Cable filling rope and preparation method thereof

The cable filling rope processed by polymerization and microwave curing technology solves the deficiencies of existing cable filling ropes in solvent resistance, high temperature resistance and mechanical properties, achieves higher tear resistance and high temperature resistance, and extends the service life.

CN118824641APending Publication Date: 2024-10-22ANHUI KENUO NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410814273.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing cable filling ropes have deficiencies in solvent resistance, high temperature resistance and mechanical properties, resulting in short service life and flammability in high temperature environments.

Method used

Polypropylene, methyl acrylate and hydroxypropyl methylcellulose are used as raw materials, heat stabilizers, plasticizers and toughening agents are added for copolymerization. The modified base material is formed through microwave curing technology and is processed in a twin-screw extruder. Melt blending and granulation are carried out in the process to form a cable filling rope with high tear resistance and high temperature resistance.

Benefits of technology

The solvent resistance, high temperature resistance and tear resistance of the cable filling rope are improved to ensure the stability and service life of the material in high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the technical field of cable manufacturing, and particularly relates to a preparation method of a cable filling rope. The method comprises the following steps: 1) pre-polymerizing raw materials, adding a heat stabilizer, a plasticizer and a flexibilizer, uniformly mixing, and adding an initiator for copolymerization to obtain a carrier; 2) uniformly mixing a carrier, a modifier and a solvent, adding an amino compound in a microwave environment, uniformly mixing, and reacting to obtain a modified base material; and (3) adding the modified base material into a double-screw extruder, carrying out melt blending and granulation, and carrying out net opening and rolling to obtain the cable filling rope. The cable filling rope prepared by the invention has better solvent resistance and high temperature resistance, can ensure normal operation of a cable at a higher use temperature, also has tear resistance, and is convenient to process and use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of filling rope manufacturing, and in particular relates to a method for preparing a cable filling rope. Background Art

[0002] With the global economic integration and rapid development of science and technology, the wire and cable industry, as the "blood vessels" of energy transmission and information exchange, has attracted much attention for its development trend. With the acceleration of global industrialization and urbanization, the rise of the new energy revolution and the digital economy, the wire and cable industry has ushered in a historical opportunity for development. Wires and cables are mainly used to transmit electrical energy, transmit information, manufacture motors, manufacture instruments and equipment, and realize electromagnetic energy conversion. They are widely used in power, rail transportation, new energy, construction, ships, communications, petrochemicals, automobiles and other fields.

[0003] Cable filling rope is a filling material commonly used in the cable manufacturing process. Its main function is to maintain the roundness of the cable and improve the appearance quality of the finished product. The filling rope can fill the gap inside the cable, so that the cable core wire maintains a good round state, thereby achieving a high roundness. At present, the cable filling ropes on the market are made of PVC, PE, silicone rubber, etc. PVC cables have very good flame retardant properties and can meet the flame retardant levels specified by various standards. Insoluble thermosetting plastics can be formed through radiation cross-linking, which has a stable molecular structure, high mechanical strength and good high temperature resistance. However, it has poor acid and alkali resistance and solvent resistance. Under certain conditions, similar dissolution will occur, and the service life is short. If combustion occurs, a large amount of thick smoke will be emitted, causing serious harm to the environment. Therefore, it is necessary to develop a low-smoke halogen-free cable filling rope. Although PE cables can improve chemical resistance, their high temperature resistance is poor. Silicone rubber cable filling rope has good high temperature resistance. According to the research of technicians in this field, it can be used stably at 200℃ and can be used for a period of time at 350℃. However, its tear resistance is poor and it is easily damaged by external forces during processing and use. In addition, the vulcanizing agent contains halogen, which has requirements on the production environment temperature and high preparation cost. Therefore, there is an urgent need for a cable filling rope that is resistant to acid and alkali corrosion, solvents, high temperature and tearing. Summary of the invention

[0004] Based on the above content, in order to solve the problems of poor solvent resistance, poor high temperature resistance and insufficient mechanical properties of the cable filling rope, the present invention proposes a method for preparing the cable filling rope.

[0005] The objects of the present invention are:

[0006] 1. Ensure that the cable filler rope is solvent resistant;

[0007] 2. Improve the high temperature resistance of cable filling rope;

[0008] 3. Improve the tear resistance of cable filling rope.

