A method for preparing high-temperature and high-humidity infrared-transmitting polyamide composite materials

By combining organic dyes and pigments with hindered amine light stabilizers to prepare high-temperature and high-humidity infrared-transmitting polyamide composites, the problems of pigment migration and color difference changes under high temperature and high humidity conditions have been solved. This method has enabled the material to maintain color stability and infrared transmittance under high temperature and high humidity conditions, thereby expanding the application range of the material.

CN118813038BActive Publication Date: 2026-11-17EMS-GRIVORY (SU ZHOU) ENG PLASTICS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310412424.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2026-11-17
Estimated Expiration
2043-04-18

AI Technical Summary

Technical Problem

Existing infrared-transmitting polyamide materials are prone to pigment migration and color difference changes under high temperature and high humidity conditions, which affects material performance and user experience.

Method used

A method for preparing high-temperature and high-humidity infrared-transmitting polyamide composites was adopted. By compounding organic dyes and pigments with hindered amine light stabilizers, and combining polyamides, antioxidants, ultraviolet light absorbers and dispersants, a composite material that maintains the initial color and infrared transmittance of the material under high-temperature and high-humidity environments was prepared.

Benefits of technology

Under high temperature and high humidity conditions, the color difference of the material decreases, the infrared transmittance remains above 90%, the welding performance is unaffected, and the application range of the material is expanded.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004183675840000131
    Figure BDA0004183675840000131
  • Figure BDA0004183675840000132
    Figure BDA0004183675840000132
  • Figure BDA0004183675840000133
    Figure BDA0004183675840000133
Patent Text Reader

Abstract

This invention relates to a method for preparing a high-temperature and high-humidity infrared-transmitting polyamide composite material. The invention provides a high-temperature and high-humidity infrared-transmitting polyamide composite material, based on a total of 100 parts by weight, comprising the following components in parts by weight: 25-75 parts polyamide, 30-70 parts chopped glass fiber, 0.05-0.5 parts antioxidant, 0.1-1 parts ultraviolet absorber, 0.1-1 parts hindered amine light stabilizer, 0.1-1 parts dispersant, and 0.5-5 parts colorant, wherein the colorant comprises three or more selected from organic solvent yellow 98, organic dye yellow 160:1, organic pigment blue 15:1, organic pigment blue 15:3, organic solvent blue 97, organic solvent red 52, organic solvent red 135, organic solvent red 179, organic solvent violet 31, organic solvent green 3, and organic solvent green 28.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of polymer materials, and in particular to a method for preparing a high-temperature and high-humidity infrared-transmitting polyamide composite material. Background Technology

[0002] Polyamide is a high-molecular-weight engineering plastic with multiple repeating polyamide groups on its molecular backbone. Polyamide possesses excellent mechanical properties, chemical resistance, heat resistance, and ease of processing, and is widely used in communication products, industrial and consumer goods, automotive functional structural components, and interior and exterior trim materials. Infrared-transmitting polyamide is widely used as a transmittance layer in laser welding and has extensive applications in the automotive and industrial consumer goods sectors. Currently, most infrared-transmitting polyamide materials exhibit problems such as pigment precipitation and significant color difference changes on the material surface under high temperature and humidity conditions, greatly affecting product performance and user experience. Due to its special formulation, infrared-transmitting polyamide engineering plastics are prone to pigment migration from the material to the surface and discoloration under the combined effects of high temperature and high humidity. This invention presents a high-temperature and high-humidity resistant infrared-transmitting polyamide composite that can maintain the initial color, infrared transmittance, and laser welding strength of the material under specific conditions.

[0003] Chinese invention patent CN106117940A (application number CN201610519673.7) describes an anti-aging, infrared-transmitting composite material. This invention describes a general-purpose engineering plastic with anti-aging, transparent infrared transmission, suitable for outdoor applications receiving infrared radiation. It improves anti-aging properties by selecting small-particle-size antioxidants, dispersants, UV resistant agents, and colorants. However, this method is not suitable for engineering plastic polyamide composite systems. Therefore, there is an urgent need in the industry to develop a high-temperature, high-humidity, infrared-transmitting polyamide material.

[0004] Polyamide engineering plastics are prone to moisture absorption, and under multiple conditions of heating, humidification, and ultraviolet light, they are more likely to experience color difference and decreased infrared transmittance. This invention patent utilizes the synergistic effect between a combination of high-coloring-strength organic pigments and light stabilizers to achieve non-migration of pigments under high temperature and high humidity conditions, maintaining a material color difference DE < 3 and infrared transmittance at 90%. Summary of the Invention

[0005] To address the shortcomings of existing technologies, one objective of this invention is to provide a high-temperature and high-humidity infrared-transmitting polyamide composite and its preparation method.

[0006] To achieve the above objectives, the present invention provides a method for preparing a high-temperature and high-humidity infrared-transmitting polyamide composite.

[0007] According to one aspect of the present invention, the high-temperature and high-humidity infrared-transmitting polyamide composite of the present invention can maintain the initial color and infrared transmittance of the material, color difference (DE<3.0), infrared laser transmittance (90%), welding strength and performance under the dual effects of high temperature and high humidity.

