KrF negative photoresist and preparation method and patterning forming method thereof
By using KrF negative photoresist with components such as resin and acid generator with a specific structure, the problems of low resolution and poor heat resistance of existing KrF negative photoresists are solved, and high-resolution and high-temperature stable patterns are achieved. Formed, suitable for Lift off process.
Patent Information
- Application Number
- CN202410879670.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-22
AI Technical Summary
The existing KrF negative photoresist has low resolution and poor heat resistance, which causes the pattern to easily deform and collapse when used at high temperatures, making it difficult to achieve high-resolution pattern formation in the lift-off process.
Using hydroxystyrene-styrene-maleic anhydride copolymer and diisocyanate resin with a specific structure as the resin matrix, and combining acid generators, cross-linking agents and acid diffusion inhibitors to form an inverted trapezoidal morphology of KrF negative light The resist is exposed and developed using a 248nm light source to form a pattern.
Significantly improves the resolution of KrF negative photoresist to 100nm, maintains pattern stability at high temperatures, is suitable for lift off processes, and provides high resolution and good heat resistance.
Smart Images

Figure CN118818901A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photoresists, and in particular relates to a KrF negative photoresist and a preparation method and a patterning method thereof. Background Art
[0002] Photoresists are divided into positive photoresists and negative photoresists according to the principle of imaging. The dissolution rate of the exposed area in the developer changes from slow to fast, while the dissolution rate of the non-exposed area in the developer is very slow, and the photoresist that finally leaves the non-exposed area on the substrate is called a positive photoresist. The dissolution rate of the non-exposed area in the developer changes from fast to slow, while the dissolution rate of the non-exposed area in the developer is still very fast, and the photoresist that finally leaves the exposed area on the substrate is called a negative photoresist.
[0003] The main components of negative photoresist include polymer resin, photoacid, crosslinker and solvent. After exposure, the photoacid produces acid, thereby catalyzing the crosslinking of the polymer resin, significantly reducing the solubility of the photoresist in the developer, turning it from soluble to insoluble, thereby leaving a negative photolithography pattern after development.
[0004] The lift-off process (also known as the lift-off process) is a process for introducing metal electrodes on a substrate by evaporation. The process flow is as follows: first, a photoresist is coated on the substrate, and a pattern is obtained after exposure and development; then, the substrate with the photoresist pattern is subjected to sputtering evaporation of metal, and the part without photoresist protection can be sputtered onto the substrate, and the part with photoresist protection has the metal sputtered onto the photoresist; after sputtering, the substrate is placed in a stripping solution for stripping, and the photoresist and the metal on its surface are stripped off, thereby introducing a metal electrode in a set area of the substrate.
[0005] In order to achieve that the stripping liquid can react with the photoresist during the photoresist stripping process and quickly remove the photoresist and the metal on its surface, the photoresist used in the stripping process is generally designed to have an inverted trapezoidal morphology. Currently, the most researched method is to use KrF negative photoresist in the stripping process, which requires balancing multiple aspects such as micro-bridging of lines, peeling of lines, and trapezoidal morphology, resulting in the difficulty in improving the resolution of lift-off KrF negative photoresist. In addition, the heat resistance of KrF negative photoresist is poor, and the pattern is easily deformed and collapsed when used at high temperatures. Summary of the invention
[0006] The first purpose of the present invention is to overcome the defects of the existing KrF negative photoresist, such as low resolution and poor heat resistance, and the pattern is easily deformed when used at high temperature, and to provide a new KrF negative photoresist. Compared with the negative photoresist using the existing KrF excimer laser, the KrF negative photoresist provided by the present invention has high resolution in a short-wavelength exposure source, and can increase the resolution of the KrF negative photoresist used in the lift off process to 100nm. At the same time, it has good heat resistance, and the pattern formed at high temperature does not deform or collapse.
[0007] The second object of the present invention is to provide a method for preparing the above-mentioned KrF negative photoresist.
[0008] A third object of the present invention is to provide a patterning method.
