtain a blend; wherein the melt blending temperature is 180°C, the rotation speed is 50r / min, and the melt blending time is 10min; the blend is compression molded in a mold, wherein the molding time is 8min, the molding pressure is 10MPa, and then the pressure is maintained and cooled for 10min to obtain a degradable modified PS plastic bowl.

[0043] Example 12 This embodiment provides a method for preparing a degradable modified PS plastic bowl, comprising the following steps: According to parts by weight, 20 parts of the flame-retardant polylactic acid prepared in Example 3, 100 parts of the PS-trimellitic anhydride copolymer prepared in Example 6, and 10 parts of the degradable polyurethane prepared in Example 9 were added to a torque rheometer for melt blending to obtain a blend; wherein the melt blending temperature was 200°C, the rotation speed was 50r / min, and the melt blending time was 20min; the blend was compression molded in a mold, wherein the molding time was 10min, the molding pressure was 10MPa, and then the pressure was maintained and cooled for 10min to obtain a degradable modified PS plastic bowl.

[0044] Comparative Example 1 The difference between this comparative example and Example 12 is that the flame-retardant polylactic acid is replaced by polylactic acid of the same mass.

[0045] Comparative Example 2 The difference between this comparative example and Example 12 is that the PS-trimellitic anhydride copolymer is replaced by PS of the same mass.

[0046] Comparative Example 3 The difference between this comparative example and Example 12 is that TAIC cross-linking is not used when preparing the flame-retardant polylactic acid.

[0047] Performance Test: 1. According to GB / T1040.2-2006, the degradable modified PS plastic bowl prepared in Examples 10-12 was prepared into dumbbell-shaped splines with a thickness of 3.2 mm. The test was performed at room temperature at a speed of 2 mm / min, and the tensile strength and elongation at break of the splines were recorded.

[0048] 2. The degradable modified PS plastic bowl prepared in Examples 10-12 was prepared into a 100×6.5×3.2 mm 3 According to ISO-4589 standard, the limiting oxygen index value of the specimens prepared in Examples 10-12 was evaluated using a JF-3 oxygen index meter.

[0049] 3. According to GB / T1633-2000, the Vicat softening temperature of the degradable modified PS plastic bowl prepared in Examples 10-12 was measured; wherein the load was 10N and the heating rate was 120°C / min.

[0050] 4. Cut the degradable modified PS plastic bowl prepared in Examples 10-12 into 1×1 cm 2 The sample pieces of different sizes were measured with an analytical balance in turn for their initial mass, recorded as N0; the sample pieces were then immersed in sterile simulated body fluids and simulated in vitro degradation in a biological incubator, with the degradation temperature set at 37°C and the degradation time set at 60 days. The sample pieces were then taken out and the SBF remaining on the surface of the sample pieces was wiped dry with absorbent paper. The sample pieces were weighed and recorded on an analytical balance, recorded as N1; the degradation rate of the sample pieces was expressed as the mass loss fraction of the sample pieces.

[0051] Degradation rate = (N0-N1 / N0) × 100% The test results are shown in Table 1: Table 1

[0052] Data Analysis: The degradable modified PS plastic bowls prepared in Examples 10-12 of the present invention all have excellent mechanical properties, as shown by excellent tensile strength values ​​and elongation at break values; the degradable modified PS plastic bowls prepared in Examples 10-12 of the present invention all have excellent flame retardant properties and fire resistance, as shown by high LOI and Vicat softening temperature values; in addition, the degradable modified PS plastic bowls prepared in Examples 10-12 of the present invention have good degradation properties, as shown by excellent degradation rates. However, since the polylactic acid in Comparative Example 1 was not flame-retardantly modified, the values ​​of LOI and Vicat softening temperature were reduced; the PS in Comparative Example 2 was not modified with trimellitic anhydride, the degradability was significantly reduced, and the mechanical properties were reduced; the flame-retardant polylactic acid in Comparative Example 3 was not cross-linked with TAIC, and the values ​​of tensile strength and elongation at break were reduced.