[0008] According to another aspect of the present invention, the high-temperature and high-humidity infrared-transmitting polyamide composite of the present invention can withstand high-temperature and high-humidity conditions: 150°C for 24 hours; 95°C for 48 hours in boiling water; 75°C for 95% relative humidity; and 25°C for 800 hours in room temperature water immersion; maintaining the initial color of the material (DE<3.0) and infrared laser transmittance (90%), and the laser welding strength is not affected.

[0009] One aspect of the present invention provides a high-temperature, high-humidity, infrared-transmitting polyamide composite, comprising, based on 100 parts by weight, the following components in parts by weight:

[0010] 25-75 parts of polyamide

[0011] 30-70 parts chopped glass fiber

[0012] Antioxidant 0.05-0.5 parts

[0013] 0.1 to 1 part of ultraviolet absorber

[0014] 0.1 to 1 part hindered amine light stabilizer

[0015] Dispersant 0.1 to 1 part

[0016] Color powder 0.5-5 parts,

[0017] The pigments mentioned therein include three or more selected from the following: organic solvent yellow 98, organic dye yellow 160:1, organic pigment blue 15:1, organic pigment blue 15:3, organic solvent blue 97, organic solvent red 52, organic solvent red 135, organic solvent red 179, organic solvent violet 31, organic solvent green 3, and organic solvent green 28.

[0018] Another aspect of the present invention provides a method for preparing a high-temperature and high-humidity infrared-transmitting polyamide composite, comprising the following steps:

[0019] Step 1, Prepare raw materials: The raw materials consist of the following components in parts by weight based on a total of 100 parts by weight:

[0020] 25-75 parts of polyamide

[0021] 30-70 parts chopped glass fiber

[0022] Antioxidant 0.05-0.5 parts

[0023] 0.1 to 1 part of ultraviolet absorber

[0024] 0.1 to 1 part hindered amine light stabilizer

[0025] Dispersant 0.1 to 1 part

[0026] The pigment comprises 0.5 to 5 parts, wherein the pigment includes three or more selected from the following: organic solvent yellow 98, organic dye yellow 160:1, organic pigment blue 15:1, organic pigment blue 15:3, organic solvent blue 97, organic solvent red 52, organic solvent red 135, organic solvent red 179, organic solvent violet 31, organic solvent green 3, and organic solvent green 28.

[0027] Step 2, Mixed Extrusion: Mix and extrude the prepared raw materials.

[0028] Beneficial effects

[0029] The high-temperature and high-humidity infrared-transmitting polyamide composite of the present invention enhances the heat resistance and moisture aging resistance of the material. Under the dual effects of heating and humidification, it maintains the initial color of the material, greatly reduces color difference changes, and has a high infrared transmittance retention rate, thus expanding the application range of laser welding grade polyamide materials. Detailed Implementation

[0030] The products and methods of the present invention will be described in more detail below. The present invention is not limited to the following specific embodiments, and other features and advantages of the inventive concept will become apparent from the following specific embodiments.

[0031] Regarding terminology definitions, unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. In case of conflict, this document (including the definitions) shall prevail. Preferred methods and materials are described below, but similar or equivalent methods and materials may also be used in the practice or testing of the invention. The materials, methods, and examples disclosed herein are illustrative only and not intended to be limiting.

[0032] As used herein, the terms “comprising,” “including,” “having,” “having,” “may,” “containing,” and variations thereof are intended to refer to open transitional phrases, terms, or words that do not exclude the presence or addition of one or more additional features, steps, operations, elements, or components. Unless the context explicitly indicates otherwise, objects without quantifiers include plural objects. However, whether explicitly stated or not, this disclosure also includes other embodiments that “include the embodiments or elements shown herein,” “consist of the embodiments or elements shown herein,” and “consist substantially of the embodiments or elements shown herein.”

[0033] Any range given in absolute or approximate terms is intended to include both, and any definitions used herein are intended to be illustrative rather than limiting. While the numerical ranges and parameters stating a wide range of the invention are approximate, the numerical values ​​stated in the specific embodiments are as precise as possible. However, any numerical value inherently includes some error that must be caused by the standard deviation found in the measurements of the respective tests. Furthermore, all ranges disclosed herein are to be understood to include any and all subranges (including all fractions and integers) included therein.

[0034] All ranges and parameters disclosed herein should be understood to encompass any and all subranges contained therein, and every number between the endpoints. For example, the specified range “1 to 10” should be considered to include any and all subranges between (and including) the minimum value of 1 and the maximum value of 10; that is, all subranges that begin with a minimum value of 1 or greater (e.g., 1 to 6.1) and end with a maximum value of 10 or less (e.g., 2.3 to 9.4, 3 to 8, 4 to 7), and finally the individual numbers 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10 contained within that range. Unless otherwise stated, all percentages, ratios, and proportions herein are by weight.

[0035] Furthermore, this invention includes any and all possible combinations of some or all of the various embodiments described herein. Any and all documents referenced in this application are incorporated herein by reference in their entirety.