[0009] Specifically, the KrF negative photoresist provided by the present invention contains resin A, resin B, an acid generator, a crosslinking agent, an acid diffusion inhibitor and a solvent, wherein the resin A is a hydroxystyrene-styrene-maleic anhydride copolymer having a structure shown in formula (I), and the resin B is a diisocyanate resin having a structure shown in formula (II);
[0010] NCO-R-OCN formula (Ⅱ),
[0011] In formula (I), x is 20% to 40%, y is 20% to 45%, z is 20% to 50%, and x+y+z is 100%; in formula (II), R is a biphenyl group or a phenoxyphenyl group, and each benzene ring in the biphenyl group and the phenoxyphenyl group has a hydrogen atom substituted by a trifluoromethyl group.
[0012] In a preferred embodiment, based on the total weight of the KrF negative photoresist, the content of the resin A is 10% to 50%, the content of the resin B is 2% to 10%, the content of the acid generator is 0.1% to 10%, the content of the cross-linking agent is 0.1% to 5%, the content of the acid diffusion inhibitor is 0.01% to 5%, and the balance is solvent.
[0013] In a preferred embodiment, the mass ratio of the resin A to the resin B is (2-6):1.
[0014] In a preferred embodiment, the weight average molecular weight of the resin A is 5,000 to 20,000.
[0015] In a preferred embodiment, R has at least one of the structures shown in formula (1) to formula (4):
[0016]
[0017] In a preferred embodiment, the acid generator is selected from at least one of triphenylsulfonium trifluoromethanesulfonate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium antimonate, methyldiphenyliodonium trifluoromethanesulfonate, di-tert-butyldiphenyliodonium trifluoromethanesulfonate, triphenylsulfonium perfluorobutylsulfonate, methylbiphenyliodonium perfluorobutylsulfonate, triphenylsulfonium perfluorooctanesulfonate and trifluoromethanesulfonic acid diaryliodonium salt.
[0018] In a preferred embodiment, the crosslinking agent is selected from at least one of tetramethoxymethyl glycoluril, tetramethoxyethyl glycoluril, tri(2,3-epoxypropyl)isocyanurate and trimethylolpropane triglycidyl ether.
[0019] In a preferred embodiment, the acid diffusion inhibitor is selected from at least one of methyltriamine, ethyltriamine, dimethylamine, diethylamine, trimethylamine, triethylamine, tributylamine, methanoltriamine, ethanoltriamine, dimethanolamine and triethanolamine.
[0020] The preparation method of the KrF negative photoresist provided by the invention comprises the steps of uniformly mixing resin A, resin B, an acid generator, a cross-linking agent, an acid diffusion inhibitor and a solvent.
[0021] The patterning forming method provided by the present invention comprises forming a photoresist layer on a substrate with the above-mentioned KrF negative photoresist, exposing the photoresist layer through a mask with a light source having a wavelength of 248nm, and then developing to form a photoresist pattern.
[0022] The key to the present invention is to use resin A and resin B with specific structures as the resin matrix of KrF negative photoresist at the same time, and use resin A, resin B, acid generator, cross-linking agent, acid diffusion inhibitor and solvent in combination. The KrF negative photoresist thus obtained has an inverted trapezoidal morphology, high resolution, high sensitivity and good heat resistance. The pattern formed at high temperature does not deform or collapse, and can be applied to the lift off process. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a resolution diagram of the KrF negative photoresist obtained in Example 1. DETAILED DESCRIPTION
[0024] The KrF negative photoresist provided by the present invention contains resin A, resin B, an acid generator, a cross-linking agent, an acid diffusion inhibitor and a solvent. Among them, the mass ratio of resin A and resin B is preferably (1-25):1, more preferably (2-6):1, such as 2:1, 3:1, 4:1, 5:1, 6:1 or any value therebetween. When the mass ratio of resin A and resin B is controlled within the above preferred range, the resolution of the corresponding KrF negative photoresist is higher. The mass ratio of acid generator and resin B is preferably (0.01-5):1, such as 0.01:1, 0.1:1, 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1 or any value therebetween. The mass ratio of the crosslinking agent to the resin B is preferably (0.01-2.5):1, such as 0.01:1, 0.1:1, 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1 or any value therebetween. The mass ratio of the acid diffusion inhibitor to the resin B is preferably (0.001-2.5):1, such as 0.001:1, 0.005:1, 0.01:1, 0.1:1, 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1 or any value therebetween. In a preferred embodiment, based on the total weight of the KrF negative photoresist, the content of the resin A is 10% to 50% (such as 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or any value therebetween), the content of the resin B is 2% to 10% (such as 2%, 4%, 6%, 8%, 10% or any value therebetween), the content of the acid generator is 0.1% to 10% (such as 0.1%, 2%, 4%, 6%, 8%, 10% or any value therebetween), and the The content of the cross-linking agent is 0.1% to 5% (such as 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% or any value therebetween), the content of the acid diffusion inhibitor is 0.01% to 5% (such as 0.01%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% or any value therebetween), and the balance is the solvent. At this time, the resolution, sensitivity and heat resistance of the corresponding KrF negative photoresist are better.
