Polyurethane fireproof thermal insulation board and preparation and recovery method thereof

By combining polyurethane recycled materials with polymer composite fireproof materials, polyurethane fireproof insulation boards are prepared, and full life cycle recycling is achieved through special-shaped extruders and thermal transfer wood grain processes, which solves the problem of difficult recycling of polyurethane materials and realizes Efficient carbon emission reduction and environmentally friendly product development.

CN118813033APending Publication Date: 2024-10-22GUANGDONG JUWEI NEW MATERIALS R&D CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411015314.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing polyurethane fireproof materials are difficult to recycle and reuse after use. The treatment process is complex and harmful to the environment. Moreover, its materials are difficult to decompose under natural conditions, leading to carbon emission problems.

Method used

Polyurethane recycled materials are combined with polymer composite fireproof materials, and polyurethane fireproof insulation boards are prepared through equipment such as autoclaves, tower reactors, kneaders, and foaming machines, and through special-shaped extruders and thermal transfer wood grain processes. Realize the recycling and reuse of boards to form products with full life cycle carbon emissions.

Benefits of technology

It realizes the full life cycle recycling of polyurethane fireproof insulation boards, reduces carbon emissions and avoids environmental pollution. The products have high durability, good insulation and waterproof effects, and are suitable for different climate environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118813033A_ABST
    Figure CN118813033A_ABST
Patent Text Reader

Abstract

The invention belongs to a fireproof thermal insulation material, and particularly relates to a polyurethane fireproof thermal insulation board and a preparation and recovery method thereof, the polyurethane fireproof thermal insulation board comprises the following raw materials by weight: 65-75 parts of a polyurethane reclaimed material, and 25-35 parts of a high-molecular polymer composite fireproof material; the high-molecular polymer composite fireproof material is prepared from the following raw materials in parts by weight: 50 to 70 parts of polystyrene, 15 to 30 parts of phosphate ester polymer, 10 to 15 parts of polycarbonate and 10 to 20 parts of polypropylene. The fireproof thermal insulation board is made of polyurethane recycled materials, the board is made of 100% high-molecular polymers, the board can be recycled to become raw materials after being used, the board is high in strength and good in fireproof thermal insulation effect, leftover materials can be recycled, regenerated and manufactured, and the purpose of carbon emission in the whole life cycle can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to fireproof and heat-insulating materials, and in particular relates to a polyurethane fireproof and heat-insulating board and a preparation and recycling method thereof. Background Art

[0002] The previous government has more and more policies on the recycling economy of waste plastics. Taking the use of polyurethane as an example, this high molecular polymer material is widely used in industrial fields such as adhesives, coatings, low-speed tires, gaskets, and car mats. In the field of daily life, polyurethane is used to make various foams and plastic sponges. Because polyurethane has a very low thermal conductivity, new wall insulation plastic wood panels based on its material have begun to gradually develop and mature in Western countries such as Europe and the United States. Polyurethane materials are extremely difficult to decompose under natural conditions. The widely used treatment method now is combustion. The gas after combustion passes through water to dissolve easily soluble toxic substances such as NO2. In the combustion process, hydrogen cyanide is also generated. Hydrogen cyanide is easily soluble in water, and the CN-root produced is highly toxic, so the water passing through the combustion exhaust gas must be specially treated. If polyurethane is buried deep underground, it will take decades to decompose. Another recycling method is cracking, which is cracked into some small molecular chemicals under high temperature and other conditions, which can be used to produce useful materials such as fuel.

[0003] There are related polyurethane fireproof patents on the market, such as "A flame-retardant low-smoke toxicity polyurethane foam material and its preparation method", publication number CN202410268211.7, application date March 2024. This patent mainly describes the method of making raw materials. After the production of this product, due to raw material problems, it cannot be recycled and reused, and the treatment is even more troublesome. Summary of the invention

[0004] The purpose of the present invention is to provide a polyurethane fireproof and thermal insulation board and a preparation and recycling method thereof. The fireproof and thermal insulation board is made of polyurethane recycled materials. The board is made of 100% high molecular polymer and can be recycled into raw materials after use. The board has high strength and good fireproof and thermal insulation effects. The scraps can be recycled and regenerated, which can achieve the purpose of carbon emissions throughout the life cycle.

[0005] In order to solve the above problems, the present invention relates to a polyurethane fireproof insulation board and a preparation and recycling method thereof, comprising the following raw materials in parts by weight: 65-75 parts of polyurethane recycled materials and 25-35 parts of high molecular polymer composite fireproof materials; the high molecular polymer composite fireproof materials comprise the following raw materials in parts by weight: 50-70 parts of polystyrene, 15-30 parts of phosphate polymers, 10-15 parts of polycarbonate, and 10-20 parts of polypropylene.