[0036] According to one embodiment of this application, the high-temperature and high-humidity infrared-transmitting polyamide composite may comprise, based on a total of 100 parts by weight, the following components in parts by weight:

[0037] 25-75 parts of polyamide

[0038] 30-70 parts chopped glass fiber

[0039] Antioxidant 0.05-0.5 parts

[0040] 0.1 to 1 part of ultraviolet absorber

[0041] 0.1 to 1 part hindered amine light stabilizer

[0042] Dispersant 0.1 to 1 part

[0043] Color powder 0.5-5 parts,

[0044] The pigments may include three or more selected from the following: Organic Solvent Yellow 98, Organic Dye Yellow 160:1, Organic Pigment Blue 15:1, Organic Pigment Blue 15:3, Organic Solvent Blue 97, Organic Solvent Red 52, Organic Solvent Red 135, Organic Solvent Red 179, Organic Solvent Violet 31, Organic Solvent Green 3, and Organic Solvent Green 28.

[0045] According to one embodiment of this application, the polyamide is preferably one or a mixture of two of PA6, PA66, PA610, PA6I / 6T, PA6T / 6I, PA8T / 66, PA12, and PA10T, with an Ubbelohde relative viscosity of 1.6 to 3.0 (m-cresol is used as solvent).

[0046] According to one embodiment of this application, the polyamide may preferably be one or a mixture of two of PA6, PA66, PA610, PA6I / 6T, PA6T / 6I, PA8T / 66, PA12, and PA10T, with an Ubbelohde relative viscosity of 1.8 to 2.5 (m-cresol as solvent).

[0047] According to one embodiment of this application, the polyamide may further preferably include PA66 and PA6I / 6T.

[0048] According to one embodiment of this application, based on 100 parts by weight of the polyamide composite, the polyamide can be 25 to 75 parts. Furthermore, based on 100 parts by weight of the polyamide composite, the polyamide can be 30 to 70 parts, for example 35 to 65 parts, preferably 40 to 65 parts, more preferably 50 to 65 parts, even more preferably 55 to 65 parts, and even more preferably 58 to 60 parts.

[0049] According to one embodiment of this application, based on 100 parts by weight of the polyamide composite, the polyamide may include 15 to 50 parts of PA66 and 10 to 25 parts of PA6I / 6T, preferably 20 to 50 parts of PA66 and 10 to 20 parts of PA6I / 6T, more preferably 40 to 45 parts of PA66 and 10 to 15 parts of PA6I / 6T.

[0050] According to one embodiment of this application, the length of the chopped glass fiber can be 3–4.5 mm, and the diameter can be 8–15 μm. Preferably, the length of the chopped glass fiber can be 3.5–4.5 mm, and the diameter can be 8–15 μm.

[0051] According to one embodiment of this application, more preferably, the length of the chopped glass fiber can be 3 to 4.5 mm, the diameter can be 8 to 15 μm, and the cross-section can be circular and / or elliptical.

[0052] According to one embodiment of this application, more preferably, the length of the chopped glass fiber can be 3 to 4.5 mm, the diameter can be 8 to 15 μm, and the cross-section can be elliptical, with the ratio of the short and long diameters of the ellipse being 1:3 to 1:6.

[0053] According to one embodiment of this application, based on 100 parts by weight of the polyamide composite, the chopped glass fibers can be 30 to 70 parts. Furthermore, based on 100 parts by weight of the polyamide composite, the chopped glass fibers can be 30 to 65 parts, for example 30 to 60 parts, preferably 30 to 55 parts, more preferably 30 to 45 parts, even more preferably 30 to 40 parts, and even more preferably 35 to 40 parts.

[0054] According to one embodiment of this application, the antioxidant preferably includes hindered phenolic antioxidants and / or phosphite heat stabilizers. Preferably, the hindered phenolic antioxidant may include... 1098N,N'-Hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide); phosphite heat stabilizers may include 626 Bis(2,4-di-tert-butylphenyl) pentaerythritol bis(diphosphite).

[0055] According to one embodiment of this application, the antioxidant can be 0.05 to 0.5 parts per 100 parts by weight of the polyamide composite. Furthermore, the antioxidant can be 0.1 to 0.5 parts per 100 parts by weight, for example 0.2 to 0.5 parts, preferably 0.3 to 0.5 parts, more preferably 0.4 to 0.5 parts, and even more preferably 0.45 to 0.5 parts.

[0056] According to one embodiment of this application, based on 100 parts by weight of the polyamide composite, the hindered phenolic antioxidant can be 0.05-0.35 parts, for example 0.1-0.3 parts, preferably 0.2-0.25 parts.

[0057] According to one embodiment of this application, based on 100 parts by weight of the polyamide composite, the phosphite heat stabilizer can be 0.05-0.35 parts, for example 0.1-0.3 parts, preferably 0.2-0.25 parts.

[0058] According to one embodiment of this application, the antioxidant may include a hindered phenolic antioxidant and a phosphite heat stabilizer, wherein based on 100 parts by weight of the polyamide composite, the hindered phenolic antioxidant may be 0.05-0.35 parts, the phosphite heat stabilizer may be 0.05-0.35 parts, preferably 0.1-0.3 parts, the phosphite heat stabilizer may be 0.1-0.3 parts, more preferably 0.2-0.25 parts, the phosphite heat stabilizer may be 0.2-0.25 parts, and the total amount of the hindered phenolic antioxidant and the phosphite heat stabilizer may be 0.05-0.5 parts.

[0059] According to one embodiment of this application, the preferred ultraviolet absorber includes 2-(2H-benzotriazole-2)-4,6-di(1-methyl-1-phenylethyl)-phenol, and more preferably 2-(2H-benzotriazole-2)-4,6-di(1-methyl-1-phenylethyl)-phenol.