[0025] In the present invention, resin A is a hydroxystyrene-styrene-maleic anhydride copolymer having a structure shown in formula (I):
[0026]
[0027] In formula (I), x, y and z are used to represent the molar percentage of hydroxystyrene structural units, the molar percentage of styrene structural units and the molar percentage of maleic anhydride structural units, respectively. x, y and x are calculated by the feed amount. x is 20% to 40%, such as 20%, 25%, 30%, 35%, 40% or any value therebetween; y is 20% to 45%, such as 20%, 25%, 30%, 35%, 40%, 42%, 45% or any value therebetween; z is 20% to 50%, such as 20%, 25%, 30%, 35%, 40%, 45%, 50% or any value therebetween; x+y+z is 100%. Formula (I) only represents the composition and content of each structural unit, and does not represent the connection relationship between each structural unit. The copolymer shown in formula (I) can be a random copolymer, a block copolymer or an alternating copolymer. In addition, the weight average molecular weight of resin A is preferably 5000-20000, such as 5000, 6000, 8000, 10000, 12000, 14000, 16000, 18000, 20000 or any value therebetween. Resin A can be obtained commercially or by free radical polymerization of hydroxystyrene, styrene and maleic anhydride. The specific preparation process is well known to those skilled in the art and will not be described in detail herein.
[0028] In the present invention, resin B is a diisocyanate resin having a structure shown in formula (II):
[0029] NCO-R-OCN formula (Ⅱ),
[0030] In formula (II), R is biphenyl or phenoxyphenyl, and each benzene ring in the biphenyl and phenoxyphenyl has a hydrogen atom substituted by a trifluoromethyl group. Preferably, R has at least one of the structures shown in formula (1) to formula (4), wherein: Indicates the key connection end:
[0031]
[0032] That is, resin B has one of the structures shown in formula (5) to formula (8):
[0033]
[0034] Resin B can be purchased commercially, or prepared by various existing methods, for example, it can be prepared according to the method disclosed in CN107955166B.