[0006] Preferably, the raw materials include the following parts by weight: 70 parts of polyurethane recycled materials and 30 parts of high molecular polymer composite fireproof materials; the high molecular polymer composite fireproof materials include the following raw materials in weight: 60 parts of polystyrene, 20 parts of phosphate polymer, 12 parts of polycarbonate and 15 parts of polypropylene.

[0007] A method for preparing a polyurethane fireproof thermal insulation board comprises the following steps: (1) Weigh the raw materials Weigh the raw materials according to the following weight proportions: 65-75 parts of polyurethane recycled material, 50-70 parts of polystyrene, 15-30 parts of phosphate polymer, 10-15 parts of polycarbonate, and 10-20 parts of polypropylene; (2) Preparation method of polymer composite fireproof material The polystyrene, phosphate polymer, polycarbonate and polypropylene weighed in step (1) are put into a hot autoclave for reaction. All materials are reacted in the hot autoclave at a temperature of 180-210° C. for 2-3 min. The materials after the reaction enter a tower reactor at a temperature of 160-180° C. for 5-10 min. After cooling to room temperature, the materials enter a kneading machine for kneading at a temperature of 120-165° C. for 35 min. The kneaded materials are then passed through a granulator to form small granules of a polymer composite fireproof material; (3) Preparation method of polyurethane fireproof insulation board The polyurethane recycled material weighed in step (1) and the high molecular polymer composite fireproof material obtained in step (2) are added into a stirring device for high-temperature liquefaction and mixing at a mixing temperature of 160-200° C. and stirred for 30 minutes to obtain a material mixture A; The mixture A is sent to the polyurethane foaming machine through a pressure pipeline. The foaming machine is equipped with a movable mold. The mixture A is sprayed and poured into the mold for foaming and shaping. A set of polyurethane foaming machines can be equipped with 10 to 15 sets of movable molds. The mold needs to be foamed for about 15 to 30 minutes after pouring. After the foaming is matured, demoulding is performed. Manual or automatic equipment can be used for demoulding. After demoulding, material B is obtained; Material B is a long block and needs to be cut into sheets by PU sheet production equipment. After cutting, sheet C is obtained. After passing the inspection, the wood grain is thermally transferred and the sheet is packaged and shipped to obtain the finished polyurethane fireproof insulation sheet.

[0008] A method for recycling polyurethane fireproof and thermal insulation boards comprises the following steps: (1) Crushing of recycled materials The scraps produced during the cutting process of the polyurethane fireproof insulation board or the polyurethane fireproof insulation board that fails the inspection are recycled materials, and the recycled materials are crushed into tiny particles by a crusher as material E; (2) Preparation method of polymer composite elastomer Weigh the raw materials according to the following weight proportions: 60-80 parts of polystyrene, 10-15 parts of polypropylene, and 20-30 parts of polyethylene, put the weighed materials into a hot autoclave for reaction at a reaction temperature of 180-210 degrees for 2-3 minutes, and the reacted materials enter a tower reactor at a reaction temperature of 160-180 degrees for 5-10 minutes, and then cool to room temperature and enter a kneading machine for kneading at a kneading temperature of 120-165 degrees for 3-5 minutes. The kneaded materials are then passed through a granulator to be made into small granular polymer composite fireproof materials; (3) Recycled material recycling method The material E obtained in step (1) and the high molecular polymer composite elastomer obtained in step (2) are mixed, and kneaded by a special-shaped extruder to obtain material F. The special-shaped extruder uses a single screw or a twin screw to extrude the material F onto a fixed heating mold for closed molding. The heating mold temperature is about 200°C. After plasticization, the material G is obtained by a cooling and molding process. The cooling and molding uses a two-pass cooling water tank at 60-90°C and a circulating water cooling system. After cooling and molding, the material G enters a heat transfer embossing device for heat transfer embossing. The heat transfer embossing temperature is 60°C. The material is quickly embossed to become a plastic wood product. The scraps generated during the production of the plastic wood product are transported to a crusher for crushing.

[0009] The key points of the present invention are as follows: 1. The polyurethane material is used to produce a full life cycle fireproof insulation board. The board can be recycled after use and then made into a plastic wood product through a special-shaped extrusion process. After use, the plastic wood can also be recycled as a raw material and can be recycled and reused. The full life cycle fireproof insulation material can completely replace the insulation foam board. It is not afraid of pressure or fire, and can be recycled and reused, achieving a true full life cycle carbon emission product, which is a better product for the circular economy.