[0060] According to one embodiment of this application, the ultraviolet absorber can be 0.1 to 1 part based on 100 parts by weight of the polyamide composite. Furthermore, the ultraviolet absorber can be 0.1 to 0.5 parts based on 100 parts by weight of the polyamide composite, for example 0.1 to 0.3 parts, preferably 0.1 to 0.25 parts, and more preferably 0.15 to 0.2 parts.

[0061] According to one embodiment of this application, the hindered amine light stabilizer preferably includes N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-N,N'-dialdehyde hexamethylenediamine, and more preferably N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-N,N'-dialdehyde hexamethylenediamine.

[0062] According to one embodiment of this application, the hindered amine light stabilizer may be 0.1 to 1 part based on 100 parts by weight of the polyamide composite. Furthermore, the hindered amine light stabilizer may be 0.1 to 0.5 parts, for example 0.1 to 0.3 parts, preferably 0.1 to 0.2 parts, and more preferably 0.1 to 0.15 parts, based on 100 parts by weight of the polyamide composite.

[0063] According to one embodiment of this application, the dispersant may include stearates and / or vinyl bis-stearamide complexes. Preferably, the stearates may include magnesium stearate and / or zinc stearate, and preferably, the vinyl bis-stearamide complex may include a vinyl bis-stearamide (EBS) complex. The dispersant may also include magnesium stearate, zinc stearate, and / or a vinyl bis-stearamide (EBS) complex.

[0064] According to one embodiment of this application, the dispersant can be 0.1 to 1 part based on 100 parts by weight of the polyamide composite. Furthermore, the dispersant can be 0.1 to 0.5 parts based on 100 parts by weight of the polyamide composite, preferably 0.15 to 0.3 parts, and more preferably 0.2 to 0.25 parts.

[0065] According to one embodiment of this application, the pigment may include three or more selected from the following: organic solvent yellow 98, organic dye yellow 160:1, organic pigment blue 15:1, organic pigment blue 15:3, organic solvent blue 97, organic solvent red 52, organic solvent red 135, organic solvent red 179, organic solvent violet 31, organic solvent green 3, and organic solvent green 28.

[0066] According to one embodiment of this application, the pigment may include four or more selected from the following: organic solvent yellow 98, organic dye yellow 160:1, organic pigment blue 15:1, organic pigment blue 15:3, organic solvent blue 97, organic solvent red 52, organic solvent red 135, organic solvent red 179, organic solvent violet 31, organic solvent green 3, and organic solvent green 28.

[0067] According to one embodiment of this application, the pigment may include five or more selected from the following: organic solvent yellow 98, organic dye yellow 160:1, organic pigment blue 15:1, organic pigment blue 15:3, organic solvent blue 97, organic solvent red 52, organic solvent red 135, organic solvent red 179, organic solvent violet 31, organic solvent green 3, and organic solvent green 28.

[0068] According to one embodiment of this application, the pigment may include six or more selected from the following: organic solvent yellow 98, organic dye yellow 160:1, organic pigment blue 15:1, organic pigment blue 15:3, organic solvent blue 97, organic solvent red 52, organic solvent red 135, organic solvent red 179, organic solvent violet 31, organic solvent green 3, and organic solvent green 28.

[0069] According to one embodiment of this application, preferred pigments may include organic solvent yellow 98, organic pigment blue 15:1, organic pigment blue 15:3, organic solvent blue 97, organic solvent red 52, and organic solvent green 3. According to one embodiment of this application, preferred pigments may include organic solvent yellow 98, organic pigment blue 15:1, organic pigment blue 15:3, organic solvent blue 97, and organic solvent red 52.

[0070] As non-limiting examples, Hostasol Yellow 98 can be used; Hostasol Yellow 3G can be used for Organic Pigment Blue 15:1; Heliogen Blue 15:3 can be used for Organic Pigment Blue K7090; Macrolex Blue 97 can be used for Organic Pigment Blue RR; Macrolex Red 52 can be used for Organic Pigment Blue 5B; and Macrolex Green 3 can be used for Organic Pigment Blue 5B.

[0071] According to one embodiment of this application, based on a total of 100% by weight of pigment, the pigment may include 1% to 30% organic solvent yellow 98, preferably 5% to 25% organic solvent yellow 98, more preferably 10% to 25% organic solvent yellow 98. For example, the pigment may include 10% organic solvent yellow 98, or 15% organic solvent yellow 98, or 20% organic solvent yellow 98, or 25% organic solvent yellow 98.

[0072] According to one embodiment of this application, based on a total of 100% by weight of pigment powder, the pigment powder may include 1% to 10% organic pigment blue 15:1, preferably 5% to 7.5% organic pigment blue 15:1. For example, the pigment powder may include 5% organic pigment blue 15:1 or 7.5% organic pigment blue 15:1.

[0073] According to one embodiment of this application, based on a total of 100% by weight of pigment powder, the pigment powder may include 1% to 10% organic pigment blue 15:3, preferably 5% to 7.5% organic pigment blue 15:3. For example, the pigment powder may include 5% organic pigment blue 15:3 or 7.5% organic pigment blue 15:3.

