A production process for bulletproof skylight nano multilayer external film
By applying a nano-multi-layer outer filming process on the panoramic sky curtain of new energy vehicles and combining carbon nanotubes, the problem of insufficient impact resistance of the sky curtain is solved, the bulletproof level is improved and the production cost is reduced, and the safety in the car is ensured.
Patent Information
- Application Number
- CN202411307334.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-19
AI Technical Summary
The panoramic skylight of new energy vehicles lacks stress dispersed structure and lacks impact and penetration resistance, making it difficult to reach the bulletproof level, and the bulletproof glass manufacturing process is complex and costly.
The nano-multi-layer outer film coating process is adopted, and the multi-layer structure of polyurea layer, polyurethane layer, pressure-sensitive adhesive layer and self-healing layer is combined with the use of carbon nanotubes to improve the impact resistance of the sky curtain and reduce production difficulty and cost.
It effectively improves the impact resistance of the panoramic sky curtain, reduces the difficulty of construction and production, and controls costs, ensuring safety in the car.
Smart Images

Figure CN118813154B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of bulletproof films, and in particular relates to a production process of a bulletproof skylight nano multilayer outer film. Background Art
[0002] Since the battery pack of new energy vehicles is located in the chassis, the thickness of the chassis is increased, resulting in a smaller interior space than a fuel vehicle of the same size. Therefore, in order to ensure that the owner has enough space inside the car, new energy vehicles will use panoramic skylight glass to cover the roof, which can provide more space on the one hand and better vision and lighting on the other hand. However, compared with the steel structure roof of fuel vehicles, the safety of the panoramic skylight is worrying.
[0003] For safety reasons, new energy vehicles mostly use tempered glass to manufacture panoramic glass. The hardness of tempered glass exceeds that of ordinary steel roof structures. According to the national standards GB 9656-2021 and GB / T 5137.1-2020, tempered glass needs to withstand the impact of a 227±2g steel ball falling from 6 meters and a 2260g steel ball falling from 4 meters without falling for 5 seconds. However, due to the lack of stress dispersion structure in the large-area panoramic skylight, the stress generated when the panoramic skylight is impacted is concentrated, making its impact resistance and penetration resistance inferior to that of the steel roof, and it is far from reaching the bulletproof level. The manufacturing process of bulletproof glass is complicated, the product processing is difficult, and it is difficult to process into the shape of a panoramic skylight. The cost is much higher than that of ordinary tempered glass. Therefore, it is necessary to provide a production process for a nano multi-layer external film for a bulletproof skylight. Summary of the invention
[0004] The purpose of the present invention is to overcome the above shortcomings and provide a production process for a bulletproof skylight nano multi-layer external film, which can improve the impact resistance of the panoramic skylight to the bulletproof level while reducing the construction difficulty and material cost.
