Adhesive tape integrated sectional material with high wind pressure resistance

By using materials such as modified carbon nanotubes and anti-UV agents in plastic steel profiles, a rubber-strip integrated profile with strong wind pressure resistance is formed, which solves the problem of insufficient wind pressure resistance and flame retardant performance of existing plastic steel profiles and achieves High strength, good sealing and environmental protection, suitable for high-rise building door and window applications.

CN118812974AInactive Publication Date: 2024-10-22ANHUI XIONGFENG BUILDING MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410757849.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing plastic steel profiles have deficiencies in wind pressure resistance and flame retardant performance, which results in performance degradation when faced with strong winds when used in high-rise building doors and windows. They also produce thick smoke and harmful gases when burned, affecting the air and human health.

Method used

By melting and blending polyvinyl chloride resin, modified carbon nanotubes, anti-UV agent, initiator and lubricant in a plastic co-extrusion machine, extrusion molding, and heating and injecting the sealing strip through a pinhole air gun to form an anti- A strip-integrated profile with strong wind pressure capability, modified carbon nanotubes are grafted with organic molecular chains through chemical bonds to improve interfacial compatibility and flame retardant properties.

Benefits of technology

It significantly improves the mechanical strength, flame retardant performance and UV resistance of the integrated profile, reduces the installation waste of the sealing strip, enhances the sealing and stability, and has good wind pressure resistance and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004890048150000031
    Figure BDA0004890048150000031
  • Figure BDA0004890048150000032
    Figure BDA0004890048150000032
  • Figure BDA0004890048150000041
    Figure BDA0004890048150000041
Patent Text Reader

Abstract

The invention discloses a rubber strip integrated sectional material with high wind pressure resistance, and belongs to the technical field of plastic steel sectional materials. Comprising the following raw materials in parts by weight: 80-100 parts of polyvinyl chloride resin, 15-25 parts of modified carbon nanotubes, 6-12 parts of an anti-ultraviolet agent, 0.1-0.3 part of an initiator and 4-6 parts of a lubricant. According to the manufactured rubber strip integrated sectional material, waste materials during installation are reduced, the sealing rubber strip is not prone to falling off, and the sealing performance and stability during installation and butt joint are enhanced; wherein the anti-ultraviolet agent can play a synergistic role, so that the anti-ultraviolet performance of the profile is greatly improved; by modifying the carbon nanotubes, the agglomeration phenomenon is relieved, the mechanical strength and flame retardant property of the profile are improved, and the performance is stable; therefore, the rubber strip of the rubber strip integrated profile is not prone to falling off, good in sealing performance and high in mechanical strength, has stable and efficient flame retardance, ultraviolet resistance and wind pressure resistance, and has important application value in the technical field of plastic steel profiles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of plastic-steel profiles, and in particular relates to a rubber strip integrated profile with strong wind pressure resistance. Background Art

[0002] The integrated profile with sealing strip is a profile design that integrates the sealing strip. The sealing strip and the profile are formed in one piece. This design can reduce assembly time and improve production efficiency. Because the strip and the profile are tightly combined, it can provide better sealing effect and overall aesthetics, and can also prevent air and moisture penetration. Due to its special properties, it is widely used in construction, furniture, machinery, automobiles, aviation and other fields.

[0003] At present, when integrated rubber strip profiles are used in the field of building doors and windows, especially high-rise buildings, they often face the invasion of strong winds. Therefore, the profiles need to have a certain ability to resist wind pressure, which has high requirements on the strength of the profiles. Therefore, plastic steel profiles are commonly used in current building doors and windows.