[0074] According to one embodiment of this application, based on a total of 100% by weight of pigment, the pigment may include 1% to 35% of organic solvent blue 97, preferably 10% to 30% of organic solvent blue 97, more preferably 20% to 30% of organic solvent blue 97. For example, the pigment may include 20% organic solvent blue 97, or 25% organic solvent blue 97, or 30% organic solvent blue 97.

[0075] According to one embodiment of this application, based on a total of 100% by weight of pigment, the pigment may include 1% to 40% organic solvent red 52, preferably 10% to 35% organic solvent red 52, more preferably 20% to 35% organic solvent red 52, and even more preferably 30% to 35% organic solvent red 52. For example, the pigment may include 35% organic solvent red 52.

[0076] According to one embodiment of this application, based on a total of 100% by weight of pigment, the pigment may include 0% to 25% organic solvent green 3, preferably 1% to 25% organic solvent green 3, more preferably 10% to 20% organic solvent green 3, and even more preferably 15% to 20% organic solvent green 3. For example, the pigment may include 20% organic solvent green 3.

[0077] According to one embodiment of this application, based on a total of 100% by weight of pigment, the preferred pigment may include 1% to 30% organic solvent yellow 98, 1% to 10% organic pigment blue 15:1, 1% to 10% organic pigment blue 15:3, 1% to 35% organic solvent blue 97, 1% to 40% organic solvent red 52 and 0% to 25% organic solvent green 3.

[0078] According to one embodiment of this application, based on a total of 100% by weight of pigments, more preferably, the pigments include 10% to 25% organic solvent yellow 98, 5% to 7.5% organic pigment blue 15:1, 5% to 7.5% organic pigment blue 15:3, 20% to 30% organic solvent blue 97, 30% to 35% organic solvent red 52 and 15% to 20% organic solvent green 3.

[0079] According to one embodiment of this application, based on a total of 100% by weight of pigments, more preferably, the pigments include 10% to 25% organic solvent yellow 98, 5% to 7.5% organic pigment blue 15:1, 5% to 7.5% organic pigment blue 15:3, 20% to 30% organic solvent blue 97, and 30% to 35% organic solvent red 52.

[0080] Besides the above-mentioned color powder combinations, there are no restrictions on the types and proportions of color powders added. For example, the types and proportions of color powders can be adjusted according to actual color requirements.

[0081] The high-temperature and high-humidity infrared-transmitting polyamide composite of the present invention can be prepared by the following method, including the following steps:

[0082] Step 1: Prepare raw materials: including the aforementioned components and their weight proportions.

[0083] Step 2, Mixed Extrusion: Mix and extrude the prepared raw materials.

[0084] According to one embodiment of this application, in the above-mentioned mixing extrusion step, polyamide, antioxidant, ultraviolet light absorber, hindered amine light stabilizer, dispersant, and colorant are mixed and stirred evenly, and then added to a twin-screw extruder; during the extrusion process of the above mixture, chopped glass fibers are added to the twin-screw extruder by side feeding and extruded together at high temperature, cooled, drawn and pelletized, with an extrusion temperature of 260℃~330℃, to obtain a high-temperature and high-humidity infrared-transmitting polyamide composite.

[0085] According to one embodiment of this application, in the above-mentioned mixing extrusion step, the extrusion temperature can be, for example, 260°C, 265°C, 270°C, 275°C, 280°C, 285°C, 290°C, 295°C, 300°C, 305°C, 310°C, 315°C, 320°C, 325°C, or 330°C.

[0086] The above description of the components (including content) in the high-temperature and high-humidity infrared-transmitting polyamide composite applies to the components (including content) in the preparation method.

[0087] The advantages of this invention are as follows: The high-temperature and high-humidity infrared-transmitting polyamide composite of this invention, through multiple compounding of organic dyes, organic pigments, and hindered amine light stabilizers, reduces the problems of easy migration and decomposition of single pigments or dyes, achieving high coloring efficiency and high infrared transmittance, thus not affecting the infrared transmittance of the material and greatly improving the temperature and humidity resistance of the infrared-transmitting polyamide material. The optimized compound color powder combination includes the following components: polyamide, antioxidant, ultraviolet light absorber, hindered amine light stabilizer, and dispersant, and the specific weights are rationally selected, so that the high-temperature and high-humidity infrared-transmitting polyamide composite maintains the initial color of the material under the dual effects of high temperature and high humidity, the color difference change is greatly reduced, the infrared transmittance is maintained at 90%, and the welding performance is not affected. Therefore, it can be widely used in the automotive, industrial and consumer goods fields.

[0088] The infrared-penetrating material of this invention can be applied to the design of laser welding for automotive engine peripherals and interior / exterior trim products. It is environmentally friendly and resistant to high temperatures and humidity, meeting the material selection requirements of major OEMs such as Volkswagen and Ford. For industrial consumer products such as watches and mobile phone interiors / exterior trim, it enhances product aesthetics, durability, and color diversity.

[0089] Example

[0090] The technical solution of the present invention will be described in more detail below with reference to specific comparative examples and embodiments. The above content can be better understood by referring to the following embodiments, but the embodiments shown are for illustrative purposes only and are not intended to limit the scope of the invention. In particular, the embodiments illustrate representative embodiments of the inherent principles of the invention, and these principles are not strictly limited to the specific conditions described in these embodiments. Therefore, it should be understood that the present invention covers various changes and modifications to the embodiments described herein, and such changes and modifications can be made without departing from the spirit and scope of the invention and without diminishing its intended advantages. Therefore, such changes and modifications are contemplated to be included in the appended claims.