[0005] The purpose of the present invention is achieved through the following technical solutions: a production process of a bulletproof skylight nano multilayer external film, comprising:
[0006] S1, preparation of polyurea coating liquid: by weight, 45-50 parts of diphenylmethane diisocyanate, 160-180 parts of polycaprolactone polyol, and 40-70 parts of polytetramethylene ether diparaaminobenzoate are mixed and stirred for 10-18 minutes, 6-10 parts of diethyltoluenediamine and 10-15 parts of dichlorodiphenylmethane diammonium are added thereto, stirring is continued for 10-18 minutes, and finally 0.8-1.2 parts of carbon nanotubes are added and stirred for 18-25 minutes;
[0007] S2, preparation of polyurethane layer coating liquid: according to weight, 30-40 parts of polypropylene glycol, 80-100 parts of polybutylene glycol, and 350-400 parts of ethyl acetate are selected and put into a stirring tank and stirred for 3-8 minutes as a mixed solution 1 for standby; 9-10 parts of hexamethylene diisocyanate and 28-32 parts of ethyl acetate are put into a stirring tank and stirred for 3-8 minutes, and mixed solution 1 is added thereto and stirred for 10-18 minutes to obtain mixed solution 2 for standby; 1-2 parts of 1,2-butanediol and 3-4 parts of butyl acetate are added to mixed solution 2 and stirred for 18-25 minutes to prepare a polyurethane layer coating liquid;
[0008] S3, preparation of pressure-sensitive adhesive coating liquid: 10-15 parts of polyacrylate and 35-50 parts of ethyl acetate are selected by weight, put into a stirring kettle and stirred for 3-8 minutes, transferred to a high-speed disperser, carbon nanotubes are added thereto, dispersed at high speed, and used as mixed liquid three for standby; 1-2 parts of p-phenylene diisocyanate and 2-5 parts of ethyl acetate are put into a stirring kettle, stirred for 3-8 minutes, mixed liquid three is added thereto, stirred for 10-18 minutes, and prepared into a pressure-sensitive adhesive coating liquid;
[0009] S4, preparation of self-repairing layer coating liquid: by weight, 4-5 parts of aminopropyl-terminated polydimethylsiloxane, 3-4 parts of polyetheramine and 25-30 parts of tetrahydrofuran are selected and put into a stirring kettle, and after stirring for 3-8 minutes, 1-2 parts of diphenylmethane diisocyanate are added thereto, and stirred for 18-25 minutes to prepare a self-repairing layer coating liquid;
[0010] S5. Coating: (a) Tear off the protective film 1 on one side of the polyurethane substrate, and apply a polyurethane layer on the surface, and after drying in an oven, stick a PET protective film 1 to prepare a semi-finished product 1; (b) Tear off the protective film 2 on the other side of the polyurethane substrate on the semi-finished product 1, and apply a polyurea layer on the surface, and after drying in an oven, stick a PET protective film 2 to prepare a semi-finished product 2; (c) Tear off the PET protective film 1 on the polyurethane layer of the semi-finished product 2, apply a pressure-sensitive adhesive layer on the base paper release film, and after drying in an oven, coat it with the polyurethane layer of the semi-finished product 2, and prepare a finished product 3; (d) Tear off the PET protective film 2 on one side of the polyurea layer of the semi-finished product 3, and apply a self-repairing layer on the surface, and after drying in an oven, stick it with a silicone protective film to make a finished product.
[0011] The further improvement of the present invention is that the polyurethane substrate is made by mixing oligomer polyol, polyisocyanate, catalyst and cross-linking agent through twin-screw extrusion, and the hardness is between 90-95.
[0012] A further improvement of the present invention is that the oligomer polyol is one or more of polycarbonate diol, polycaprolactone diol, polybutylene glycol and polypropylene glycol.
[0013] A further improvement of the present invention is that the polyisocyanate is one or more of xylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, p-phenylene diisocyanate, 4,4',4''4-thiophosphoric acid triphenyl triisocyanate and the like.
[0014] A further improvement of the present invention is that the catalyst is dibutyltin dilaurate.
[0015] A further improvement of the present invention is that the cross-linking agent is one or more of diethyltoluenediamine, 3,3'-4,4'-4-diaminodiphenylmethane, 3,5-dimethylthiotoluenediamine, and 3,5-dimethylthiotoluenediamine.
[0016] The further improvement of the present invention is that the thickness of the silicone protective film is 50 μm, the thickness of the self-healing layer is 7-8 μm, the thickness of the polyurea layer is 9-10 μm, the thickness of the polyurethane layer is 13-16 μm, the thickness of the polyurethane substrate is 150 μm, the thickness of the pressure-sensitive adhesive layer is 27-30 μm, and the thickness of the base paper release film is 75 μm.
[0017] Compared with the prior art, the present invention has the following advantages:
[0018] The outer film prepared by the present invention is used for a bulletproof skylight, which can protect the outer side of the skylight from being scratched by the external environment, reduce the difficulty of construction and production, and the bulletproof functional layer is provided with a multi-layer structure, which can absorb a large amount of impact energy. The pressure-sensitive adhesive layer is added with carbon nanotubes, which can absorb impact energy and increase adhesion, thereby protecting the safety of people in the car when the glass is broken. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Schematic diagram of the structure of the polyurethane substrate in step S5 (a) of the present invention.