[0010] 2. The key point of the present invention is to use a high temperature 160 to 200 degrees liquefaction stirring and mixing process. This process generates a full life cycle fireproof and thermal insulation material through foaming. Because the high molecular polymer composite fireproof material is evenly mixed, after being cut by the board production equipment, the cut surface is still fireproof. Even if it is made into a full life cycle fireproof and thermal insulation board through thermal transfer wood grain equipment, it can still be fireproof. This is the biggest difference from other polyurethane fireproof products that are only made of materials that are fireproof on the surface, and the cut surface cannot be fireproof.

[0011] Compared with the prior art, the technical advantage of the present invention is that the use of polyurethane waste plastics can achieve the use of carbon emissions throughout the life cycle, which can quickly solve the problem of polyurethane recycling being unable to be processed, and has the following advantages: 1. The present invention is a green process: the present invention does not require the use of harmful chemical components, does not cause air pollution or water pollution, and does not cause pollution to the human body or the environment.

[0012] 2. Energy saving and emission reduction: The energy consumption of manufacturing the product of the present invention is much lower than that of foam processing. At the same time, due to its long life, it can effectively maintain heat, thus achieving carbon reduction and energy saving.

[0013] 3. The product of the present invention adopts high molecular polymer material, which makes it more durable and not easy to break, rot, deform, etc. Compared with foam, it has a longer service life and does not need to be replaced frequently, which can effectively reduce maintenance costs.

[0014] 4. The product of the present invention is made of all plastic material, which has good heat preservation and waterproof effect. It will not be deformed by squeezing or sun exposure, and can be used for a long time in different climate environments, especially in outdoor environments.

[0015] 5. Since the surface layer of the product of the present invention is made of composite plastic material, it is easier to clean and maintain than foam material. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a process flow chart of an embodiment. DETAILED DESCRIPTION

[0017] In order to make the technical purpose, technical solution and beneficial effects of the present invention clearer, the technical solution of the present invention is further described below in conjunction with specific embodiments.

[0018] Example 1: A polyurethane fireproof insulation board comprises the following raw materials in parts by weight: 65 parts of polyurethane recycled materials and 25 parts of high molecular polymer composite fireproof materials; the high molecular polymer composite fireproof materials comprise the following raw materials in parts by weight: 50 parts of polystyrene, 15 parts of phosphate polymer, 10 parts of polycarbonate and 10 parts of polypropylene.

[0019] A method for preparing a polyurethane fireproof thermal insulation board comprises the following steps: (1) Weigh the raw materials Weigh the following raw materials by weight: 65 parts of polyurethane recycled material, 50 parts of polystyrene, 15 parts of phosphate polymer, 10 parts of polycarbonate, and 10 parts of polypropylene; (2) Preparation method of polymer composite fireproof material The polystyrene, phosphate polymer, polycarbonate and polypropylene weighed in step (1) are put into a hot autoclave for reaction. All materials are reacted in the hot autoclave at a temperature of 180° C. for 2 minutes. The reacted materials are put into a tower reactor at a temperature of 160° C. for 5 minutes. After cooling to room temperature, the materials are put into a kneading machine for kneading at a temperature of 120° C. for 35 minutes. The kneaded materials are then put into a granulator to be made into small granular polymer composite fireproof materials; (3) Preparation method of polyurethane fireproof insulation board The polyurethane recycled material weighed in step (1) and the high molecular polymer composite fireproof material obtained in step (2) are added into a stirring device for high-temperature liquefaction and mixing at a mixing temperature of 160° C. and stirred for 30 minutes to obtain a material mixture A; The mixture A is sent to the polyurethane foaming machine through a pressure pipeline. The foaming machine is equipped with a movable mold. The mixture A is sprayed and poured into the mold for foaming and shaping. A set of polyurethane foaming machines can be equipped with 10 sets of movable molds. The molds must be foamed for about 15 minutes after pouring. After the foaming and ripening, demoulding is performed. Manual or automatic equipment can be used for demoulding. After demoulding, material B is obtained; Material B is a long block and needs to be cut into sheets by PU sheet production equipment. After cutting, sheet C is obtained. After passing the inspection, the wood grain is thermally transferred and the sheet is packaged and shipped to obtain the finished polyurethane fireproof insulation sheet.