[0091] Comparative Example 1

[0092] The dark brown-black infrared-transmitting glass fiber reinforced polyamide material of this comparative example is composed of the following components in parts by weight: 47 parts polyamide PA66 (U4840NL NC01), 15 parts polyamide PA6I / 6T (TI1207), and 35 parts chopped glass fibers (…). 540H), 0.25 parts hindered phenolic antioxidant ( 1098), 0.25 parts phosphite heat stabilizer ( 626), 0.15 parts UV absorber ( UV-234), 0.1 parts light stabilizer ( UV-944), 0.25 parts dispersant (CMS P-130), 2 parts pigment (30% organic solvent green 5 Macrolex 5B, 30% organic solvent blue 97 Macrolex Blue RR, 40% organic solvent red 135 Clariant RED G).

[0093] The preparation method of the dark brown-black infrared-transmitting glass fiber reinforced polyamide material of Comparative Example 1 includes the following steps:

[0094] Step 1: Mix polyamide PA66, polyamide PA6I / 6T, hindered phenolic antioxidant, phosphite heat stabilizer, ultraviolet absorber, light stabilizer, dispersant, and colorant until homogeneous.

[0095] Step 2: Add the mixture obtained in Step 1 into a twin-screw extruder. The twin-screw extruder has a total of 9 temperature sections. The temperature of the first and second sections is 260 degrees Celsius, and the temperature of the other three sections is 285 degrees Celsius. The main machine speed is 850 rpm. Short glass fibers are added from the side feed during the extrusion process. Finally, after extrusion, cooling, traction, and pelletizing, a dark brown-black infrared-transmitting glass fiber reinforced polyamide material is obtained.

[0096] The obtained material was dried at 80 degrees Celsius for 6 hours in a dehumidifying dryer, and then injection molded into test samples.

[0097] Comparative Example 2

[0098] This comparative example of a light brown-black infrared-transmitting glass fiber reinforced polyamide material consists of the following components in parts by weight: 48 parts polyamide PA66, 15 parts polyamide PA6I / 6T, 35 parts chopped glass fiber, 0.25 parts hindered phenolic antioxidant, 0.25 parts phosphite heat stabilizer, 0.15 parts ultraviolet absorber, 0.1 parts light stabilizer, 0.25 parts dispersant, and 1 part colorant (35% organic solvent green 5 Macrolex 5B, 35% organic solvent blue 97 Macrolex Blue RR, and 30% organic solvent red 135 Clariant RED G).

[0099] The preparation method of the light brown-black infrared-transmitting glass fiber reinforced polyamide material in Comparative Example 2 is the same as that in Comparative Example 1.

[0100] Example 1

[0101] The brown-red-black 1 high-temperature and high-humidity infrared-transmitting polyamide composite of this embodiment is composed of the following components in parts by weight: 45 parts polyamide PA66, 15 parts polyamide PA6I / 6T, 35 parts chopped glass fiber, 0.25 parts hindered phenolic antioxidant, 0.25 parts phosphite heat stabilizer, 0.15 parts ultraviolet absorber, 0.1 parts light stabilizer, 0.25 parts dispersant, and 4 parts pigments (15% organic solvent yellow 98 (Hostasol Yellow 3G), 5% organic pigment blue 15:1 (HOSTAPERM BLUE A2R), 5% organic pigment blue 15:3 (HELIOGENBLUE K7090), 20% organic solvent blue 97 (MACROLEX BLAU RR), 35% organic solvent red 52 (MACROLEX RED 5B), and 20% organic solvent green 3 (Macrolex GREEN 5B).

[0102] The preparation method of the brown-red-black 1 high-temperature and high-humidity infrared-transmitting polyamide composite in Example 1 is the same as that in Comparative Example 1.

[0103] Example 2

[0104] The brown-red-black high-temperature and high-humidity infrared-transmitting polyamide composite of this embodiment is composed of the following components in parts by weight: 47 parts polyamide PA66, 15 parts polyamide PA6I / 6T, 35 parts chopped glass fiber, 0.25 parts hindered phenolic antioxidant, 0.25 parts phosphite heat stabilizer, 0.15 parts ultraviolet absorber, 0.1 parts light stabilizer, 0.25 parts dispersant, and 2 parts pigments (10% organic solvent yellow 98 (Hostasol Yellow 3G), 7.5% organic pigment blue 15:1 (HOSTAPERM BLUEA2R), 7.5% organic pigment blue 15:3 (HELIOGENBLUE K7090), 20% organic solvent blue 97 (MACROLEX BLAURR), 35% organic solvent red 52 (MACROLEX RED 5B), and 20% organic solvent green 3 (Macrolex GREEN 5B).

[0105] The preparation method of the brown-red-black 2 high-temperature and high-humidity infrared-transmitting polyamide composite in Example 2 is the same as that in Comparative Example 1.