[0020] Figure 2 Schematic diagram of the structure of finished product 1 in step S5 (a) of the present invention.
[0021] Figure 3 This is a schematic diagram of the structure of the finished product 2 in step S5 (b) of the present invention.
[0022] Figure 4 This is a schematic diagram of the structure of the finished product before three coatings in step S5 (c) of the present invention.
[0023] Figure 5 This is a schematic diagram of the structure of finished product three in step S5 (c) of the present invention.
[0024] Figure 6 Schematic diagram of the finished product structure of the bulletproof skylight nano multilayer outer film in step S5 (d) of the present invention.
[0025] Numbers in the figure:
[0026] 1-polyurethane substrate, 2-protective film 1, 3-polyurethane layer, 4-PET protective film 1, 5-protective film 2, 6-polyurea layer, 7-PET protective film 2, 8-base paper release film, 9-pressure-sensitive adhesive layer, 10-self-healing layer, 11-silicone protective film. DETAILED DESCRIPTION
[0027] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with embodiments and drawings. The embodiments are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.
[0028] In the description of the present invention, it is necessary to understand that terms indicating orientation or positional relationships, such as orientation or positional relationships based on the drawings, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the structure or unit referred to must have a specific orientation. Therefore, it should not be understood as a limitation on the present invention.
[0029] In the present invention, unless otherwise clearly stipulated and limited, terms such as "connected", "provided with", "having" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection. It can be said to be a mechanical connection, or it can be directly connected, or it can be connected through an intermediate medium. For those skilled in the art, the basic meaning of the above terms in the present invention can be understood according to the specific circumstances.
[0030] A production process for bulletproof skylight nano multilayer external film, comprising:
[0031] S1, preparation of polyurea coating liquid: by weight, 45-50 parts of diphenylmethane diisocyanate, 160-180 parts of polycaprolactone polyol, and 40-70 parts of polytetramethylene ether diparaaminobenzoate are mixed and stirred for 10-18 minutes, 6-10 parts of diethyltoluenediamine and 10-15 parts of dichlorodiphenylmethane diammonium are added thereto, stirring is continued for 10-18 minutes, and finally 0.8-1.2 parts of carbon nanotubes are added and stirred for 18-25 minutes;
[0032] S2, preparation of polyurethane layer coating liquid: according to weight, 30-40 parts of polypropylene glycol, 80-100 parts of polybutylene glycol, and 350-400 parts of ethyl acetate are selected and put into a stirring tank and stirred for 3-8 minutes as a mixed solution 1 for standby; 9-10 parts of hexamethylene diisocyanate and 28-32 parts of ethyl acetate are put into a stirring tank and stirred for 3-8 minutes, and mixed solution 1 is added thereto and stirred for 10-18 minutes to obtain mixed solution 2 for standby; 1-2 parts of 1,2-butanediol and 3-4 parts of butyl acetate are added to mixed solution 2 and stirred for 18-25 minutes to prepare a polyurethane layer coating liquid;
[0033] S3, preparation of pressure-sensitive adhesive coating liquid: 10-15 parts of polyacrylate and 35-50 parts of ethyl acetate are selected by weight, put into a stirring kettle and stirred for 3-8 minutes, transferred to a high-speed disperser, carbon nanotubes are added thereto, dispersed at high speed, and used as mixed liquid three for standby; 1-2 parts of p-phenylene diisocyanate and 2-5 parts of ethyl acetate are put into a stirring kettle, stirred for 3-8 minutes, mixed liquid three is added thereto, stirred for 10-18 minutes, and prepared into a pressure-sensitive adhesive coating liquid;
[0034] S4, preparation of self-repairing layer coating liquid: by weight, 4-5 parts of aminopropyl-terminated polydimethylsiloxane, 3-4 parts of polyetheramine and 25-30 parts of tetrahydrofuran are selected and put into a stirring kettle, and after stirring for 3-8 minutes, 1-2 parts of diphenylmethane diisocyanate are added thereto, and stirred for 18-25 minutes to prepare a self-repairing layer coating liquid;