[0009] To achieve the above objectives, the present invention adopts the following technical solutions.

[0010] A method for preparing a cable filling rope,

[0011] The method comprises:

[0012] 1) Prepolymerize the raw materials, add a heat stabilizer, a plasticizer, and a toughening agent, mix them evenly, and then add an initiator to copolymerize to obtain a carrier;

[0013] 2) mixing the carrier, the modifier and the solvent evenly, adding the amino compound under a microwave environment and mixing evenly, and reacting to obtain a modified substrate;

[0014] 3) adding the modified substrate into a twin-screw extruder for melt blending and granulation, and then opening the net and winding the net to obtain the cable filling rope.

[0015] As a preference,

[0016] Step 1) The raw materials are polypropylene, methyl acrylate, and hydroxypropyl methylcellulose;

[0017] The polypropylene, methyl acrylate and hydroxypropyl methylcellulose are prepared in a mass ratio of 2: (4.78-9.56): (4-5).

[0018] As a preference,

[0019] The prepolymerization in step 1) is carried out at a temperature of 85 to 90° C. and a constant temperature of 0.5 to 1 hour.

[0020] As a preference,

[0021] Step 1) The heat stabilizer is stearyl benzoyl methane, and its dosage is 0.05-0.1 g / g raw material;

[0022] Step 1) The plasticizer is tributyl acetyl citrate, and its dosage is 0.5-0.8 mL / g raw material;

[0023] Step 1) The toughening agent is nano calcium carbonate, and its dosage is 0.2-0.3 g / g raw material;

[0024] The initiator in step 1) is dodecyl peroxide, and its usage is 0.01-0.03 g / g raw material.

[0025] As a preference,

[0026] The copolymerization in step 1) is carried out at a constant temperature of 85 to 90° C. for 5 to 10 hours.

[0027] As a preference,

[0028] Step 2) the modifier is hydrogenated abietic alcohol, and the amount thereof is 0.2-0.3 mL / g carrier;

[0029] Step 2) The solvent is tetrahydrofuran, and its usage is 0.4-0.6 mL / g carrier.

[0030] As a preference,

[0031] The parameters of the microwave environment in step 2) are as follows:

[0032] The frequency is 0.8~1.2GHz and the wavelength is 30~40cm.

[0033] As a preference,

[0034] Step 2) the amino compound is triethylamine, and its usage is 0.08-0.15 mL / g carrier;

[0035] Step 2) The reaction time is 10 to 20 minutes.

[0036] A cable filler rope.

[0037] The present invention uses polypropylene, methyl acrylate and hydroxypropyl methylcellulose as raw materials for polymerization. Hydroxypropyl methylcellulose is a nonionic water-soluble polymer, which provides abundant grafting sites. Hydroxypropyl methylcellulose is grafted with polypropylene and methyl acrylate, and stearoyl benzoyl methane and acetyl tributyl citrate are used to introduce aromatic heterocyclic structures into the molecular long chain, thereby improving its mechanical properties and thermal stability. The present invention uses two monomers for polymerization, and polypropylene and methyl acrylate form a copolymer through a cross-linked structure between molecular chains. After characterization, the copolymer has an orthogonal and monoclinic crystal structure. As the methyl acrylate in the copolymer gradually increases, the methyl acrylate will play an "internal lubrication" effect inside the copolymer, which can promote better compatibility between polypropylene and hydroxypropyl methylcellulose molecules, reduce the molecular chain forces of the copolymer, thereby improving the stretching and activity of the molecular chains, and can effectively improve the mechanical properties of the cable filling rope. However, due to the weakening effect of methyl acrylate on the molecular chain forces of the copolymer, if the proportion of methyl acrylate in the copolymer continues to increase, the tear strength of the cable filling rope will gradually decrease. If the methyl acrylate component is excessive, a large number of unsaturated carbon-carbon double bonds and hydroxyl groups will be generated inside the copolymer at a higher temperature, which will destroy the copolymer's crystallization ability and lead to a decrease in the thermal stability of the cable filling rope. If the polypropylene content is too high, the thermal oxidation effect will lead to crosslinking between the molecular chains inside the copolymer and possible molecular chain scission, resulting in dislocation and irregular molecular friction in the internal structure of the carrier material at a higher temperature, which will lead to a decrease in the thermal stability of the cable filling rope.