[0106] Example 3

[0107] The brown-black 3-temperature- and high-humidity infrared-transmitting polyamide composite of this embodiment is composed of the following components in parts by weight: 44 parts polyamide PA66, 15 parts polyamide PA6I / 6T, 35 parts chopped glass fiber, 0.25 parts hindered phenolic antioxidant, 0.25 parts phosphite heat stabilizer, 0.15 parts ultraviolet absorber, 0.1 parts light stabilizer, 0.25 parts dispersant, and 4 parts pigments (25% organic solvent yellow 98 (Hostasol Yellow 3G), 5% organic pigment blue 15:1 (HOSTAPERM BLUE A2R), 5% organic pigment blue 15:3 (HELIOGENBLUE K7090), 30% organic solvent blue 97 (MACROLEX BLAU RR), and 35% organic solvent red 52 (MACROLEX RED 5B).

[0108] The preparation method of the brown-black 3 high-temperature and high-humidity infrared-transmitting polyamide composite in Example 3 is the same as that in Comparative Example 1.

[0109] Example 4

[0110] The brown-black, high-temperature and high-humidity infrared-transmitting polyamide composite of this embodiment is composed of the following components in parts by weight: 46 parts polyamide PA66, 14 parts polyamide PA6I / 6T, 35 parts chopped glass fiber, 0.25 parts hindered phenolic antioxidant, 0.25 parts phosphite heat stabilizer, 0.15 parts ultraviolet absorber, 0.1 parts light stabilizer, 0.25 parts dispersant, 2 parts pigments (25% organic solvent yellow 98 (Hostasol Yellow 3G), 5% organic pigment blue 15:1 (HOSTAPERM BLUE A2R), 5% organic pigment blue 15:3 (HELIOGENBLUE K7090), 30% organic solvent blue 97 (MACROLEX BLAU RR), and 35% organic solvent red 52 (MACROLEX RED 5B).

[0111] The preparation method of the brown-black 3 high-temperature and high-humidity infrared-transmitting polyamide composite in Example 4 is the same as that in Comparative Example 1.

[0112] High temperature and high humidity aging performance test

[0113] The performance of the materials obtained in the comparative examples and embodiments was tested and evaluated using the following methods.

[0114] 1) Color difference measurement equipment: 600, D65 light source, 10-degree angle, D8 structural colorimeter

[0115] 2) Color difference measurement environment: 23℃, 50% relative humidity

[0116] 3) Infrared transmittance testing equipment: TMG 3,980nm

[0117] 4) The experimental sample was an injection-molded template: dimensions 50 x 45 x 1 mm

[0118] 5) Heating and humidifying aging conditions include: Condition 1: 25℃, 800 hours; Condition 2: 75℃, 95%RH, 48 hours; Condition 3: 95℃, 48 hours of boiling water immersion; Condition 4: 150℃, 24 hours of hot air.

[0119] After each heating and humidification test was completed, the sample was removed and allowed to recover for 2 hours at 23°C and 50% relative humidity before color difference measurement was performed.

[0120] The formula for calculating the infrared transmittance retention rate is as follows: T before aging and T after aging are the infrared transmittance rates of the samples before and after aging, respectively.

[0121]

[0122] The table below shows the test results for high temperature and high humidity resistance of the comparative examples and embodiments:

[0123] Table 1: Data after aging under condition 1: 25℃, 800 hours

[0124]

[0125] Table 2: Data after aging under condition 2: 75℃, 95%RH, 48 hours

[0126]

[0127] Table 3: Data after aging under condition 3: 95℃, 48-hour boiling water immersion

[0128]

[0129] Table 4: Data after aging under condition 4: 150℃, 24 hours of hot air

[0130]

[0131]

[0132] Based on the test results in the table above, it can be seen that the high-temperature and high-humidity infrared-transmitting polyamide composite of the present invention has excellent high-temperature and high-humidity aging resistance. Under the dual effects of heating and humidification, it maintains the initial color of the material, the color difference change is greatly reduced, and the infrared transmittance remains above 90%.

[0133] The high-temperature and high-humidity infrared-transmitting polyamide composite of the present invention achieves infrared-transmitting materials of different colors by compounding organic dyes and organic pigments. It is combined with polyamide, antioxidants, ultraviolet light absorbers, hindered amine light stabilizers, and dispersants, and the specific weights are reasonably selected so that the high-temperature and high-humidity infrared-transmitting polyamide composite retains the initial color of the material under the dual effects of heating and moisture absorption and ultraviolet light. The color difference change is greatly reduced, the infrared transmittance retention rate is high, and the application range of laser welding grade polyamide materials is expanded.

[0134] Although the invention can be embodied in many different forms, specific preferred embodiments of the invention are described in detail herein. This disclosure is an example of the principles of the invention and is not intended to limit the invention to the specific embodiments described. Furthermore, the invention covers any possible combination of some or all of the various embodiments mentioned herein, described herein, and / or incorporated herein. In addition, the invention also specifically excludes any possible combination of any or some of the various embodiments mentioned herein, described herein, and / or incorporated herein.

[0135] The foregoing disclosure is intended to be illustrative and not exhaustive. Individual elements or features of a particular embodiment are generally not limited to that particular embodiment, but may be used in other embodiments and may be combined in other ways, even if not specifically shown or described. Such variations are included in this invention. Based on the description herein, many modifications and alternatives will be conceived by those skilled in the art. All such alternatives and modifications are intended to be included within the scope of the claims. Those skilled in the art will recognize other equivalents of the specific embodiments described herein, which are also intended to be covered by the claims.