[0035] S5, coating: refer to Figures 1 to 6 , (a), tear off the protective film 2 on one side of the polyurethane substrate 1, and apply the polyurethane layer 3 on the surface, and after drying in an oven, stick the PET protective film 4 to prepare a semi-finished product 1 for use; (b), tear off the protective film 2 5 on the other side of the polyurethane substrate 1 on the semi-finished product 1, and apply the polyurea layer 6 on the surface, and after drying in an oven, stick the PET protective film 2 7 to prepare a semi-finished product 2 for use; (c), tear off the PET protective film 4 on the polyurethane layer 3 of the semi-finished product 2, apply the pressure-sensitive adhesive layer 9 on the base paper release film 8, and after drying in an oven, coat it with the polyurethane layer 3 of the semi-finished product 2 to prepare a finished product 3 for use; (d), tear off the PET protective film 2 7 on one side of the polyurea layer 6 of the semi-finished product 3, and cover the self-repairing layer 10 on the surface, and after drying in an oven, stick it with the silicone protective film 11 to make a finished product.
[0036] The outer film prepared by the present invention is used for a bulletproof skylight, which can protect the outer side of the skylight from being scratched by the external environment, reduce the difficulty of construction and production, and the bulletproof functional layer is provided with a multi-layer structure, which can absorb a large amount of impact energy. The pressure-sensitive adhesive layer is added with carbon nanotubes, which can absorb impact energy and increase adhesion, thereby protecting the safety of people in the car when the glass is broken.
[0037] In the present application, the polyurethane substrate 1 is made by mixing oligomer polyol, polyisocyanate, catalyst and cross-linking agent through twin-screw extrusion, and has a hardness of 90-95.
[0038] In the present application, the oligomer polyol is one or more of polycarbonate diol, polycaprolactone diol, polybutylene glycol, and polypropylene glycol.
[0039] In the present application, the polyisocyanate is one or more of xylyl diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, p-phenylene diisocyanate, 4,4',4''-triphenyl triisocyanate, and the like.
[0040] In the present application, the catalyst is dibutyltin dilaurate.
[0041] In the present application, the crosslinking agent is one or more of diethyltoluenediamine, 3,3'-4,4'-4-diaminodiphenylmethane, 3,5-dimethylthiotoluenediamine, and 3,5-dimethylthiotoluenediamine.
[0042] In the present application, the thickness of the silicone protective film 11 is 50 μm, the thickness of the self-healing layer 10 is 7-8 μm, the thickness of the polyurea layer 6 is 9-10 μm, the thickness of the polyurethane layer 3 is 13-16 μm, the thickness of the polyurethane substrate 1 is 150 μm, the thickness of the pressure-sensitive adhesive layer 9 is 27-30 μm, and the thickness of the base paper release film 8 is 75 μm. Example 1
[0043] A production process for bulletproof skylight nano multilayer external film, comprising:
[0044] S1, preparation of polyurea coating liquid: by weight, 45 parts of diphenylmethane diisocyanate, 160 parts of polycaprolactone polyol, and 40 parts of polytetramethylene ether diparaaminobenzoate were selected and mixed and stirred for 10 minutes, 6 parts of diethyltoluenediamine and 10 parts of dichlorodiphenylmethane diammonium were added thereto, and stirring was continued for 10 minutes, and finally 0.8 parts of carbon nanotubes were added and stirred for 18 minutes;
[0045] S2, preparation of polyurethane layer coating liquid: according to weight, 30 parts of polypropylene glycol, 80 parts of polybutylene glycol, and 350 parts of ethyl acetate are selected and put into a stirring tank and stirred for 3 minutes to prepare a mixed solution 1 for standby use; 9 parts of hexamethylene diisocyanate and 28 parts of ethyl acetate are put into a stirring tank and stirred for 3 minutes, and mixed solution 1 is added thereto and stirred for 10 minutes to obtain mixed solution 2 for standby use; 1 part of 1,2-butanediol and 3 parts of butyl acetate are added to mixed solution 2 and stirred for 18 minutes to prepare a polyurethane layer coating liquid;