[0035] In the present invention, the acid generator mainly plays the role of promoting the cross-linking reaction of the resin. The acid generator can be a conventional photoacid generator (PAG) and / or a thermal acid generator (thermal acid generator), and can be specifically selected from at least one of a sulfonium salt-based compound, an iodine salt-based compound, a salt-based compound, an organic sulfonic acid, etc. Specific examples of the acid generator include, but are not limited to, dodecylbenzenesulfonic acid, p-toluenesulfonic acid, phthalimido trifluoromethanesulfonate, phthalimido trifluoromethanesulfonate, dinitrobenzyl toluenesulfonate, dinitrobenzyl toluenesulfonate, n-decyl disulfone, naphthyl imino trifluoromethanesulfonate, naphthyl imino trifluoromethanesulfonate, diphenyl iodine trifluoromethanesulfonate, diphenyl iodine perfluorobutyl sulfonate, diphenyl iodine hexafluorophosphate, diphenyl iodine hexafluorophosphate, Fluoroarsenate, diphenyliodonium hexafluoroantimonate, diphenyl p-methoxyphenylsulfonium trifluoromethanesulfonate, diphenyl p-toluenesulfonium trifluoromethanesulfonate, diphenyl p-tert-butylphenylsulfonium trifluoromethanesulfonate, diphenyl p-isobutylphenylsulfonium trifluoromethanesulfonate, triphenylsulfonium trifluoromethanesulfonate, tri(p-tert-butylphenyl)sulfonium trifluoromethanesulfonate, diphenyl p-methoxyphenylsulfonium perfluorobutylsulfonate, diphenyl p-tolylsulfonium perfluorobutylsulfonate, diphenyl p-tert-butylphenyl sulfonium perfluorobutylsulfonate, diphenyl p-isobutylphenylsulfonium perfluorobutylsulfonate, diphenyl iodonium trifluoromethanesulfonate, diphenyl iodonium antimonate, methyl diphenyl iodonium trifluoromethanesulfonate, di-tert-butyl diphenyl iodonium trifluoromethanesulfonate, triphenyl sulfonium perfluorobutylsulfonate, methyl biphenyl iodonium perfluorobutylsulfonate, triphenyl sulfonium perfluorooctanesulfonate and trifluoromethanesulfonic acid diaryliodonium salt tri-p-tert-butylphenyl sulfonium perfluorobutylsulfonate, hexafluoroarsenate, hexafluoro At least one of arsenate, triphenylsulfonium hexafluoroantimonate and dibutylnaphthylsulfonium trifluoromethanesulfonate, preferably at least one selected from triphenylsulfonium trifluoromethanesulfonate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium antimonate, methyldiphenyliodonium trifluoromethanesulfonate, di-tert-butyldiphenyliodonium trifluoromethanesulfonate, triphenylsulfonium perfluorobutylsulfonate, methylbiphenyliodonium perfluorobutyl, triphenylsulfonium perfluorooctanesulfonate and trifluoromethanesulfonic acid diaryliodonium salt.
[0036] In the present invention, the crosslinking agent may be any existing substance capable of promoting the crosslinking reaction of the resin, preferably at least one selected from tetramethoxymethyl glycoluril, tetramethoxyethyl glycoluril, tri(2,3-epoxypropyl)isocyanurate and trimethylolpropane triglycidyl ether.
[0037] In the present invention, the acid diffusion inhibitor can be any of the existing substances that can inhibit acid diffusion, and specific examples thereof include but are not limited to at least one of methyltriamine, ethyltriamine, dimethylamine, diethylamine, trimethylamine, triethylamine, tributylamine, methanoltriamine, ethanoltriamine, dimethanolamine and triethanolamine.
[0038] In the present invention, the solvent may be any existing inert liquid medium that can dissolve or evenly disperse resin A, resin B, acid generator, crosslinking agent, and acid diffusion inhibitor, and may be selected from at least one of ether solvents, aromatic hydrocarbon solvents, ester solvents, and ketone solvents. Among them, ether solvents may be, for example, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, etc. Aromatic hydrocarbon solvents may be, for example, toluene, xylene, etc. Ester solvents may be, for example, propylene glycol methyl ether acetate, butyl acetate, ethyl lactate, etc. Ketone solvents may be, for example, 2-heptanone, etc.
[0039] The preparation method of the KrF negative photoresist provided by the present invention comprises uniformly mixing resin A, resin B, an acid generator, a cross-linking agent, an acid diffusion inhibitor and a solvent. The mixing method can be carried out in any order, which will not be described in detail herein.
[0040] The patterning method provided by the present invention comprises forming a photoresist layer on a substrate with the above-mentioned KrF negative photoresist, then exposing the photoresist layer to a light source with a wavelength of 248nm through a mask, and then developing to form a photoresist pattern. The main improvement of the patterning method provided by the present invention is that a new KrF negative photoresist is used, and other conditions such as the material of the substrate, the method of forming the photoresist layer, the conditions of exposure and development, etc. can be conventionally selected in the art, which can be known to those skilled in the art and will not be described in detail here.
[0041] The present invention will be described in detail below through examples.