[0020] A method for recycling polyurethane fireproof and thermal insulation boards comprises the following steps: (1) Crushing of recycled materials The scraps produced during the cutting process of the polyurethane fireproof insulation board or the polyurethane fireproof insulation board that fails the inspection are recycled materials, and the recycled materials are crushed into tiny particles by a crusher as material E; (2) Preparation method of polymer composite elastomer Weigh the raw materials according to the following weight proportions: 60 parts of polystyrene, 10 parts of polypropylene, and 20 parts of polyethylene, put the weighed materials into a hot autoclave for reaction at a reaction temperature of 180 degrees for 2 minutes, and the reacted materials enter a tower reactor at a reaction temperature of 160 degrees for 5 minutes, and then cool to room temperature and enter a kneading machine for kneading at a kneading temperature of 120 degrees for 3-5 minutes. The kneaded materials are then passed through a granulator to be made into small granular polymer composite fireproof materials; (3) Recycled material recycling method The material E obtained in step (1) and the high molecular polymer composite elastomer obtained in step (2) are mixed, and kneaded by a special-shaped extruder to obtain material F. The special-shaped extruder uses a single screw or a twin screw to extrude the material F onto a fixed heating mold for closed molding. The heating mold temperature is about 200°C. After plasticization, the material G is obtained by a cooling and molding process. A 60°C two-pass cooling water tank is used for cooling and molding, and a circulating water cooling system is used. After cooling and molding, the material G enters a heat transfer embossing device for heat transfer embossing. The heat transfer embossing temperature is 60°C. The material is quickly embossed to become a plastic wood product. The scraps generated during the production of the plastic wood product are transported to a crusher for crushing.

[0021] Example 2: A polyurethane fireproof thermal insulation board comprises the following raw materials in parts by weight: 75 parts of polyurethane recycled materials and 35 parts of high molecular polymer composite fireproof materials; the high molecular polymer composite fireproof materials comprise the following raw materials in parts by weight: 70 parts of polystyrene, 30 parts of phosphate polymers, 15 parts of polycarbonate, and 20 parts of polypropylene.

[0022] A method for preparing a polyurethane fireproof thermal insulation board comprises the following steps: (1) Weigh the raw materials Weigh the raw materials according to the following weight proportions: 75 parts of polyurethane recycled material, 70 parts of polystyrene, 30 parts of phosphate polymer, 15 parts of polycarbonate, and 20 parts of polypropylene; (2) Preparation method of polymer composite fireproof material The polystyrene, phosphate polymer, polycarbonate and polypropylene weighed in step (1) are put into a hot autoclave for reaction. All materials are reacted in the hot autoclave at a temperature of 210° C. for 3 minutes. The reacted materials are put into a tower reactor at a temperature of 180° C. for 10 minutes. After cooling to room temperature, the materials are put into a kneading machine for kneading at a temperature of 165° C. for 35 minutes. The kneaded materials are then put into a granulator to be made into small granular polymer composite fireproof materials; (3) Preparation method of polyurethane fireproof insulation board The polyurethane recycled material weighed in step (1) and the high molecular polymer composite fireproof material obtained in step (2) are added into a stirring device for high-temperature liquefaction and mixing at a mixing temperature of 200° C. and stirred for 30 minutes to obtain a material mixture A; The mixture A is sent to the polyurethane foaming machine through a pressure pipeline. The foaming machine is equipped with a movable mold. The mixture A is sprayed and poured into the mold for foaming and shaping. A set of polyurethane foaming machines can be equipped with 15 sets of movable molds. The mold needs to be foamed for about 30 minutes after pouring. After the foaming and ripening, demoulding is performed. The demoulding process can be performed manually or by automatic equipment. After demoulding, material B is obtained; Material B is a long block and needs to be cut into sheets by PU sheet production equipment. After cutting, sheet C is obtained. After passing the inspection, the wood grain is thermally transferred and the sheet is packaged and shipped to obtain the finished polyurethane fireproof insulation sheet.