[0046] S3, preparation of pressure-sensitive adhesive coating liquid: 10 parts of polyacrylate and 35 parts of ethyl acetate are selected by weight, put into a stirring kettle and stirred for 3 minutes, transferred to a high-speed disperser, carbon nanotubes are added thereto, dispersed at high speed, and used as mixed solution three for standby; 1 part of p-phenylene diisocyanate and 2 parts of ethyl acetate are put into a stirring kettle, stirred for 3 minutes, mixed solution three is added thereto, stirred for 10 minutes, and prepared into a pressure-sensitive adhesive coating liquid;
[0047] S4, preparation of self-repairing layer coating liquid: 4 parts of aminopropyl-terminated polydimethylsiloxane, 3 parts of polyetheramine and 25 parts of tetrahydrofuran are selected by weight and put into a stirring kettle. After stirring for 3 minutes, 1 part of diphenylmethane diisocyanate is added thereto, and the self-repairing layer coating liquid is prepared after stirring for 18 minutes;
[0048] S5, coating: refer to Figures 1 to 6 , (a), tear off the protective film 2 on one side of the polyurethane substrate 1, and apply the polyurethane layer 3 on the surface, and after drying in an oven, stick the PET protective film 4 to prepare a semi-finished product 1 for use; (b), tear off the protective film 2 5 on the other side of the polyurethane substrate 1 on the semi-finished product 1, and apply the polyurea layer 6 on the surface, and after drying in an oven, stick the PET protective film 2 7 to prepare a semi-finished product 2 for use; (c), tear off the PET protective film 4 on the polyurethane layer 3 of the semi-finished product 2, apply the pressure-sensitive adhesive layer 9 on the base paper release film 8, and after drying in an oven, coat it with the polyurethane layer 3 of the semi-finished product 2 to prepare a finished product 3 for use; (d), tear off the PET protective film 2 7 on one side of the polyurea layer 6 of the semi-finished product 3, and cover the self-repairing layer 10 on the surface, and after drying in an oven, stick it with the silicone protective film 11 to make a finished product. Example 2
[0049] A production process for bulletproof skylight nano multilayer external film, comprising:
[0050] S1, preparation of polyurea coating liquid: by weight, 50 parts of diphenylmethane diisocyanate, 180 parts of polycaprolactone polyol, and 70 parts of polytetramethylene ether diparaaminobenzoate were mixed and stirred for 18 minutes, 10 parts of diethyltoluenediamine and 15 parts of dichlorodiphenylmethane diammonium were added thereto, stirring was continued for 18 minutes, and finally 1.2 parts of carbon nanotubes were added and stirred for 25 minutes;
[0051] S2, preparation of polyurethane layer coating liquid: according to weight, 40 parts of polypropylene glycol, 100 parts of polybutylene glycol, and 400 parts of ethyl acetate are selected and put into a stirring tank and stirred for 8 minutes to prepare a mixed solution 1 for standby use; 10 parts of hexamethylene diisocyanate and 32 parts of ethyl acetate are put into a stirring tank and stirred for 8 minutes, and mixed solution 1 is added thereto and stirred for 18 minutes to obtain mixed solution 2 for standby use; 2 parts of 1,2-butanediol and 4 parts of butyl acetate are added to mixed solution 2 and stirred for 25 minutes to prepare a polyurethane layer coating liquid;
[0052] S3, preparation of pressure-sensitive adhesive coating liquid: 15 parts of polyacrylate and 50 parts of ethyl acetate are selected by weight and put into a stirring kettle and stirred for 8 minutes, then transferred to a high-speed disperser, carbon nanotubes are added thereto, and dispersed at high speed to prepare a third mixed solution for standby use; 1-2 parts of p-phenylene diisocyanate and 5 parts of ethyl acetate are put into a stirring kettle and stirred for 8 minutes, and the third mixed solution is added thereto and stirred for 18 minutes to prepare a pressure-sensitive adhesive coating liquid;
[0053] S4, preparation of self-repairing layer coating liquid: 5 parts of aminopropyl-terminated polydimethylsiloxane, 4 parts of polyetheramine and 30 parts of tetrahydrofuran are selected by weight and put into a stirring kettle. After stirring for 8 minutes, 2 parts of diphenylmethane diisocyanate are added thereto, and stirred for 25 minutes to prepare a self-repairing layer coating liquid;