[0038] The interfacial adhesion performance has a significant impact on the physical structure and mechanical properties of the material. Modifying the surface of the material can effectively improve the interfacial bonding of the material. Introducing the rosin structure into the molecular side chain can significantly improve the hardness and adhesion strength of the material. Hydrogenated rosin alcohol is a rosin derivative that has been hydrogenated. Its molecular structure retains the reactive carboxyl group, while the double bond content is significantly reduced. Its molecular structure has a large spatial volume, which improves the rigid molecular chain. The synergistic effect of the above-mentioned modification additives can avoid the excessive unsaturated double bond structure affecting the aging resistance of the material.

[0039] The present invention uses a synergistic acid-binding agent triethylamine to rearrange the modified material on the fiber surface through microwave curing, strengthen the structural characteristics of the fiber material, and ensure that the modified auxiliary agent and hydroxypropyl methylcellulose fully cross-link. During the microwave process, the polar groups move freely, the molecular chain segments are extended, and when the material surface is close to being completely cured, the macromolecular segments are cross-linked to form a complex three-dimensional network structure. In a smaller space, a dendritic structure with nano calcium carbonate as the central particle is formed. This structure allows the molecular chains to form a fiber-condensed particle system, and at this time the system tends to aggregate, the density increases, and the tensile strength of the material is improved. In addition, the microwave curing method can ensure the stability of the material thermal curing process, avoid stress gradients inside the material, and avoid bending and cracking of the material.

[0040] The beneficial effects of the present invention are as follows:

[0041] (1) The cable filling rope prepared by the present invention has good solvent resistance;

[0042] (2) The cable filling rope prepared by the present invention is resistant to high temperatures and can ensure the normal operation of the cable at higher operating temperatures;

[0043] (3) The cable filling rope prepared by the present invention is tear-resistant and easy to process and use. DETAILED DESCRIPTION

[0044] The present invention is further described in detail below in conjunction with specific embodiments and the specification. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0045] Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0046] Example 1

[0047] A method for preparing a cable filling rope, the method comprising:

[0048] 1) 2 g of polypropylene, 4.78 g (5 mL) of methyl acrylate, and 4 g of hydroxypropyl methylcellulose were taken, kept at a constant temperature of 85° C. for 1 h, 1 g of stearylbenzoylmethane, 8.5 mL of acetyl tributyl citrate, and 3.2 g of nano calcium carbonate were added and mixed evenly, and then 0.3 g of dodecyl peroxide was added, and kept at a constant temperature of 90° C. for 5 h to obtain a carrier;

[0049] 2) preparing a carrier, hydrogenated abietic alcohol, and tetrahydrofuran in a ratio of 15 g: 4 mL: 8 mL and mixing them evenly, adding 1.5 mL of triethylamine and mixing them evenly under a microwave environment with a frequency of 1 GHz and a wavelength of 30 cm, and reacting for 20 minutes to obtain a modified substrate;

[0050] 3) adding the modified substrate into a twin-screw extruder for melt blending and granulation, and then opening the net and winding the net to obtain the cable filling rope.

[0051] The cable filling rope prepared in this example was subjected to technical index tests and performance tests, wherein the technical index tests included tensile strength and elongation at break, and the performance tests were as follows.

[0052] 1. Tear strength:

[0053] The cable filling rope is torn longitudinally with a certain force, the maximum stress that the cable filling rope can withstand is measured and the tearing strength is calculated.

[0054] 2.Solvent resistance:

[0055] In an environment with a temperature of 25°C and a humidity of 50-60%, 10g of cable filling rope was immersed in an ethanol dispersion of oil for 120 hours. After being taken out, it was cleaned, dried, weighed, and its mass change was calculated.

[0056] 3. High temperature resistance:

[0057] Place the cable filling rope at a constant temperature of 150℃ for 1 hour and test its technical indicators. If the performance is not lower than 20% of the material before the test, continue to increase the temperature by 10℃ each time and keep the temperature constant for 1 hour until the performance is lower than the standard and bending, cracking, etc. appear. Record the material's maximum working temperature.