[0023] A method for recycling polyurethane fireproof and thermal insulation boards comprises the following steps: (1) Crushing of recycled materials The scraps produced during the cutting process of the polyurethane fireproof insulation board or the polyurethane fireproof insulation board that fails the inspection are recycled materials, and the recycled materials are crushed into tiny particles by a crusher as material E; (2) Preparation method of polymer composite elastomer Weigh the raw materials according to the following weight proportions: 80 parts of polystyrene, 15 parts of polypropylene, and 30 parts of polyethylene. Put the weighed materials into a hot autoclave for reaction at a reaction temperature of 210 degrees for 3 minutes. The reacted materials enter a tower reactor at a reaction temperature of 180 degrees for 10 minutes, and then cool to room temperature before entering a kneading machine for kneading at a kneading temperature of 165 degrees for 5 minutes. The kneaded materials are then passed through a granulator to form a small granular polymer composite fireproof material. (3) Recycling methods of recycled materials The material E obtained in step (1) and the high molecular polymer composite elastomer obtained in step (2) are mixed, and kneaded by a special-shaped extruder to obtain material F. The special-shaped extruder uses a single screw or a twin screw to extrude material F onto a fixed heating mold for closed molding. The heating mold temperature is about 200°C. After plasticization, the material G is obtained by a cooling and molding process. A 90°C two-pass cooling water tank is used for cooling and molding, and a circulating water cooling system is used. After cooling and molding, the material G enters a heat transfer embossing device for heat transfer embossing. The heat transfer embossing temperature is 60°C. The material is quickly embossed to become a plastic wood product. The scraps generated during the production of the plastic wood product are transported to a crusher for crushing.

[0024] Example 3: A polyurethane fireproof insulation board: comprising the following raw materials in parts by weight: 65 parts of polyurethane recycled materials and 35 parts of high molecular polymer composite fireproof materials; the high molecular polymer composite fireproof materials comprise the following raw materials in parts by weight: 50 parts of polystyrene, 30 parts of phosphate polymers, 10 parts of polycarbonate and 20 parts of polypropylene.

[0025] A method for preparing a polyurethane fireproof thermal insulation board comprises the following steps: (1) Weigh the raw materials Weigh the following raw materials according to the following weight proportions: 65 parts of polyurethane recycled material, 50 parts of polystyrene, 30 parts of phosphate polymer, 10 parts of polycarbonate, and 20 parts of polypropylene; (2) Preparation method of polymer composite fireproof material The polystyrene, phosphate polymer, polycarbonate and polypropylene weighed in step (1) are put into a hot autoclave for reaction. All materials are reacted in the hot autoclave at a temperature of 180° C. for 3 minutes. The reacted materials are put into a tower reactor at a temperature of 160° C. for 10 minutes. After cooling to room temperature, the materials are put into a kneading machine for kneading at a temperature of 120° C. for 35 minutes. The kneaded materials are then put into a granulator to be made into small granular polymer composite fireproof materials; (3) Preparation method of polyurethane fireproof insulation board The polyurethane recycled material weighed in step (1) and the high molecular polymer composite fireproof material obtained in step (2) are added into a stirring device for high-temperature liquefaction and mixing at a mixing temperature of 160° C. and stirred for 30 minutes to obtain a material mixture A; The mixture A is sent to the polyurethane foaming machine through a pressure pipeline. The foaming machine is equipped with a movable mold. The mixture A is sprayed and poured into the mold for foaming and shaping. A set of polyurethane foaming machines can be equipped with 15 sets of movable molds. The molds must be foamed for about 15 minutes after pouring. After the foaming and ripening, demoulding is performed. Manual or automatic equipment can be used for demoulding. After demoulding, material B is obtained; Material B is a long block and needs to be cut into sheets by PU sheet production equipment. After cutting, sheet C is obtained. After passing the inspection, the wood grain is thermally transferred and the sheet is packaged and shipped to obtain the finished polyurethane fireproof insulation sheet.

[0026] A method for recycling polyurethane fireproof and thermal insulation boards comprises the following steps: (1) Crushing of recycled materials The scraps produced during the cutting process of the polyurethane fireproof insulation board or the polyurethane fireproof insulation board that fails the inspection are recycled materials, and the recycled materials are crushed into tiny particles by a crusher as material E; (2) Preparation method of polymer composite elastomer Weigh the raw materials according to the following weight proportions: 80 parts of polystyrene, 10 parts of polypropylene, and 30 parts of polyethylene, put the weighed materials into a hot autoclave for reaction at a reaction temperature of 180 degrees for 3 minutes, and the reacted materials enter a tower reactor at a reaction temperature of 160 degrees for 10 minutes, and then cool to room temperature and enter a kneading machine for kneading at a kneading temperature of 120 degrees for 3-5 minutes. The kneaded materials are then passed through a granulator to be made into small granular polymer composite fireproof materials; (3) Recycling methods of recycled materials The material E obtained in step (1) and the high molecular polymer composite elastomer obtained in step (2) are mixed, and kneaded by a special-shaped extruder to obtain material F. The special-shaped extruder uses a single screw or a twin screw to extrude the material F onto a fixed heating mold for closed molding. The heating mold temperature is about 200°C. After plasticization, the material G is obtained by a cooling and molding process. A 60°C two-pass cooling water tank is used for cooling and molding, and a circulating water cooling system is used. After cooling and molding, the material G enters a heat transfer embossing device for heat transfer embossing. The heat transfer embossing temperature is 60°C. The material is quickly embossed to become a plastic wood product. The scraps generated during the production of the plastic wood product are transported to a crusher for crushing.