[0054] S5, coating: refer to Figures 1 to 6 , (a), tear off the protective film 2 on one side of the polyurethane substrate 1, and apply the polyurethane layer 3 on the surface, and after drying in an oven, stick the PET protective film 4 to prepare a semi-finished product 1 for use; (b), tear off the protective film 2 5 on the other side of the polyurethane substrate 1 on the semi-finished product 1, and apply the polyurea layer 6 on the surface, and after drying in an oven, stick the PET protective film 2 7 to prepare a semi-finished product 2 for use; (c), tear off the PET protective film 4 on the polyurethane layer 3 of the semi-finished product 2, apply the pressure-sensitive adhesive layer 9 on the base paper release film 8, and after drying in an oven, coat it with the polyurethane layer 3 of the semi-finished product 2 to prepare a finished product 3 for use; (d), tear off the PET protective film 2 7 on one side of the polyurea layer 6 of the semi-finished product 3, and cover the self-repairing layer 10 on the surface, and after drying in an oven, stick it with the silicone protective film 11 to make a finished product. Example 3
[0055] A production process for bulletproof skylight nano multilayer external film, comprising:
[0056] S1, preparation of polyurea coating liquid: by weight, 48 parts of diphenylmethane diisocyanate, 170 parts of polycaprolactone polyol, and 50 parts of polytetramethylene ether diparaaminobenzoate were selected and mixed and stirred for 15 minutes, 8 parts of diethyltoluenediamine and 12 parts of dichlorodiphenylmethane diammonium were added thereto, stirring was continued for 15 minutes, and finally 1 part of carbon nanotubes was added and stirred for 20 minutes;
[0057] S2, preparation of polyurethane layer coating liquid: according to weight, 35 parts of polypropylene glycol, 90 parts of polybutylene glycol, and 380 parts of ethyl acetate are selected and put into a stirring tank and stirred for 5 minutes to prepare a mixed solution 1 for standby; 9.5 parts of hexamethylene diisocyanate and 30 parts of ethyl acetate are put into a stirring tank and stirred for 5 minutes, and mixed solution 1 is added thereto and stirred for 15 minutes to obtain mixed solution 2 for standby; 1.5 parts of 1,2-butanediol and 3.5 parts of butyl acetate are added to mixed solution 2 and stirred for 20 minutes to prepare a polyurethane layer coating liquid;
[0058] S3, preparation of pressure-sensitive adhesive coating liquid: 12 parts of polyacrylate and 40 parts of ethyl acetate are selected by weight and put into a stirring kettle and stirred for 5 minutes, then transferred to a high-speed disperser, carbon nanotubes are added thereto, and dispersed at high speed to prepare mixed solution three for standby use; 1.5 parts of p-phenylene diisocyanate and 3 parts of ethyl acetate are put into a stirring kettle and stirred for 5 minutes, mixed solution three is added thereto, and stirred for 15 minutes to prepare a pressure-sensitive adhesive coating liquid;
[0059] S4, preparation of self-repairing layer coating liquid: by weight, 4-5 parts of aminopropyl-terminated polydimethylsiloxane, 3-4 parts of polyetheramine and 25-30 parts of tetrahydrofuran are selected and put into a stirring kettle, and after stirring for 3-8 minutes, 1-2 parts of diphenylmethane diisocyanate are added thereto, and stirred for 18-25 minutes to prepare a self-repairing layer coating liquid;
[0060] S5, coating: refer to Figures 1 to 6 , (a), tear off the protective film 2 on one side of the polyurethane substrate 1, and apply the polyurethane layer 3 on the surface, and after drying in an oven, stick the PET protective film 4 to prepare a semi-finished product 1 for use; (b), tear off the protective film 2 5 on the other side of the polyurethane substrate 1 on the semi-finished product 1, and apply the polyurea layer 6 on the surface, and after drying in an oven, stick the PET protective film 2 7 to prepare a semi-finished product 2 for use; (c), tear off the PET protective film 4 on the polyurethane layer 3 of the semi-finished product 2, apply the pressure-sensitive adhesive layer 9 on the base paper release film 8, and after drying in an oven, coat it with the polyurethane layer 3 of the semi-finished product 2 to prepare a finished product 3 for use; (d), tear off the PET protective film 2 7 on one side of the polyurea layer 6 of the semi-finished product 3, and cover the self-repairing layer 10 on the surface, and after drying in an oven, stick it with the silicone protective film 11 to make a finished product.