Claims

1. A high-temperature and high-humidity infrared-transmitting polyamide composite, based on a total of 100 parts by weight, comprising the following components in parts by weight: 25-75 parts of polyamide 30-70 parts chopped glass fiber Antioxidant 0.05-0.5 parts 0.1 to 1 part of ultraviolet absorber 0.1 to 1 part hindered amine light stabilizer Dispersant 0.1 to 1 part Color powder 0.5-5 parts, The pigments, based on a total weight of 100%, include 1% to 30% organic solvent yellow 98, 1% to 10% organic pigment blue 15:1, 1% to 10% organic pigment blue 15:3, 1% to 35% organic solvent blue 97, 1% to 40% organic solvent red 52, and 0% to 25% organic solvent green 3.

2. The polyamide composite according to claim 1, wherein the polyamide is one or a mixture of two of PA6, PA66, PA610, PA6I / 6T, PA6T / 6I, PA8T / 66, PA12, and PA10T, and the Ubbelohde relative viscosity of the polyamide with m-cresol as solvent is 1.6 to 3.

0.

3. The polyamide composite according to claim 2, wherein the polyamide is one or a mixture of two of PA6, PA66, PA610, PA6I / 6T, PA6T / 6I, PA8T / 66, PA12, and PA10T, and the Ubbelohde relative viscosity of the polyamide with m-cresol as solvent is 1.8 to 2.

5.

4. The polyamide composite according to claim 1, wherein the chopped glass fibers have a length of 3.5 to 4.5 mm and a diameter of 8 to 15 μm.

5. The polyamide composite according to claim 1, wherein the chopped glass fibers have a length of 3 to 4.5 mm, a diameter of 8 to 15 μm, and a circular and / or elliptical cross-section.

6. The polyamide composite according to claim 1, wherein the chopped glass fibers have a length of 3-4.5 mm, a diameter of 8-15 μm, and an elliptical cross-section, wherein the ratio of the short and long diameters of the ellipse is 1:3 to 1:

6.

7. The polyamide composite according to claim 1, wherein the antioxidant comprises a hindered phenolic antioxidant and a phosphite heat stabilizer, wherein the hindered phenolic antioxidant comprises N,N'-hexamethylene bis(3,5-di-tert-butyl-4-hydroxyphenylpropionamide); and the phosphite heat stabilizer comprises bis(2,4-di-tert-butylphenyl)pentaerythritol bis(diphosphite).

8. The polyamide composite according to claim 7, wherein the hindered phenolic antioxidant is 0.05-0.35 parts, the phosphite heat stabilizer is 0.05-0.35 parts, and the total amount of the hindered phenolic antioxidant and the phosphite heat stabilizer is 0.05-0.5 parts.

9. The polyamide composite according to claim 1, wherein the ultraviolet absorber comprises 2-(2H-benzotriazole-2)-4,6-di(1-methyl-1-phenylethyl)-phenol.

10. The polyamide composite according to claim 1, wherein the hindered amine light stabilizer comprises N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-N,N'-dialdehyde hexamethylenediamine.

11. The polyamide composite of claim 1, wherein the dispersant comprises stearates and / or vinyl bis-stearamide composites, wherein the stearates comprise magnesium stearate and / or zinc stearate, and the vinyl bis-stearamide composite comprises a vinyl bis-stearamide EBS composite.

12. A method for preparing high-temperature and high-humidity infrared-transmitting polyamide composites, comprising the following steps: Step 1, Prepare raw materials: The raw materials consist of the following components in parts by weight based on a total of 100 parts by weight: 25-75 parts of polyamide 30-70 parts chopped glass fiber Antioxidant 0.05-0.5 parts 0.1 to 1 part of ultraviolet absorber 0.1 to 1 part hindered amine light stabilizer Dispersant 0.1 to 1 part The pigment comprises 0.5 to 5 parts, based on a total weight of 100%, of which 1% to 30% is organic solvent yellow 98, 1% to 10% is organic pigment blue 15:1, 1% to 10% is organic pigment blue 15:3, 1% to 35% is organic solvent blue 97, 1% to 40% is organic solvent red 52, and 0% to 25% is organic solvent green 3. Step 2, Mixed Extrusion: Mix and extrude the prepared raw materials.

13. The method according to claim 12, wherein in the mixing extrusion step, the polyamide, the antioxidant, the ultraviolet absorber, the hindered amine light stabilizer, the dispersant and the colorant are mixed and stirred evenly, and then added to a twin-screw extruder; during the extrusion process of the mixture, the chopped glass fibers are added to the twin-screw extruder by side feeding and extruded together at high temperature, cooled, drawn and pelletized, with the extrusion temperature being 260℃~330℃, to obtain the high-temperature and high-humidity infrared-transmitting polyamide composite.

14. A high-temperature and high-humidity infrared-transmitting polyamide composite prepared by the method according to claim 12 or 13.

15. The use of the high-temperature and high-humidity infrared-transmitting polyamide composite according to any one of claims 1 to 11 and 14 for use in automotive engine peripherals and interior and exterior trim products.

16. The use of the high-temperature and high-humidity infrared-transmitting polyamide composite according to any one of claims 1 to 11 and 14 for use in the interior and exterior trim of watches and mobile phones.

Citation Information

Patent Citations

  • Anti-aging infrared penetrable composite material and preparation method thereof

    CN106117940A

  • Polyamide composition and preparation method and application thereof

    CN111621147A