[0058] The results are as follows.

[0059]

[0060] According to the results in the table, the material of the present invention has good mechanical properties such as tensile strength and tear resistance, as well as good solvent resistance and high temperature resistance. The material has good interface bonding and no obvious cracks appear after long-term use. Characterization shows that obvious structural changes occur inside the material.

[0061] Example 2

[0062] A method for preparing a cable filling rope, the method comprising:

[0063] 1) 2 g of polypropylene, 7.85 g (7.5 mL) of methyl acrylate, and 4 g of hydroxypropyl methylcellulose were taken, kept at a constant temperature of 85° C. for 1 h, 1 g of stearylbenzoylmethane, 8.5 mL of acetyl tributyl citrate, and 3.2 g of nano calcium carbonate were added and mixed evenly, and then 0.3 g of dodecyl peroxide was added, and kept at a constant temperature of 90° C. for 5 h to obtain a carrier;

[0064] 2) preparing a carrier, hydrogenated abietic alcohol, and tetrahydrofuran in a ratio of 15 g: 4 mL: 8 mL and mixing them evenly, adding 1.5 mL of triethylamine and mixing them evenly under a microwave environment with a frequency of 1 GHz and a wavelength of 30 cm, and reacting for 20 minutes to obtain a modified substrate;

[0065] 3) adding the modified substrate into a twin-screw extruder for melt blending and granulation, and then opening the net and winding the net to obtain the cable filling rope.

[0066] The cable filling rope prepared in this example was subjected to the same technical index test and performance test as in Example 1, and the results are as follows.

[0067]

[0068] The present invention uses two monomers for polymerization, and a copolymer is formed between polypropylene and methyl acrylate through a cross-linked structure between molecular chains. According to the results in the table, as the methyl acrylate in the copolymer gradually increases, the methyl acrylate will play an "internal lubrication" effect inside the copolymer, which can promote better compatibility between polypropylene and hydroxypropyl methylcellulose molecules, reduce the interaction between the molecular chains of the copolymer, thereby improving the stretching and activity of the molecular chains, and can effectively improve the mechanical properties of the cable filling rope.

[0069] Example 3

[0070] A method for preparing a cable filling rope, the method comprising:

[0071] 1) 2 g of polypropylene, 9.56 g (10 mL) of methyl acrylate, and 4 g of hydroxypropyl methylcellulose were taken, kept at a constant temperature of 85° C. for 1 h, 1 g of stearylbenzoylmethane, 8.5 mL of acetyl tributyl citrate, and 3.2 g of nano calcium carbonate were added and mixed evenly, and then 0.3 g of dodecyl peroxide was added, and kept at a constant temperature of 90° C. for 5 h to obtain a carrier;

[0072] 2) preparing a carrier, hydrogenated abietic alcohol, and tetrahydrofuran in a ratio of 15 g: 4 mL: 8 mL and mixing them evenly, adding 1.5 mL of triethylamine and mixing them evenly under a microwave environment with a frequency of 1 GHz and a wavelength of 30 cm, and reacting for 20 minutes to obtain a modified substrate;

[0073] 3) adding the modified substrate into a twin-screw extruder for melt blending and granulation, and then opening the net and winding the net to obtain the cable filling rope.

[0074] The cable filling rope prepared in this example was subjected to the same technical index test and performance test as in Example 1, and the results are as follows.

[0075]

[0076] In this case, a high content of polymethyl acrylate is formed. Due to the weakening effect of methyl acrylate on the inter-chain interaction of copolymer molecules, the tear strength of the cable filling rope is reduced. Moreover, at higher temperatures, a large number of unsaturated carbon-carbon double bonds and hydroxyl groups will be generated inside the copolymer, which will destroy the crystallization ability of the copolymer, thereby reducing the thermal stability of the cable filling rope.