[0061] Select test samples and comparison samples and conduct tests according to GB 17840-1999:
[0062] Comparison sample 1: panoramic skylight glass;
[0063] Comparison sample 2: panoramic skylight glass + internal PET window film;
[0064] Test sample 1: panoramic skylight glass + external film (without bulletproof layer and without carbon nanotubes added to the pressure-sensitive adhesive layer);
[0065] Test sample 2: panoramic skylight glass + external film (without bulletproof layer, carbon nanotubes added to the pressure-sensitive adhesive);
[0066] Test sample 3: panoramic skylight glass + external film (including bulletproof layer, no carbon nanotubes added in the pressure-sensitive adhesive);
[0067] Test sample 4: panoramic skylight glass + external film 1 in Example 1 (bulletproof skylight nano multi-layer external film);
[0068] Test sample 5: panoramic skylight glass + external film 2 in Example (bulletproof skylight nano multi-layer external film);
[0069] Test sample 6: panoramic skylight glass + external film 3 in Example (bulletproof skylight nano multi-layer external film);
[0070]
[0071] Among them, F means that the bullet hits the glass surface but does not penetrate, 64, 54, and 79 respectively represent 7.62mm bullets fired by a 64-type pistol, a 54-type pistol, and a 79-type submachine gun, L means that glass fragments fly but do not penetrate the test card, M means that fragments fly but do not embed into the test card, and H means that glass fragments do not fly. It can be seen that test sample 6, that is, embodiment 3, is the best technical solution.
[0072] Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A production process for bulletproof skylight nano multilayer external film, characterized in that: include S1, preparation of polyurea coating liquid: by weight, 45-50 parts of diphenylmethane diisocyanate, 160-180 parts of polycaprolactone polyol, and 40-70 parts of polytetramethylene ether diparaaminobenzoate are mixed and stirred for 10-18 minutes, 6-10 parts of diethyltoluenediamine and 10-15 parts of dichlorodiphenylmethane diammonium are added thereto, stirring is continued for 10-18 minutes, and finally 0.8-1.2 parts of carbon nanotubes are added and stirred for 18-25 minutes; S2, preparation of polyurethane layer coating liquid: according to weight, 30-40 parts of polypropylene glycol, 80-100 parts of polybutylene glycol, and 350-400 parts of ethyl acetate are selected and put into a stirring tank and stirred for 3-8 minutes as a mixed solution 1 for standby; 9-10 parts of hexamethylene diisocyanate and 28-32 parts of ethyl acetate are put into a stirring tank and stirred for 3-8 minutes, and mixed solution 1 is added thereto and stirred for 10-18 minutes to obtain mixed solution 2 for standby; 1-2 parts of 1,2-butanediol and 3-4 parts of butyl acetate are added to mixed solution 2 and stirred for 18-25 minutes to prepare a polyurethane layer coating liquid; S3, preparation of pressure-sensitive adhesive coating liquid: 10-15 parts of polyacrylate and 35-50 parts of ethyl acetate are selected by weight, put into a stirring kettle and stirred for 3-8 minutes, transferred to a high-speed disperser, carbon nanotubes are added thereto, dispersed at high speed, and used as mixed liquid three for standby; 1-2 parts of p-phenylene diisocyanate and 2-5 parts of ethyl acetate are put into a stirring kettle, stirred for 3-8 minutes, mixed liquid three is added thereto, stirred for 10-18 minutes, and prepared into a pressure-sensitive adhesive coating