Temporary bonding and de-bonding method
During the temporary bonding and debonding process of semiconductor devices, pre-baking curing and negative pressure vacuum treatment are used to remove air bubbles, and the thermal expansion coefficient of the carrier is controlled and pyrolytic slip debonding technology is used to solve the problem of wafer thinning during the process. Improves the reliability of the process by eliminating chipping problems caused by loss of support and excessive warpage.
Patent Information
- Application Number
- CN202410884892.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the three-dimensional stacking manufacturing process of semiconductor devices, traditional temporary bonding and debonding technology is difficult to effectively discharge air bubbles in the bonding dielectric layer, causing the wafer to lose support during the thinning process and fragment, and the warpage is too large. Increased risk of fragmentation.
By preparing a bonding dielectric layer on the wafer and performing pre-baking and curing, combined with negative pressure vacuum treatment, the temperature and pressure during the vacuum hot pressing process are adjusted to remove bubbles; the thermal expansion coefficient of the carrier is set to not exceed 60% of the wafer. , and uses pyrolytic slip debonding technology to reduce warpage, and uses porous suction cups for separation and cleaning.
Effectively removes bubbles in the bonding medium layer, avoids uneven thickness and hollowing out, improves wafer support, reduces the risk of fragmentation, and improves the reliability of the temporary bonding and debonding process.
Smart Images

Figure CN118824932A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of semiconductor device preparation, and specifically relates to a temporary bonding and debonding method. Background Art
[0002] As new semiconductor products have higher and higher requirements for the integration and functions of various components, traditional two-dimensional integrated circuits can no longer meet the needs. TSV (Through-Silicon Vias) technology and three-dimensional stacked 3D integration technology have come into being. In order to meet the manufacturing needs of TSV and three-dimensional stacked 3D integration, the thickness of the wafer becomes thinner and thinner after thinning. When the wafer is thinned to 150um, it becomes flexible and easy to deform or warp, making it difficult to carry out subsequent process operations.
[0003] In order to reduce the fragmentation rate in the thinning process, temporary bonding and de-bonding technology is usually used. However, during the temporary bonding process, the bubbles generated in the bonding medium layer cannot be effectively discharged. The bubbles cause the wafer to be unable to be supported during the thinning process and break. In addition, the excessive warping of the bonding sheet after temporary bonding will also cause the wafer to have a greater risk of breakage due to uneven force. Summary of the invention
[0004] The present application provides a temporary bonding and debonding method, which can avoid wafer breakage due to bubbles or excessive warpage during temporary bonding and debonding of wafers, and has high reliability.
[0005] In order to solve the above technical problems, the present application provides a method for temporary bonding and debonding, the method comprising the following steps:
[0006] preparing a bonding dielectric layer on the wafer;
[0007] Pre-baking and curing the wafer and the bonding medium layer, and providing negative pressure vacuum;
[0008] Arranging a carrier on the bonding medium layer, and performing thermal compression bonding on the wafer and the carrier;
[0009] Grinding the wafer to reduce the thickness of the wafer to a preset thickness value;
[0010] A porous suction cup is arranged on the side of the wafer facing away from the carrier, and the wafer and the carrier are subjected to thermal decomposition and sliding debonding to separate the wafer from the carrier;
[0011] Air is blown to the porous suction cup to separate the wafer from the porous suction cup.
[0012] As a further improvement of the present application, the step of preparing a bonding dielectric layer on a wafer includes:
[0013] coating liquid wax or liquid glue on the wafer;
[0014] Controlling the wafer to rotate at a first speed so that the liquid wax or liquid glue is evenly covered on the wafer;
[0015] Allowing the wafer to stand still so that bubbles in the liquid wax or liquid glue can burst;
[0016] The wafer is controlled to rotate at a second speed to form the bonding preparation layer on the wafer; wherein the second speed is greater than the first speed.