[0042] Synthesis Example 1 Synthesis of Resin A
[0043] 10 g of p-hydroxystyrene, 10 g of styrene, 5 g of maleic anhydride and 0.5 g of AIBN were weighed and dissolved in a mixed solvent consisting of 30 g of tetrahydrofuran and 20 g of methyl ethyl ketone, and the mixture was stirred at 60° C. for 8 h. After the reaction was completed, the reaction product was precipitated in ether and then filtered. The solid was dried at 70° C. under vacuum conditions for 48 h to obtain a p-hydroxystyrene-styrene-maleic anhydride copolymer with a weight average molecular weight of 12,000, namely resin A, denoted as A1.
[0044] Synthesis Example 2 Synthesis of Resin A
[0045] 8 g of p-hydroxystyrene, 6 g of styrene, 8 g of maleic anhydride and 0.5 g of AIBN were weighed and dissolved in a mixed solvent consisting of 30 g of tetrahydrofuran and 20 g of methyl ethyl ketone, and the mixture was stirred at 60° C. for 8 h. After the reaction was completed, the reaction product was precipitated in ether and then filtered. The solid was dried at 70° C. under vacuum conditions for 48 h to obtain a p-hydroxystyrene-styrene-maleic anhydride copolymer with a weight average molecular weight of 8900, namely resin A, denoted as A2.
[0046] Synthesis Example 3 Synthesis of Resin B
[0047] Slowly dissolve 3.2023 g of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl in 5 mL of concentrated sulfuric acid and stir until clear to obtain a 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl concentrated sulfuric acid solution. Add 170 g of NaNO2 to the 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl concentrated sulfuric acid at low temperature (0-5°C) while stirring, then stir and mix the two, place the mixed solution in a low temperature tank, control the temperature at -5°C, stir for 10 minutes, and let stand for 2 hours. Then the mixed solution was slowly added to a three-necked flask and heated under reflux for 3 hours, cooled naturally to room temperature, a solid mixture was precipitated, the supernatant was removed, the solid mixture was washed with water three times, 0.2L CHCl3 was added, heated under reflux until completely dissolved, and then 5g of anhydrous MgSO4 was added to remove moisture and allowed to stand for 2 hours. The standing product was filtered and rotary evaporated, and the rotary evaporated product was filtered again and dried to obtain 2,2'-bis(trifluoromethyl)-4,4'-dihydroxybiphenyl, which was then cyanated with cyanogen bromide to obtain cyanate, i.e., resin B, denoted as B1, whose structural formula is shown in the following formula (5).
[0048]
[0049] Synthesis Example 4 Synthesis of Resin B
[0050] Slowly dissolve 3.3426 g of 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether in 5 mL of concentrated sulfuric acid and stir until clear to obtain a 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether concentrated sulfuric acid solution. Add 170 g of NaNO2 to the 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether concentrated sulfuric acid at low temperature (0-5°C) while stirring, then stir and mix the two, place the mixed solution in a low temperature tank, control the temperature at -5°C, stir for 10 minutes, and let stand for 2 hours. Then the mixed solution was slowly added to a three-necked flask and heated under reflux for 3 hours, cooled naturally to room temperature, a solid mixture was precipitated, the supernatant was removed, the solid mixture was washed with water three times, 0.2L CHCl3 was added, heated under reflux until completely dissolved, and then 5g of anhydrous MgSO4 was added to remove moisture and allowed to stand for 2 hours. The standing product was filtered and rotary evaporated, and the rotary evaporated product was filtered again and dried to obtain 2,2'-bis(trifluoromethyl)-4,4'-dihydroxydiphenyl ether, which was then cyanated with cyanogen bromide to obtain cyanate, i.e., resin B, denoted as B2, and its structural formula is shown in the following formula (8).
[0051]
[0052] Example 1
[0053] Mix 50g of resin A1, 10g of resin B1, 2g of triphenylsulfonium trifluoromethanesulfonate (photoacid generator), 8g of tetramethoxymethyl glycoluril (cross-linker), 0.8g of triethylamine (acid diffusion inhibitor), and 200g of propylene glycol methyl ether acetate (solvent), place on a shaker to mix at a uniform speed for 24h in the dark, filter with a 0.1μm organic microporous filter membrane after mixing evenly, and obtain KrF negative photoresist.