[0004] Plastic steel usually refers to a composite material that combines plastic with steel or other metal materials. This material combines the lightness, corrosion resistance, insulation of plastic with the high strength and durability of metal. The main component of plastic steel profiles is polyvinyl chloride (PVC), so it is also called PVC profiles. PVC has good flame retardancy and mechanical properties. It was once the world's largest general-purpose plastic. However, plastic steel profiles are often composite materials made of PVC resin as the main raw material and some additives. However, these additives have poor compatibility with PVC resin, which will cause the oxygen index and mechanical strength of PVC to decrease, reduce its wind pressure resistance and flame retardant properties, and make it difficult to quickly and completely self-extinguish during combustion. The combustion process is prone to produce thick smoke and harmful gases, which are harmful to the air and human health. Therefore, it is urgent to solve the above problems to meet the higher demands in the field of plastic steel profile technology. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a rubber strip integrated profile with strong wind pressure resistance.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A rubber strip integrated profile with strong wind pressure resistance is prepared by the following steps:

[0008] In a plastic co-extruder, polyvinyl chloride resin, modified carbon nanotubes, anti-ultraviolet agent, initiator and lubricant are melt-blended and extruded into a mold for forming. The molten sealing strip is then injected by heating with a pinhole air gun. After the injection is completed, the strip is cooled and formed, and demolded to obtain an integrated strip profile with strong wind pressure resistance.

[0009] Furthermore, the raw materials are calculated in parts by weight as follows: 80-100 parts of polyvinyl chloride resin, 15-25 parts of modified carbon nanotubes, 6-12 parts of anti-ultraviolet agent, 0.1-0.3 parts of initiator, and 4-6 parts of lubricant.

[0010] Furthermore, the anti-ultraviolet agent is prepared by compounding the light stabilizer WG-944 and the ultraviolet absorber UV-531 in a mass ratio of 2:1.

[0011] Furthermore, the initiator is one of benzoyl peroxide and lauroyl peroxide.

[0012] Furthermore, the lubricant is one of paraffin and stearamide fatty acid.

[0013] The integrated combination of plastic-steel profiles and sealing strips does not require the separate installation of sealing strips, which reduces the waste generated during the installation of sealing strips and is more environmentally friendly. The sealing strips are not easy to fall off after molding, which enhances the sealing and stability during installation and docking. In addition, the anti-ultraviolet agent is a hindered amine light stabilizer and a benzophenone ultraviolet absorber, which can play a synergistic role and greatly improve the anti-ultraviolet performance of the integrated profile.

[0014] Furthermore, the modified carbon nanotubes are prepared by the following steps:

[0015] S1. After dichloromethylphosphine, triethylamine and toluene were mixed and stirred evenly in a three-necked flask equipped with a stirring reflux device, 9-decenol was added dropwise. After the addition was completed, the temperature was slowly raised to 60° C. and refluxed for 4 hours. After the reaction was completed, triethylamine hydrochloride was filtered out and the solvent was removed by distillation under reduced pressure to obtain intermediate 1; the ratio of dichloromethylphosphine, triethylamine, toluene and 9-decenol was 14.5 g: 15 mL: 100 mL: 15.6 g;

[0016] Triethylamine is used as an acid binding agent to remove the hydrogen chloride generated by the reaction. Dichloromethylphosphine reacts with 9-decenol. By controlling the molar ratio of the two to be close to 1:1 and the dichloromethylphosphine to be slightly excessive, only one -Cl on the dichloromethylphosphine participates in the reaction to obtain intermediate 1. The specific reaction process is shown below:

[0017]

[0018] S2. At room temperature, in a three-necked flask equipped with a stirring device, melamine, intermediate 1, triethylamine and toluene were mixed and stirred uniformly under nitrogen protection, and the reaction temperature was controlled to be 65° C. for 6 hours. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by vacuum distillation. The mixture was purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 1:2), and the eluent was removed by rotary evaporation to obtain intermediate 2. The ratio of melamine, intermediate 1, triethylamine and toluene was 13.4 g:50.4 g:30 mL:100 mL.