[0017] As a further improvement of the present application, the step of thermally pressing the wafer and the carrier comprises:
[0018] The carrier is aligned with a wafer provided with the bonding medium layer, and the wafer and the carrier are bonded by heat pressing; wherein, the temperature, air and pressure during the vacuum heat pressing process are adjusted so that the void bubbles in the bonding medium layer are moved to the edge of the wafer and discharged.
[0019] As a further improvement of the present application, the thermal expansion coefficient of the carrier does not exceed 60% of the thermal expansion coefficient of the wafer.
[0020] As a further improvement of the present application, grinding the wafer to reduce the thickness of the wafer to a preset thickness value includes:
[0021] The wafer is mechanically ground to reduce the thickness of the wafer to 100 μm or less.
[0022] As a further improvement of the present application, a porous suction cup is arranged on the side of the wafer facing away from the carrier, and the wafer and the carrier are subjected to thermal decomposition and sliding debonding to separate the wafer from the carrier, comprising:
[0023] Adsorbing the porous suction cup on the side of the wafer facing away from the carrier, and adsorbing the vacuum suction cup on the side of the carrier facing away from the wafer;
[0024] heating the wafer, the bonding medium layer and the carrier so that the bonding medium layer is heated and melted;
[0025] The carrier is moved in a horizontal direction to separate the wafer from the carrier.
[0026] As a further improvement of the present application, the porous suction cup is adsorbed on the side of the wafer facing away from the carrier through a silicon carbide porous carrier, and the vacuum suction cup is adsorbed on the side of the carrier facing away from the wafer.
[0027] As a further improvement of the present application, after separating the wafer from the carrier, the method further includes:
[0028] The separated wafer is cleaned to remove the residual bonding medium layer on the wafer.
[0029] As a further improvement of the present application, the blowing of the porous suction cup comprises:
[0030] Place the separated wafer and the porous suction cup upside down on dust-free paper or dust-free cloth;
[0031] Blow air through a plurality of air guide holes provided on the porous suction cup to release the vacuum between the wafer and the porous suction cup, so as to separate the wafer from the porous suction cup.
[0032] As a further improvement of the present application, the wafer is a silicon wafer, and the carrier is borosilicate glass.
[0033] The temporary bonding and debonding method provided in the present application has the following beneficial effects:
[0034] The present application prepares a bonding dielectric layer on a wafer, pre-bakes and solidifies the bonding dielectric layer and the wafer, and provides a negative pressure vacuum. By adjusting the temperature, air and pressure during the vacuum hot pressing process, the void bubbles in the bonding dielectric layer are moved to the edge of the wafer for discharge, and the bubbles generated in the center and edge of the bonding dielectric layer can be effectively removed to avoid uneven thickness of the bonding dielectric layer or hollowing caused by the bubbles, resulting in the area with bubbles being unable to support the wafer, causing the wafer to break due to local loss of support during thinning. It can also avoid the infiltration of waste generated during the thinning process due to insufficient edge sealing of the bonding dielectric layer, resulting in unremovable contamination on the wafer surface; the thermal expansion coefficient of the carrier is set to not exceed 60% of the thermal expansion coefficient of the wafer, so as to avoid the subsequent grinding process effect during the wafer thinning process being seriously affected by excessive warping of the bonding sheet, and avoid the subsequent debonding process. The risk of greater breakage due to uneven force is avoided, thereby improving the reliability of the temporary bonding and debonding processes. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only part of the embodiments of the present application, rather than all the embodiments. For ordinary technicians in this field, without paying creative work, other drawings obtained based on these drawings all fall within the scope of protection of this application.