[0077] Comparative Example 1

[0078] A method for preparing a cable filling rope, the method comprising:

[0079] 1) 2 g of polypropylene, 7.85 g (7.5 mL) of methyl acrylate, and 4 g of commercially available non-woven fabric filaments were taken, kept at a constant temperature of 85° C. for 1 h, 1 g of stearylbenzoylmethane, 8.5 mL of acetyl tributyl citrate, and 3.2 g of nano calcium carbonate were added and mixed evenly, and then 0.3 g of dodecyl peroxide was added, and kept at a constant temperature of 90° C. for 5 h to obtain a carrier;

[0080] 2) preparing a carrier, hydrogenated abietic alcohol, and tetrahydrofuran in a ratio of 15 g: 4 mL: 8 mL and mixing them evenly, adding 1.5 mL of triethylamine and mixing them evenly under a microwave environment with a frequency of 1 GHz and a wavelength of 30 cm, and reacting for 20 minutes to obtain a modified substrate;

[0081] 3) adding the modified substrate into a twin-screw extruder for melt blending and granulation, and then opening the net and winding the net to obtain the cable filling rope.

[0082] The cable filling rope prepared in this example was subjected to the same technical index test and performance test as in Example 1, and the results are as follows.

[0083]

[0084] The cotton and linen filaments produced by Jintong are used in the present invention. Compared with Example 2, the grafting sites are insufficient, the modification effects of the monomers, stearylbenzoylmethane and acetyl tributyl citrate are limited, and the mechanical properties and thermal stability of the material are insufficient.

[0085] Comparative Example 2

[0086] A method for preparing a cable filling rope, the method comprising:

[0087] 1) 2 g of polypropylene, 3.14 g (3 mL) of methyl acrylate, and 4 g of hydroxypropyl methylcellulose were taken, kept at a constant temperature of 85° C. for 1 h, 1 g of stearylbenzoylmethane, 8.5 mL of acetyl tributyl citrate, and 3.2 g of nano calcium carbonate were added and mixed evenly, and then 0.3 g of dodecyl peroxide was added, and kept at a constant temperature of 90° C. for 5 h to obtain a carrier;

[0088] 2) preparing a carrier, hydrogenated abietic alcohol, and tetrahydrofuran in a ratio of 15 g: 4 mL: 8 mL and mixing them evenly, adding 1.5 mL of triethylamine and mixing them evenly under a microwave environment with a frequency of 1 GHz and a wavelength of 30 cm, and reacting for 20 minutes to obtain a modified substrate;

[0089] 3) adding the modified substrate into a twin-screw extruder for melt blending and granulation, and then opening the net and winding the net to obtain the cable filling rope.

[0090] The cable filling rope prepared in this example was subjected to the same technical index test and performance test as in Example 1, and the results are as follows.

[0091]

[0092] In this case, the polypropylene content is too high, which will lead to cross-linking between the internal molecular chains of the copolymer and possible molecular chain scission under the effect of thermal oxidation, resulting in dislocation and irregular molecular friction in the internal structure of the carrier material at a higher temperature, thereby causing a decrease in the thermal stability of the cable filling rope.

[0093] Comparative Example 3

[0094] A method for preparing a cable filling rope, the method comprising:

[0095] 1) 2 g of polypropylene, 7.85 g (7.5 mL) of methyl acrylate, and 4 g of hydroxypropyl methylcellulose were taken, kept at a constant temperature of 85° C. for 1 h, 1 g of stearylbenzoylmethane, 8.5 mL of acetyl tributyl citrate, and 3.2 g of nano calcium carbonate were added and mixed evenly, and then 0.3 g of dodecyl peroxide was added, and kept at a constant temperature of 90° C. for 5 h to obtain a carrier;

[0096] 2) preparing a carrier and tetrahydrofuran in a ratio of 15 g:8 mL and mixing them evenly, adding 1.5 mL of triethylamine and mixing them evenly under a microwave environment with a frequency of 1 GHz and a wavelength of 30 cm, and reacting for 20 minutes to obtain a modified substrate;

[0097] 3) adding the modified substrate into a twin-screw extruder for melt blending and granulation, and then opening the net and winding the net to obtain the cable filling rope.

[0098] The cable filling rope prepared in this example was subjected to the same technical index test and performance test as in Example 1, and the results are as follows.

[0099]

[0100]

[0101] In this example, no hydrogenated rosin alcohol is added. Compared with the material in Example 2, the double bond content is higher, which makes it easy to break the bonds during use. At the same time, the molecular structure has a smaller spatial volume, the molecular chain has greater rigidity, and the tensile strength is lower.