[0019] Melamine and intermediate 1 undergo nucleophilic substitution. By controlling the molar ratio of the two to be close to 1:2 and a slight excess of melamine, two amino groups on melamine participate in the reaction. Triethylamine removes the hydrogen chloride generated by the reaction to obtain intermediate 2. The specific reaction process is as follows:

[0020]

[0021] S3. In a three-necked flask equipped with a stirring device, the carboxylated carbon nanotubes and N,N-dimethylformamide (DMF) were mixed and magnetically stirred for 2 hours. After uniform dispersion, the intermediate 2, dicyclohexylcarbodiimide (DCC, dehydrating agent) and 4-dimethylaminopyridine (DMAP, catalyst) were added in sequence. After uniform stirring, the mixture was placed in a 55°C water bath for 4 hours for ultrasonic treatment. The water bath was then removed and magnetically stirred at room temperature for 8 hours. After the reaction was completed, the mixture was filtered and washed with anhydrous ethanol for 3-4 times, dried and ground to obtain modified carbon nanotubes. The ratio of the amount of carboxylated carbon nanotubes, N,N-dimethylformamide, intermediate 2, dicyclohexylcarbodiimide and 4-dimethylaminopyridine was 5g:100mL:12g:14.5g:0.2g.

[0022] Under the action of DCC and DMAP, -COOH on the surface of the carboxylated carbon nanotubes undergoes an amidation reaction with -NH2 on the intermediate 2, and organic molecules are grafted on the surface of the carbon nanotubes to obtain modified carbon nanotubes. The specific reaction process is as follows:

[0023]

[0024] As a reinforcing material, carbon nanotubes are grafted with organic molecular chains through chemical bonding, that is, an organic layer is formed on its surface, which can greatly improve the interfacial compatibility between carbon nanotubes and PVC matrix, thereby promoting the uniform dispersion of modified carbon nanotubes in the matrix, reducing the agglomeration of carbon nanotubes, and greatly enhancing the mechanical strength of the matrix; in addition, carbon nanotubes are inorganic fillers, and organic molecular chains are dispersed in the matrix by grafting on their surface, which is difficult to seep out and migrate, ensuring the durability of various properties; not only that, the grafted organic molecules also contain PN flame retardant components, triazine structures, long carbon chain structures and carbon-carbon double bonds; among them, PN The flame retardant component has the synergistic flame retardant effect of phosphorus and nitrogen flame retardants, which can give the coating safe and efficient flame retardant properties; the introduced triazine structure will produce nitrogen-containing gas during combustion, dilute and reduce the smoke density, and self-condense at high temperature to form melem to make the carbon layer tight, further improving the flame retardant and smoke suppression properties of the matrix; the introduced long carbon chain is a flexible chain segment, which can improve the mechanical properties of the matrix to a certain extent, and can be interspersed in the molecular chain of the matrix to improve stability; finally, the unsaturated carbon-carbon double bond at the end can produce chemical bonding with the PVC matrix, further enhancing the interaction between the modified carbon nanotubes and the matrix, thereby improving various performances.

[0025] Furthermore, the carboxylated carbon nanotubes are prepared by the following steps:

[0026] The carbon nanotubes are placed in a conical flask, and then mixed acid is added, and ultrasonic treatment is performed in a water bath at 50°C for 8 hours. After the mixture is cooled to room temperature, deionized water is added for dilution, centrifugation is performed, and the mixture is washed with anhydrous ethanol and deionized water for 4-5 times in sequence, dried, and ground to obtain carboxylated carbon nanotubes; the mixed acid is a mixture of concentrated sulfuric acid with a mass fraction of 98% and concentrated hydrochloric acid with a mass fraction of 37.2% in a volume ratio of 4:1; the ratio of the amount of carbon nanotubes to the mixed acid is 1g:100mL;

[0027] By subjecting carbon nanotubes to ultrasonic shearing and oxidation treatment with strong acid, a certain number of carboxyl active groups can be introduced into the side walls and tops of the carbon nanotubes, thus laying the foundation for reaction sites for subsequent chemical reactions.