[0036] Figure 1 A flowchart of a temporary bonding and debonding method provided in an embodiment of the present application;
[0037] Figure 2 for Figure 1 A flow chart of preparing a bonding medium layer in the temporary bonding and debonding method shown;
[0038] Figure 3 for Figure 1 A schematic diagram of the structure of the wafer in the temporary bonding and debonding method shown;
[0039] Figure 4 for Figure 2 A schematic diagram of the structure for preparing a bonding dielectric layer is shown;
[0040] Figure 5 Schematic diagram of thermal expansion coefficients of silicon materials and common carrier materials;
[0041] Figure 6 for Figure 5 Schematic diagram of the warpage of the bonded wafer formed by the silicon material and the common carrier material;
[0042] Figure 7 for Figure 1 A schematic diagram of the structure of a bonding sheet formed in the temporary bonding and debonding method shown;
[0043] Figure 8 for Figure 1 A flow chart of separating a wafer and a carrier in the temporary bonding and debonding method shown;
[0044] Fig. 9 for Figure 1 A flow chart of separating a wafer and a porous chuck in a temporary bonding and debonding method;
[0045] Description of reference numerals:
[0046] 1-wafer; 2-bonding dielectric layer; 3-carrier. DETAILED DESCRIPTION
[0047] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0048] In order to make the description of the disclosed content more detailed and complete, the following is an illustrative description of the implementation methods and specific examples of the present application; however, this is not the only form of implementing or applying the specific embodiments of the present application. The implementation methods cover the features of multiple specific embodiments and the method steps and their sequences for constructing and operating these specific embodiments. However, other specific embodiments can also be used to achieve the same or equal functions and step sequences. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0049] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the numbers used in this way can be interchanged where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein.
[0050] In the description of the embodiments of the present application, unless otherwise specified, " / " means or, for example, A / B can mean A or B; "and / or" in the text is merely a description of the association relationship of associated objects, indicating that three relationships may exist, for example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. In addition, in the description of the embodiments of the present application, "multiple" refers to two or more than two, and other quantifiers are similar. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present application, and are not used to limit the present application, and the embodiments of the present application and the features in the embodiments may be combined with each other without conflict.
[0051] Please refer to Figure 1-Figure 9 The present application provides a temporary bonding and debonding method, which can avoid wafer breakage due to bubbles or excessive warpage during temporary bonding and debonding of the wafer, has high reliability, and improves the wafer manufacturing yield.
[0052] Please refer to Figure 1 , is a flow chart of a temporary bonding and debonding method provided in an embodiment of the present application, the method comprising the following steps:
[0053] Step S1: preparing a bonding dielectric layer on a wafer;
[0054] As an optional implementation, please refer to Figure 2 ,for Figure 1 The flowchart of preparing a bonding dielectric layer in the temporary bonding and debonding method shown in the figure, wherein the bonding dielectric layer is prepared on a wafer, comprising:
[0055] Step S10: coating liquid wax or liquid glue on the wafer;
[0056] Step S11: controlling the wafer to rotate at a first speed so that the liquid wax or liquid glue is evenly covered on the wafer;
[0057] Step S12: leaving the wafer to stand to break bubbles in the liquid wax or liquid glue;
[0058] The wafer is controlled to rotate at a second speed to form the bonding preparation layer on the wafer; wherein the second speed is greater than the first speed.
[0059] Exemplarily, the wafer 1 may be in the form of a silicon wafer, and the present application does not further limit the specific thickness of the silicon wafer in this step.
[0060] In the embodiments of this application, please refer to Figure 3 ,for Figure 1 The structural schematic diagram of the wafer in the temporary bonding and debonding method shown in the figure requires preparing a bonding medium layer 2 on the wafer 1. The bonding medium can be first coated on the wafer 1, and the wafer 1 is controlled to rotate at a low speed at a first speed, so that the bonding medium coated on the wafer 1 is evenly spread so that the bonding medium is evenly covered on the wafer.
[0061] Furthermore, the round wafer covered with the bonding medium is allowed to stand still so that the bubbles visible to the naked eye in the bonding medium burst naturally; wherein, the above-mentioned bonding medium can be set to liquid wax or liquid glue, and the present application does not impose further restrictions on the specific selection of the bonding medium.
[0062] Afterwards, the wafer 1 is further controlled to rotate at a second high speed, so that a bonding medium layer 2 having a certain thickness and being uniform is prepared on the wafer 1 .