[0027] Example 4: A polyurethane fireproof insulation board comprises the following raw materials in parts by weight: 75 parts of polyurethane recycled materials and 25 parts of high molecular polymer composite fireproof materials; the high molecular polymer composite fireproof materials comprise the following raw materials in parts by weight: 70 parts of polystyrene, 15 parts of phosphate polymer, 15 parts of polycarbonate and 10 parts of polypropylene.

[0028] A method for preparing a polyurethane fireproof thermal insulation board comprises the following steps: (1) Weigh the raw materials Weigh the following raw materials by weight: 75 parts of polyurethane recycled material, 70 parts of polystyrene, 15 parts of phosphate polymer, 15 parts of polycarbonate, and 10 parts of polypropylene; (2) Preparation method of polymer composite fireproof material The polystyrene, phosphate polymer, polycarbonate and polypropylene weighed in step (1) are put into a hot autoclave for reaction. All materials are reacted in the hot autoclave at a temperature of 210° C. for 2 minutes. The reacted materials are put into a tower reactor at a temperature of 180° C. for 5 minutes. After cooling to room temperature, the materials are put into a kneading machine for kneading at a temperature of 165° C. for 35 minutes. The kneaded materials are then put into a granulator to be made into small granular polymer composite fireproof materials; (3) Preparation method of polyurethane fireproof insulation board The polyurethane recycled material weighed in step (1) and the high molecular polymer composite fireproof material obtained in step (2) are added into a stirring device for high-temperature liquefaction and mixing at a mixing temperature of 200° C. and stirred for 30 minutes to obtain a material mixture A; The mixture A is sent to the polyurethane foaming machine through a pressure pipeline. The foaming machine is equipped with a movable mold. The mixture A is sprayed and poured into the mold for foaming and shaping. A set of polyurethane foaming machines can be equipped with 10 sets of movable molds. The molds must be foamed for about 30 minutes after pouring. After the foaming and ripening, demoulding is performed. Manual or automatic equipment can be used for demoulding. After demoulding, material B is obtained; Material B is a long block and needs to be cut into sheets by PU sheet production equipment. After cutting, sheet C is obtained. After passing the inspection, the wood grain is thermally transferred and the sheet is packaged and shipped to obtain the finished polyurethane fireproof insulation sheet.

[0029] A method for recycling polyurethane fireproof and thermal insulation boards comprises the following steps: (1) Crushing of recycled materials The scraps produced during the cutting process of the polyurethane fireproof insulation board or the polyurethane fireproof insulation board that fails the inspection are recycled materials, and the recycled materials are crushed into tiny particles by a crusher as material E; (2) Preparation method of polymer composite elastomer Weigh the raw materials according to the following weight proportions: 60 parts of polystyrene, 15 parts of polypropylene, and 20 parts of polyethylene, put the weighed materials into a hot autoclave for reaction at a reaction temperature of 210 degrees for 2 minutes, and the reacted materials enter a tower reactor at a reaction temperature of 180 degrees for 5 minutes, and then cool to room temperature and enter a kneading machine for kneading at a kneading temperature of 165 degrees for 3 minutes. The kneaded materials are then passed through a granulator to be made into small granular polymer composite fireproof materials; (3) Recycled material recycling method The material E obtained in step (1) and the high molecular polymer composite elastomer obtained in step (2) are mixed, and kneaded by a special-shaped extruder to obtain material F. The special-shaped extruder uses a single screw or a twin screw to extrude material F onto a fixed heating mold for closed molding. The heating mold temperature is about 200°C. After plasticization, the material G is obtained by a cooling and molding process. A 90°C two-pass cooling water tank is used for cooling and molding, and a circulating water cooling system is used. After cooling and molding, the material G enters a heat transfer embossing device for heat transfer embossing. The heat transfer embossing temperature is 60°C. The material is quickly embossed to become a plastic wood product. The scraps generated during the production of the plastic wood product are transported to a crusher for crushing.