[0102] Comparative Example 4

[0103] A method for preparing a cable filling rope, the method comprising:

[0104] 1) 2 g of polypropylene, 7.85 g (7.5 mL) of methyl acrylate, and 4 g of hydroxypropyl methylcellulose were taken, kept at a constant temperature of 85° C. for 1 h, 1 g of stearylbenzoylmethane, 8.5 mL of acetyl tributyl citrate, and 3.2 g of nano calcium carbonate were added and mixed evenly, and then 0.3 g of dodecyl peroxide was added, and kept at a constant temperature of 90° C. for 5 h to obtain a carrier;

[0105] 2) Prepare a carrier, hydrogenated rosin alcohol, and tetrahydrofuran in a ratio of 15 g: 4 mL: 8 mL and mix them evenly, add 1.5 mL of triethylamine and mix evenly, heat to 50° C. and react for 20 min to obtain a modified substrate;

[0106] 3) adding the modified substrate into a twin-screw extruder for melt blending and granulation, and then opening the net and winding the net to obtain the cable filling rope.

[0107] The cable filling rope prepared in this example was subjected to the same technical index test and performance test as in Example 1, and the results are as follows.

[0108]

[0109] In this case, there is not enough energy to rearrange the molecular chains, the material itself is not strong enough, the three-dimensional network structure is easily destroyed, and the material is not dense enough, resulting in a significant decrease in tensile strength and a significant deterioration in solvent resistance.

Claims

1. A method for preparing a cable filling rope, It is characterized in that The method comprises: 1) Prepolymerize the raw materials, add a heat stabilizer, a plasticizer, and a toughening agent, mix them evenly, and then add an initiator to copolymerize to obtain a carrier; 2) mixing the carrier, the modifier and the solvent evenly, adding the amino compound under a microwave environment and mixing evenly, and reacting to obtain a modified substrate; 3) adding the modified substrate into a twin-screw extruder for melt blending and granulation, and then opening the net and winding the net to obtain the cable filling rope.

2. A method for preparing a cable filling rope according to claim 1, It is characterized in that Step 1) The raw materials are polypropylene, methyl acrylate, and hydroxypropyl methylcellulose; The polypropylene, methyl acrylate and hydroxypropyl methylcellulose are prepared in a mass ratio of 2: (4.78-9.56): (4-5).

3. A method for preparing a cable filling rope according to claim 1 or 2, It is characterized in that The prepolymerization in step 1) is carried out at a temperature of 85 to 90° C. and a constant temperature of 0.5 to 1 hour.

4. The method for preparing a cable filling rope according to claim 1, It is characterized in that Step 1) The heat stabilizer is stearyl benzoyl methane, and its dosage is 0.05-0.1 g / g raw material; Step 1) The plasticizer is tributyl acetyl citrate, and its dosage is 0.5-0.8 mL / g raw material; Step 1) The toughening agent is nano calcium carbonate, and its dosage is 0.2-0.3 g / g raw material; The initiator in step 1) is dodecyl peroxide, and its usage is 0.01-0.03 g / g raw material.

5. A method for preparing a cable filling rope according to claim 1 or 4, It is characterized in that The copolymerization in step 1) is carried out at a constant temperature of 85 to 90° C. for 5 to 10 hours.

6. A method for preparing a cable filling rope according to claim 1, It is characterized in that Step 2) the modifier is hydrogenated abietic alcohol, and the amount thereof is 0.2-0.3 mL / g carrier; Step 2) The solvent is tetrahydrofuran, and its usage is 0.4-0.6 mL / g carrier.

7. A method for preparing a cable filling rope according to claim 1 or 6, It is characterized in that The parameters of the microwave environment in step 2) are as follows: The frequency is 0.8~1.2GHz and the wavelength is 30~40cm.

8. The method for preparing a cable filling rope according to claim 1, It is characterized in that Step 2) the amino compound is triethylamine, and its usage is 0.08-0.15 mL / g carrier; Step 2) The reaction time is 10 to 20 minutes.

9. A cable filling rope obtained by the method according to any one of claims 1 to 8.