liquid; S4, preparation of self-repairing layer coating liquid: by weight, 4-5 parts of aminopropyl-terminated polydimethylsiloxane, 3-4 parts of polyetheramine and 25-30 parts of tetrahydrofuran are selected and put into a stirring kettle, and after stirring for 3-8 minutes, 1-2 parts of diphenylmethane diisocyanate are added thereto, and stirred for 18-25 minutes to prepare a self-repairing layer coating liquid; S5, coating: (a), tear off the protective film 1 (2) on one side of the polyurethane substrate (1), and apply a polyurethane layer (3) on the surface, and after drying in an oven, adhere a PET protective film 1 (4) to prepare a semi-finished product 1 for use; (b), tear off the protective film 2 (5) on the other side of the polyurethane substrate (1) on the semi-finished product 1, and apply a polyurea layer (6) on the surface, and after drying in an oven, adhere a PET protective film 2 (7) to prepare a semi-finished product 2 for use; (c), tear off the PET protective film 1 (4) on the polyurethane layer (3) of the semi-finished product 2, apply a pressure-sensitive adhesive layer (9) on the base paper release film (8), and after drying in an oven, coat the pressure-sensitive adhesive layer with the polyurethane layer (3) of the semi-finished product 2 to prepare a finished product 3 for use; (d), tear off the PET protective film 2 (7) on one side of the polyurea layer (6) of the semi-finished product 3, and apply a self-repairing layer (10) on the surface, and after drying in an oven, adhere the pressure-sensitive adhesive layer with the silicone protective film (11) to prepare a finished product.
2. According to the production process of a bulletproof skylight nano multilayer outer film according to claim 1, it is characterized in that: The polyurethane substrate (1) is prepared by mixing oligomer polyol, polyisocyanate, catalyst and cross-linking agent through twin-screw extrusion, and has a hardness of 90-95.
3. According to the production process of a bulletproof skylight nano multilayer outer film according to claim 2, it is characterized in that: The oligomer polyol is one or more of polycarbonate diol, polycaprolactone diol, polybutylene glycol and polypropylene glycol.
4. According to claim 3, a production process of a bulletproof skylight nano multilayer outer film is characterized in that: The polyisocyanate is one or more of tolyl diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, p-phenylene diisocyanate, 4,4',4''4-thiophosphoric acid triphenyl triisocyanate and the like.
5. The production process of a bulletproof skylight nano multilayer outer film according to claim 4, characterized in that: The catalyst is dibutyltin dilaurate.
6. The production process of a bulletproof skylight nano multilayer outer film according to claim 5, characterized in that: The crosslinking agent is one or more of diethyltoluenediamine, 3,3'-4,4'-4-diaminodiphenylmethane, 3,5-dimethylthiotoluenediamine, and 3,5-dimethylthiotoluenediamine.
7. The production process of a bulletproof skylight nano multilayer outer film according to claim 6, characterized in that: The thickness of the silicone protective film (11) is 50 μm, the thickness of the self-healing layer (10) is 7-8 μm, the thickness of the polyurea layer (6) is 9-10 μm, the thickness of the polyurethane layer (3) is 13-16 μm, the thickness of the polyurethane substrate (1) is 150 μm, the thickness of the pressure-sensitive adhesive layer (9) is 27-30 μm, and the thickness of the base paper release film (8) is 75 μm.