[0030] Example 5: A polyurethane fireproof thermal insulation board comprises the following raw materials in parts by weight: 70 parts of polyurethane recycled materials and 30 parts of high molecular polymer composite fireproof materials; the high molecular polymer composite fireproof materials comprise the following raw materials in parts by weight: 60 parts of polystyrene, 20 parts of phosphate polymers, 12 parts of polycarbonate and 15 parts of polypropylene.

[0031] A method for preparing a polyurethane fireproof thermal insulation board comprises the following steps: (1) Weigh the raw materials Weigh the raw materials according to the following weight proportions: 70 parts of polyurethane recycled material, 60 parts of polystyrene, 20 parts of phosphate polymer, 12 parts of polycarbonate, and 15 parts of polypropylene; (2) Preparation method of polymer composite fireproof material The polystyrene, phosphate polymer, polycarbonate and polypropylene weighed in step (1) are put into a hot autoclave for reaction. All materials are reacted in the hot autoclave at a temperature of 200° C. for 3 minutes. The reacted materials are put into a tower reactor at a temperature of 170° C. for 10 minutes. After cooling to room temperature, the materials are put into a kneading machine for kneading at a temperature of 150° C. for 35 minutes. The kneaded materials are then put into a granulator to be made into small granular polymer composite fireproof materials; (3) Preparation method of polyurethane fireproof insulation board The polyurethane recycled material weighed in step (1) and the high molecular polymer composite fireproof material obtained in step (2) are added into a stirring device for high-temperature liquefaction and mixing at a mixing temperature of 180° C. and stirred for 30 minutes to obtain a material mixture A; The mixture A is sent to the polyurethane foaming machine through a pressure pipeline. The foaming machine is equipped with a movable mold. The mixture A is sprayed and poured into the mold for foaming and shaping. A set of polyurethane foaming machines can be equipped with 12 sets of movable molds. The mold needs to be foamed for about 20 minutes after pouring. After the foaming and ripening, demoulding is performed. The demoulding process can be performed manually or by automatic equipment. After demoulding, material B is obtained; Material B is a long block and needs to be cut into sheets by PU sheet production equipment. After cutting, sheet C is obtained. After passing the inspection, the wood grain is thermally transferred and the sheet is packaged and shipped to obtain the finished polyurethane fireproof insulation sheet.

[0032] A method for recycling polyurethane fireproof and thermal insulation boards comprises the following steps: (1) Crushing of recycled materials The scraps produced during the cutting process of the polyurethane fireproof insulation board or the polyurethane fireproof insulation board that fails the inspection are recycled materials, and the recycled materials are crushed into tiny particles by a crusher as material E; (2) Preparation method of polymer composite elastomer Weigh the raw materials according to the following weight proportions: 70 parts of polystyrene, 12 parts of polypropylene, and 25 parts of polyethylene, put the weighed materials into a hot autoclave for reaction at a reaction temperature of 200 degrees for 3 minutes, and the reacted materials enter a tower reactor at a reaction temperature of 170 degrees for 10 minutes, and then cool to room temperature and enter a kneading machine for kneading at a kneading temperature of 150 degrees for 5 minutes. The kneaded materials are then passed through a granulator to be made into small granular polymer composite fireproof materials; (3) Recycled material recycling method The material E obtained in step (1) and the high molecular polymer composite elastomer obtained in step (2) are mixed, and kneaded by a special-shaped extruder to obtain material F. The special-shaped extruder uses a single screw or a twin screw to extrude the material F onto a fixed heating mold for closed molding. The heating mold temperature is about 200°C. After plasticization, the material G is obtained by a cooling and molding process. A 75°C two-pass cooling water tank is used for cooling and molding, and a circulating water cooling system is used. After cooling and molding, the material G enters a heat transfer embossing device for heat transfer embossing. The heat transfer embossing temperature is 60°C. The material is quickly embossed to become a plastic wood product. The scraps generated during the production of the plastic wood product are transported to a crusher for crushing.

[0033] Among the above embodiments, embodiment 5 is the best embodiment. The polyurethane fireproof insulation board obtained in embodiment 5 was used to prepare three tests for fireproofing experiments: The experimental results show that the polyurethane fireproof thermal insulation board obtained by the present invention has excellent fireproof performance.

[0034] Finally, it should be noted that the above embodiments are only used to illustrate but not limit the technical solutions of the present invention, and any equivalent substitutions of the present invention and any modifications or partial substitutions that do not depart from the spirit and scope of the present invention should be included in the scope of protection of the claims of the present invention.