[0028] Beneficial effects of the present invention:

[0029] 1. The integrated rubber strip profile prepared by the present invention reduces waste generated during the installation of the sealing strip, is more environmentally friendly, and the sealing strip is not easy to fall off, thereby enhancing the sealing and stability during installation and docking;

[0030] 2. The anti-ultraviolet agent is a hindered amine light stabilizer and a benzophenone ultraviolet absorber, which can play a synergistic role and greatly improve the anti-ultraviolet performance of the one-piece profile;

[0031] 3. By modifying carbon nanotubes, compared with ordinary carbon nanotubes, they have better compatibility with PVC, reduce agglomeration, and can significantly improve the mechanical strength and flame retardant properties of the rubber strip integrated profile, and have stable performance;

[0032] Therefore, the integrated rubber strip profile produced by the present invention is not easy to fall off, has good sealing performance, high mechanical strength, and has stable and efficient flame retardancy, UV resistance and wind pressure resistance, and has important application value in the field of plastic-steel profile technology. DETAILED DESCRIPTION

[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Example 1

[0035] Preparation of carboxylated carbon nanotubes:

[0036] 20 g of carbon nanotubes were placed in a conical flask, and then 2000 mL of concentrated sulfuric acid (mass fraction 98%) and concentrated hydrochloric acid (mass fraction 37.2%) were added in a volume ratio of 4:1 to obtain a mixed acid, and the mixture was ultrasonically treated in a 50°C water bath for 8 h. After the mixture was cooled to room temperature, deionized water was added to dilute it, centrifuged, and washed with anhydrous ethanol and deionized water for 4 times in sequence, dried, and ground to obtain carboxylated carbon nanotubes.

[0037] Example 2

[0038] Preparation of modified carbon nanotubes:

[0039] S1. In a three-necked flask equipped with a stirring reflux device, 14.5 g of dichloromethylphosphine, 15 mL of triethylamine and 100 mL of toluene were mixed and stirred uniformly, and then 15.6 g of 9-decenol was added dropwise. After the addition was completed, the temperature was slowly raised to 60° C. and refluxed for 4 hours. After the reaction was completed, triethylamine hydrochloride was removed by filtration, and the solvent was removed by distillation under reduced pressure to obtain intermediate 1;

[0040] S2. At room temperature and under nitrogen protection, 13.4 g of melamine, 50.4 g of intermediate 1, 30 mL of triethylamine and 100 mL of toluene were mixed and stirred evenly in a three-necked flask equipped with a stirring device. The reaction temperature was controlled to be kept at 65° C. for 6 h. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by distillation under reduced pressure. The mixture was then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 1:2), and the eluent was removed by rotary evaporation to obtain intermediate 2.

[0041] S3. In a three-necked flask equipped with a stirring device, 5 g of the carboxylated carbon nanotubes prepared in Example 1 were mixed with 100 mL of N,N-dimethylformamide and magnetically stirred for 2 h. After uniform dispersion, 12 g of intermediate 2, 14.5 g of dicyclohexylcarbodiimide and 0.2 g of 4-dimethylaminopyridine were added in sequence. After uniform stirring, the mixture was placed in a 55°C water bath for ultrasonic treatment for 4 h. The water bath was then removed and magnetically stirred for 8 h at room temperature. After the reaction was completed, the mixture was filtered, washed with anhydrous ethanol for 3 times, dried and ground to obtain modified carbon nanotubes.

[0042] Example 3

[0043] Preparation of modified carbon nanotubes:

[0044] S1. In a three-necked flask equipped with a stirring reflux device, 29.0 g of dichloromethylphosphine, 30 mL of triethylamine and 200 mL of toluene were mixed and stirred uniformly, and then 31.2 g of 9-decenol was added dropwise. After the addition was completed, the temperature was slowly raised to 60° C. and refluxed for 4 hours. After the reaction was completed, triethylamine hydrochloride was removed by filtration, and the solvent was removed by distillation under reduced pressure to obtain intermediate 1;

[0045] S2. At room temperature and under nitrogen protection, 26.8 g of melamine, 100.8 g of intermediate 1, 60 mL of triethylamine and 200 mL of toluene were mixed and stirred evenly in a three-necked flask equipped with a stirring device. The reaction temperature was controlled to be kept at 65° C. for 6 h. After the reaction was completed, the mixture was filtered, and part of the solvent was removed by distillation under reduced pressure. The mixture was then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 1:2), and the eluent was removed by rotary evaporation to obtain intermediate 2.