[0054] Example 2
[0055] A KrF negative photoresist was prepared by referring to the method of Example 1, except that resin A1 was replaced by resin A2 of the same mass, and the other conditions were the same as those of Example 1, to obtain a KrF negative photoresist.
[0056] Example 3
[0057] A KrF negative photoresist was prepared by referring to the method of Example 1, except that the amount of resin A1 used was 40 g, and the other conditions were the same as those of Example 1, to obtain a KrF negative photoresist.
[0058] Example 4
[0059] A KrF negative photoresist was prepared by referring to the method of Example 1, except that the amount of resin A1 used was 30 g, and the other conditions were the same as those of Example 1, to obtain a KrF negative photoresist.
[0060] Example 5
[0061] Mix 50g of resin A1, 10g of resin B2, 2g of triphenylsulfonium trifluoromethanesulfonate (photoacid generator), 8g of tri(2,3-epoxypropyl)isocyanurate (cross-linker), 0.8g of diethylamine (acid diffusion inhibitor), and 200g of propylene glycol methyl ether acetate (solvent), place on a shaker to mix at a uniform speed for 24h in the dark, filter with a 0.1μm organic microporous filter membrane after mixing evenly, and obtain KrF negative photoresist.
[0062] Example 6
[0063] Mix 50g of resin A2, 10g of resin B2, 2g of triphenylsulfonium trifluoromethanesulfonate (photoacid generator), 8g of trimethylolpropane triglycidyl ether (cross-linker), 0.8g of triethylamine (acid diffusion inhibitor), and 200g of propylene glycol methyl ether acetate (solvent), place on a shaker to mix at a uniform speed for 24h in the dark, filter with a 0.1μm organic microporous filter membrane after mixing evenly, and obtain KrF negative photoresist.
[0064] Comparative Example 1
[0065] A KrF negative photoresist was prepared according to the method of Example 1, except that the resin B1 was replaced by the same weight portion of the resin A1, and the other conditions were the same as those of Example 1, to obtain a reference KrF negative photoresist.
[0066] Comparative Example 2
[0067] A KrF negative photoresist was prepared according to the method of Example 6, except that the resin B2 was replaced by the same weight portion of the resin A2. The other conditions were the same as those of Example 6, to obtain a reference KrF negative photoresist.
[0068] Test Case
[0069] The KrF negative photoresists obtained in Examples 1 to 6 and the reference KrF negative photoresists obtained in Comparative Examples 1 to 4 were spin-coated on an 8-inch silicon wafer, and then pre-baked at 100° C. for 90 seconds to form a 1.2 μm thick photoresist layer, which was then exposed under an exposure machine (exposure wavelength 248 nm), dried at 100° C. for 90 seconds after exposure, and then developed in 2.38% TMAH.
[0070] (1) Resolution and sensitivity:
[0071] After the photoresist is developed, the resolution of the space area where line / space=1 / 1 is tested using a scanning electron microscope CDSEM (CG6300). Sensitivity is measured by determining the energy (Energy) of the minimum line width (resolution). The results of the obtained resolution and sensitivity are shown in Table 1. Among them, the resolution of the pattern formed after the development of the KrF negative photoresist obtained in Example 1 at line / space=1 / 1 is shown in the figure below. Figure 1 shown.
[0072] Table 1
[0073] serial number Resolution(nm) <![CDATA[Sensitivity (mJ / cm 2 )]]> Example 1 150nm 26 Example 2 170nm 28 Example 3 165nm 27 Example 4 160nm 30 Example 5 170nm 27 Example 6 168nm 29 Comparative Example 1 210nm 35 Comparative Example 2 220nm 38
[0074] (2) Heat resistance:
[0075] After the photoresist is developed, the obtained photoresist pattern is baked at 110°C, 120°C and 130°C for 120s, and the changes in the pattern morphology are observed. The results of the pattern are shown in Table 2, where "○" indicates a good pattern morphology and "X" indicates a collapsed pattern.