[0053] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0054] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0055] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a degradable modified PS plastic bowl, characterized in that: The preparation method comprises the following steps: According to weight parts, 10-20 parts of flame-retardant polylactic acid, 100 parts of PS-trimellitic anhydride copolymer and 5-10 parts of degradable polyurethane are added into a torque rheometer, melt-blended to obtain a blend; the blend is compression molded in a mold, and cooled under pressure to obtain a degradable modified PS plastic bowl; The method for preparing the flame retardant polylactic acid comprises the following steps: S1, hexachlorocyclotriphosphazene and ethanol are evenly mixed to obtain an ethanol solution of hexachlorocyclotriphosphazene; S2, anhydrous potassium carbonate and ethylenediamine are evenly mixed to obtain a mixed solid-liquid; an ethanol solution of hexachlorocyclotriphosphazene is added dropwise to the mixed solid-liquid at 5-10°C, and after the addition is completed, the temperature is raised to 20°C, and the reaction is continued for 2-3 hours to obtain a reaction liquid; the reaction liquid is heated to 80-90°C, the solvent is removed by reaction, and a solid is obtained; the solid is washed with deionized water and vacuum dried to obtain a solid intermediate A; S3, mixing TAIC and solid intermediate A, and then adding polylactic acid to blend to obtain a blend; adding the blend to a torque rheometer, blending at 190-200° C. for 5-10 minutes to obtain flame-retardant polylactic acid.

2. The method for preparing a degradable modified PS plastic bowl according to claim 1, characterized in that: In step S1, the usage ratio of hexachlorocyclotriphosphazene and ethanol is 35-45 g:200 mL; in step S2, the usage ratio of anhydrous potassium carbonate and ethylenediamine is 10 g:35-50 mL; in step S2, the vacuum drying temperature is 70-80° C. and the vacuum drying time is 30-60 min.

3. The method for preparing a degradable modified PS plastic bowl according to claim 1, characterized in that: In step S3, the usage ratio of TAIC, intermediate A and polylactic acid is 5-10g:30-40g:200-300g; the mixing speed is 100r / min, and the mixing time is 5min; the blending speed is 100r / min, and the blending time is 5-10min.

4. The method for preparing a degradable modified PS plastic bowl according to claim 1, characterized in that: The preparation method of PS-trimellitic anhydride copolymer comprises the following steps: PS, trimellitic anhydride and DMF are mixed evenly, and then an initiator BPO is added, and the temperature is raised to 120-140°C, and the reaction is carried out for 3 hours to obtain a mixed solid-liquid; the mixed solid-liquid is then heated to 155-160°C, and the DMF solvent is distilled off to obtain a solid; the solid is washed with deionized water and then vacuum dried to obtain a PS-trimellitic anhydride copolymer.

5. The method for preparing a degradable modified PS plastic bowl according to claim 4, characterized in that: The usage ratio of PS, trimellitic anhydride, DMF and initiator BPO is 8-10g:10-15g:100mL:0.3g; the vacuum drying temperature is 70-80°C, and the vacuum drying time is 30min.

6. The method for preparing a degradable modified PS plastic bowl according to claim 1, characterized in that: The degradable polyurethane is prepared by the following steps: A1. Mix sorbitol and polyol vegetable oil, raise the temperature to 80-100° C., then add toluene diisocyanate, stir to obtain a mixed solid-liquid; add a catalyst to the mixed solid-liquid, and react at a constant temperature of 80° C. for 3-5 hours to obtain a polymer; A2. Add 10-20 g of a small molecule chain extender to the polymer, stir at a constant temperature of 50-60° C. for 10-20 min to obtain a sample; cast the sample in a polytetrafluoroethylene mold, and cure at 70° C. for 5-7 days to obtain a degradable polyurethane.

7. The method for preparing a degradable modified PS plastic bowl according to claim 6, characterized in that: In step A1, the polyol vegetable oil is any one of castor oil, soybean oil or palm oil and a combination thereof, and the catalyst is dibutyltin dilaurate; the dosage ratio of sorbitol, polyol vegetable oil, toluene diisocyanate and catalyst is 18-25g:5-10mL:17g:0.3-0.5g; the stirring speed is 5-10min and the stirring time is 100r / min; in step A2, the small molecule chain extender is any one of ethylene glycol, 1,3-butanediol, 1,4-butanediol or 1,6-propylene glycol and a combination thereof.

8. The method for preparing a degradable modified PS plastic bowl according to claim 1, characterized in that: The temperature of melt blending is 180-200°C, the rotation speed is 50r / min, the melt blending time is 10-20min; the molding time is 8-10min, the molding pressure is 10MPa; the pressure holding cooling time is 10min.

9. A degradable modified PS plastic bowl, characterized in that: The degradable modified PS plastic bowl is prepared by the preparation method of a degradable modified PS plastic bowl according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Halogen-free flame retardant sheath material for nuclear cable, cable sheath, preparation method and application

    CN102875947A

  • Hyperbranched polyphosphazene flame retardant charring agent and preparing method thereof

    CN103992481A

  • Synthesis method for castoryl maleate-styrene copolymer

    CN106519097A

  • Halogen-free flame retardant irradiation-crosslinked cable material and preparation method thereof

    CN106554574A

  • Halogen-free flame-retardant cross-linking cable material and preparation method thereof

    CN107674328A