Claims

1. A polyurethane fireproof and thermal insulation board, characterized in that: The invention comprises the following raw materials in parts by weight: 65-75 parts of polyurethane recycled materials and 25-35 parts of high molecular polymer composite fireproof materials; the high molecular polymer composite fireproof materials comprise the following raw materials in parts by weight: 50-70 parts of polystyrene, 15-30 parts of phosphate polymers, 10-15 parts of polycarbonate and 10-20 parts of polypropylene.

2. The polyurethane fireproof and heat-insulating board according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 70 parts of polyurethane recycled materials and 30 parts of high molecular polymer composite fireproof materials; the high molecular polymer composite fireproof materials comprise the following raw materials in parts by weight: 60 parts of polystyrene, 20 parts of phosphate polymer, 12 parts of polycarbonate and 15 parts of polypropylene.

3. A method for preparing the polyurethane fireproof and thermal insulation board according to claim 1, characterized in that: The following steps are involved: (1) Weigh the raw materials Weigh the raw materials according to the following weight proportions: 65-75 parts of polyurethane recycled material, 50-70 parts of polystyrene, 15-30 parts of phosphate polymer, 10-15 parts of polycarbonate, and 10-20 parts of polypropylene; (2) Preparation method of polymer composite fireproof material The polystyrene, phosphate polymer, polycarbonate and polypropylene weighed in step (1) are put into a hot autoclave for reaction. All materials are reacted in the hot autoclave at a temperature of 180-210° C. for 2-3 min. The materials after the reaction enter a tower reactor at a temperature of 160-180° C. for 5-10 min. After cooling to room temperature, the materials enter a kneading machine for kneading at a temperature of 120-165° C. for 35 min. The kneaded materials are then passed through a granulator to form small granules of a polymer composite fireproof material; (3) Preparation method of polyurethane fireproof insulation board The polyurethane recycled material weighed in step (1) and the high molecular polymer composite fireproof material obtained in step (2) are added into a stirring device for high-temperature liquefaction and mixing at a mixing temperature of 160-200° C. and stirred for 30 minutes to obtain a material mixture A; The mixture A is sent to the polyurethane foaming machine through a pressure pipeline. The foaming machine is equipped with a movable mold. The mixture A is sprayed and poured into the mold for foaming and shaping. A set of polyurethane foaming machines can be equipped with 10-15 sets of movable molds. The mold needs to be foamed for about 15-30 minutes after pouring. After the foaming and ripening, demoulding is performed. The demoulding process can be performed manually or by automatic equipment. After demoulding, material B is obtained; Material B is a long block and needs to be cut into sheets by PU sheet production equipment. After cutting, sheet C is obtained. After passing the inspection, the wood grain is thermally transferred and the sheet is packaged and shipped to obtain the finished polyurethane fireproof insulation sheet.

4. A method for recycling the polyurethane fireproof and thermal insulation board according to claim 1, characterized in that: The following steps are involved: (1) Crushing of recycled materials The scraps produced during the cutting process of the polyurethane fireproof insulation board or the polyurethane fireproof insulation board that fails the inspection are recycled materials, and the recycled materials are crushed into tiny particles by a crusher as material E; (2) Preparation method of polymer composite elastomer Weigh the raw materials according to the following weight proportions: 60-80 parts of polystyrene, 10-15 parts of polypropylene, and 20-30 parts of polyethylene, put the weighed materials into a hot autoclave for reaction at a reaction temperature of 180-210 degrees for 2-3 minutes, and the reacted materials enter a tower reactor at a reaction temperature of 160-180 degrees for 5-10 minutes, and then cool to room temperature and enter a kneading machine for kneading at a kneading temperature of 120-165 degrees for 3-5 minutes. The kneaded materials are then passed through a granulator to be made into small granular polymer composite fireproof materials; (3) Recycling methods of recycled materials The material E obtained in step (1) and the high molecular polymer composite elastomer obtained in step (2) are mixed, and kneaded by a special-shaped extruder to obtain material F. The special-shaped extruder uses a single screw or a twin screw to extrude the material F onto a fixed heating mold for closed molding. The heating mold temperature is about 200°C. After plasticization, the material G is obtained by a cooling and molding process. The cooling and molding uses a two-pass cooling water tank at 60-90°C and a circulating water cooling system. After cooling and molding, the material G enters a heat transfer embossing device for heat transfer embossing. The heat transfer embossing temperature is 60°C. The material is quickly embossed to become a plastic wood product. The scraps generated during the production of the plastic wood product are transported to a crusher for crushing.