[0076] Table 2
[0077] serial number temperature Graphics temperature Graphics temperature Graphics Example 1 110℃ ○ 120℃ ○ 130℃ ○ Example 2 110℃ ○ 120℃ ○ 130℃ ○ Example 3 110℃ ○ 120℃ ○ 130℃ ○ Example 4 110℃ ○ 120℃ ○ 130℃ ○ Example 5 110℃ ○ 120℃ ○ 130℃ ○ Example 6 110℃ ○ 120℃ ○ 130℃ ○ Comparative Example 1 110℃ ○ 120℃ X 130℃ X Comparative Example 2 110℃ ○ 120℃ X 130℃ X
[0078] From Table 1 and Table 2 and Figure 1It can be seen from the results that the KrF negative photoresist provided by the present invention has an inverted trapezoidal morphology, and has high resolution, high sensitivity and good heat resistance. The pattern formed at high temperature does not deform or collapse, and has broad application prospects.
[0079] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.
Claims
1. A KrF negative photoresist, It is characterized in that The KrF negative photoresist contains resin A, resin B, an acid generator, a crosslinking agent, an acid diffusion inhibitor and a solvent, wherein the resin A is a hydroxystyrene-styrene-maleic anhydride copolymer having a structure shown in formula (I), and the resin B is a diisocyanate resin having a structure shown in formula (II); NCO-R-OCN formula (Ⅱ), In formula (I), x is 20% to 40%, y is 20% to 45%, z is 20% to 50%, and x+y+z is 100%; in formula (II), R is a biphenyl group or a phenoxyphenyl group, and each benzene ring in the biphenyl group and the phenoxyphenyl group has a hydrogen atom substituted by a trifluoromethyl group.
2. The KrF negative photoresist according to claim 1, It is characterized in that Based on the total weight of the KrF negative photoresist, the content of the resin A is 10% to 50%, the content of the resin B is 2% to 10%, the content of the acid generator is 0.1% to 10%, the content of the cross-linking agent is 0.1% to 5%, the content of the acid diffusion inhibitor is 0.01% to 5%, and the balance is solvent.
3. The KrF negative photoresist according to claim 1, It is characterized in that The mass ratio of the resin A to the resin B is (2-6):
1.
4. The KrF negative photoresist according to any one of claims 1 to 3, It is characterized in that The weight average molecular weight of the resin A is 5,000 to 20,000.
5. The KrF negative photoresist according to any one of claims 1 to 3, It is characterized in that R has at least one of the structures shown in formula (1) to formula (4):
6. The KrF negative photoresist according to any one of claims 1 to 3, It is characterized in that The acid generator is selected from at least one of triphenylsulfonium trifluoromethanesulfonate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium antimonate, methyldiphenyliodonium trifluoromethanesulfonate, di-tert-butyldiphenyliodonium trifluoromethanesulfonate, triphenylsulfonium perfluorobutylsulfonate, methylbiphenyliodonium perfluorobutylsulfonate, triphenylsulfonium perfluorooctanesulfonate and trifluoromethanesulfonic acid diaryliodonium salt.
7. The KrF negative photoresist according to any one of claims 1 to 3, It is characterized in that The crosslinking agent is at least one selected from tetramethoxymethyl glycoluril, tetramethoxyethyl glycoluril, tri(2,3-epoxypropyl)isocyanurate and trimethylolpropane triglycidyl ether.
8. The KrF negative photoresist according to any one of claims 1 to 3, It is characterized in that The acid diffusion inhibitor is selected from at least one of methyltriamine, ethyltriamine, dimethylamine, diethylamine, trimethylamine, triethylamine, tributylamine, methanoltriamine, ethanoltriamine, dimethanolamine and triethanolamine.
9. A method for preparing the KrF negative photoresist according to any one of claims 1 to 8, It is characterized in that The method comprises uniformly mixing resin A, resin B, an acid generator, a cross-linking agent, an acid diffusion inhibitor and a solvent.
10. A patterning method, It is characterized in that The method comprises forming a photoresist layer on a substrate using the KrF negative photoresist described in any one of claims 1 to 8, exposing the photoresist layer through a mask using a light source with a wavelength of 248 nm, and then developing to form a photoresist pattern.