[0046] S3. In a three-necked flask equipped with a stirring device, 10 g of the carboxylated carbon nanotubes prepared in Example 1 was mixed with 200 mL of N,N-dimethylformamide and magnetically stirred for 2 h. After uniform dispersion, 24 g of intermediate 2, 29 g of dicyclohexylcarbodiimide and 0.4 g of 4-dimethylaminopyridine were added in sequence. After uniform stirring, the mixture was placed in a 55°C water bath for ultrasonic treatment for 4 h. The water bath was then removed and magnetically stirred for 8 h at room temperature. After the reaction was completed, the mixture was filtered and washed with anhydrous ethanol for 3 times. The mixture was dried and ground to obtain modified carbon nanotubes.

[0047] Example 4

[0048] In a plastic co-extruder, 80 g of polyvinyl chloride resin, 15 g of the modified carbon nanotubes prepared in Example 2, 6 g of an anti-ultraviolet agent (prepared by compounding 4 g of a light stabilizer WG-944 and 2 g of an ultraviolet absorber UV-531), 0.1 g of benzoyl peroxide and 4 g of paraffin were melt-blended and extruded to obtain a test sample.

[0049] Example 5

[0050] In a plastic co-extruder, 90 g of polyvinyl chloride resin, 20 g of the modified carbon nanotubes prepared in Example 3, 9 g of an anti-ultraviolet agent (prepared by compounding 6 g of a light stabilizer WG-944 and 3 g of an ultraviolet absorber UV-531), 0.2 g of lauroyl peroxide and 5 g of stearamide fatty acid were melt-blended and extruded to obtain a test sample.

[0051] Example 6

[0052] In a plastic co-extruder, 100 g of polyvinyl chloride resin, 25 g of the modified carbon nanotubes prepared in Example 3, 12 g of an anti-ultraviolet agent (8 g of a light stabilizer WG-944 and 4 g of an ultraviolet absorber UV-531), 0.3 g of lauroyl peroxide and 6 g of stearamide fatty acid were melt-blended and extruded to obtain a test sample.

[0053] Example 7

[0054] Preparation of integrated rubber strip profiles with strong wind pressure resistance:

[0055] In a plastic co-extruder, 100 g of polyvinyl chloride resin, 25 g of modified carbon nanotubes prepared in Example 3, 12 g of an anti-ultraviolet agent (8 g of a light stabilizer WG-944 and 4 g of an ultraviolet absorber UV-531), 0.3 g of lauroyl peroxide and 6 g of stearamide fatty acid are melt-blended and extruded into a mold for forming. A molten sealing strip (commercially available, 3M polyurethane sealant 590) is then injected by heating with a pinhole air gun. After the injection is completed, the strip is cooled and formed, and demolded to obtain a one-piece strip profile with strong wind pressure resistance.

[0056] Comparative Example 1

[0057] Ordinary carbon nanotubes of the same mass were used to replace the modified carbon nanotubes in Example 6, and the remaining steps were the same as those in Example 6.

[0058] Comparative Example 2

[0059] Use commercially available flame-retardant polyvinyl chloride environmentally friendly plastic steel plastic material produced by Xingtai Hengxiang Rubber and Plastic Products Co., Ltd.

[0060] The samples of Examples 4-6 and Comparative Examples 1-2 were made into corresponding shapes according to different test standards and subjected to the following performance tests:

[0061] The national standard GB / T 2406-2008 "Test method for combustion performance of plastics" is used to determine the limiting oxygen index;

[0062] The smoke density is measured using the national standard GB / T 8323.2-2008 "Plastic smoke generation Part 2: Single chamber method for determination of smoke density test method";

[0063] The impact resistance is determined using the national standard GB / T 1043.1-2008 "Determination of impact properties of simply supported plastic beams Part 1: Non-instrumented impact test";

[0064] The bending properties are measured using the national standard GB / T 9341-2008 "Determination of bending properties of plastics";

[0065] According to the national standard GB / T 16422.2-1999 "Plastics Laboratory Light Source Exposure Test Method Part 2: Xenon Arc Lamp", the sample was placed in a xenon lamp aging test chamber for accelerated aging for 480 hours. The aging conditions were air atmosphere, xenon lamp wavelength 280-800nm, and irradiation intensity 550W / m 2 , test the tensile strength of the specimens before and after aging (GB / T 1040-2006);

[0066] The measured results are shown in the following table:

[0067]

[0068] It can be seen from the above table that the profiles prepared in the embodiments of the present invention have higher flame retardancy and smoke suppression properties than the control examples, and have excellent anti-ultraviolet properties. Their outstanding mechanical strength can give the profiles significant wind pressure resistance; therefore, the prepared profiles have important application value in the field of plastic-steel profile technology.

[0069] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0070] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A one-piece rubber strip profile with strong wind pressure resistance. It is characterized in that Prepared by the following steps: The polyvinyl chloride resin, modified carbon nanotubes, anti-ultraviolet agent, initiator and lubricant are melt-blended and extruded into a mold to form, and then the molten sealing strip is injected. After the injection is completed, the strip is cooled and molded, and demolded to obtain a strip integrated profile with strong wind pressure resistance; Wherein, the modified carbon nanotubes are prepared by the following steps: S1. Mix dichloromethylphosphine, triethylamine and toluene and stir evenly, add 9-decenol dropwise, and reflux at 60° C. for 4 h. After the reaction is complete, filter and distill under reduced pressure to obtain intermediate 1. S2, at room temperature, under nitrogen protection, melamine, intermediate 1, triethylamine and toluene were mixed and stirred evenly, reacted at 65°C for 6 hours, and after the reaction was completed, filtered, distilled under reduced pressure, purified by column chromatography, and rotary evaporated to obtain intermediate 2; S3. Mix the carboxylated carbon nanotubes with N,N-dimethylformamide and stir for 2 hours. After uniform dispersion, add intermediate 2, dicyclohexylcarbodiimide and 4-dimethylaminopyridine. After uniform stirring, ultrasonicate at 55°C for 4 hours. Remove the water bath and stir at room temperature for 8 hours. After the reaction is completed, filter, wash, dry and grind to obtain modified carbon nanotubes.

2. According to claim 1, a rubber strip integrated profile with strong wind pressure resistance, It is characterized in that In step S1, the ratio of the amount of dichloromethylphosphine, triethylamine, toluene and 9-decenol is 14.5 g: 15 mL: 100 mL: 15.6 g.

3. According to claim 1, a rubber strip integrated profile with strong wind pressure resistance, It is characterized in that In step S2, the ratio of melamine, intermediate 1, triethylamine and toluene is 13.4 g:50.4 g:30 mL:100 mL.

4. The one-piece rubber strip profile with strong wind pressure resistance according to claim 1, It is characterized in that In step S3, the ratio of the amount of carboxylated carbon nanotubes, N,N-dimethylformamide, intermediate 2, dicyclohexylcarbodiimide, and 4-dimethylaminopyridine is 5 g:100 mL:12 g:14.5 g:0.2 g.

5. The one-piece rubber strip profile with strong wind pressure resistance according to claim 1, It is characterized in that The raw materials are calculated in parts by weight as follows: 80-100 parts of polyvinyl chloride resin, 15-25 parts of modified carbon nanotubes, 6-12 parts of anti-ultraviolet agent, 0.1-0.3 parts of initiator, and 4-6 parts of lubricant.

6. The one-piece rubber strip profile with strong wind pressure resistance according to claim 1, It is characterized in that The anti-ultraviolet agent is prepared by compounding a light stabilizer WG-944 and an ultraviolet absorber UV-531 in a mass ratio of 2:

1.

7. The one-piece rubber strip profile with strong wind pressure resistance according to claim 1, It is characterized in that The initiator is one of benzoyl peroxide and lauroyl peroxide.

8. The integrated rubber strip profile with strong wind pressure resistance according to claim 1, It is characterized in that The lubricant is one of paraffin and stearamide fatty acid.

Citation Information

Cited By

  • Preparation process of high-thermal-conductivity polyimide film

    CN119912719A