[0063] It can be understood that the second speed is greater than the first speed. The purpose of setting the first speed is to make the bonding medium evenly cover the wafer, and the purpose of setting the second speed is to make the bonding medium after the bubbles burst be unscrewed at high speed, so as to prepare the required bonding medium layer 2 on the wafer 1, avoiding the appearance of bubbles in the bonding medium layer 2, resulting in uneven thickness of the bonding medium layer 2 or hollowing out.
[0064] Step S2: pre-baking and curing the wafer 1 and the bonding medium layer 2, and providing negative pressure vacuum;
[0065] As an optional implementation, please refer to Figure 4 ,for Figure 2 As shown in the structural schematic diagram of preparing the bonding dielectric layer 2, a certain negative pressure vacuum should be provided when pre-baking and curing the wafer 1 and the bonding dielectric layer 2, so that the bubbles invisible to the naked eye in the bonding dielectric layer 2 are broken by the vacuum and the air pressure difference, thereby avoiding bulging of the bonding dielectric layer 2 due to the presence of the bubbles in the subsequent process.
[0066] It should be noted that the above-mentioned negative pressure cannot be too strong to avoid the violent volatilization of a large amount of volatile diluent in the bonding medium layer 2, thereby generating more and larger foam tissues. The above-mentioned negative pressure needs to be adjusted according to the actual scenario during the preparation process. In principle, the negative pressure needs to cause the bubbles in the bonding medium layer 2 that are invisible to the naked eye to burst, while avoiding the generation of more and larger foam tissues in the bonding medium layer 2. This application does not impose further restrictions on the above-mentioned negative pressure value.
[0067] Step S3: placing a carrier 3 on the bonding medium layer 2, and performing thermocompression bonding on the wafer 1 and the carrier 3;
[0068] As an optional implementation, the above-mentioned thermal compression bonding of the wafer 1 and the carrier 3 includes:
[0069] The carrier 3 is aligned with the wafer 1 provided with the bonding medium layer 2, and the wafer 1 and the carrier 3 are bonded by hot pressing; wherein, the temperature, air and pressure during the vacuum hot pressing process are adjusted so that the void bubbles in the bonding medium layer 2 are moved to the edge of the wafer 1 and discharged.
[0070] In an optional embodiment, when the wafer 1 and the carrier 3 are heat-pressed and bonded, the temperature, air and pressure during the vacuum heat-pressing process need to be adjusted so that the void bubbles in the bonding medium layer 2 move to the edge of the wafer 1 and are discharged.
[0071] Specifically, taking the bonding medium as liquid wax and the formed bonding medium layer 2 as a wax layer as an example, when the temperature during the vacuum hot pressing process is too low, the viscosity of the wax layer will be high and the fluidity will be poor, resulting in the inability of the bubbles and voids to move to the edge of the wafer 1 and be discharged smoothly; when the temperature during the vacuum hot pressing process is too high, the viscosity of the wax layer will be low and the fluidity will be good. The wax layer will be squeezed and overflowed under the action of pressure, resulting in the thickness of the bonding medium layer 2 being thin. The carrier 3 will damage the surface of the wafer 1 due to the thin wax layer. Therefore, in this step, it is necessary to adjust the temperature, vacuum, and pressure to obtain a bonding medium layer 2 that meets a certain thickness and is free of bubbles in the center and the edge.
[0072] The present application can effectively remove bubbles generated in the center and edge of the bonding medium layer 2 through the above-mentioned pre-baking and curing, alignment of the wafer 1 and the carrier 3, and vacuum hot pressing processes, thereby avoiding uneven thickness or hollowing of the bonding medium layer 2 caused by the bubbles, resulting in the area with bubbles being unable to support the wafer 1, causing the wafer 1 to break due to local loss of support during thinning; it can also avoid the infiltration of waste generated during the thinning process due to insufficient sealing of the edge of the bonding medium layer 2, resulting in inremovable contamination on the surface of the wafer 1.
[0073] In principle, the prepared bonding medium layer 2 should evenly cover the surface of the wafer 1 and be firmly and reliably connected to the wafer 1 , and no bubbles or hollows should appear on the bonding medium layer 2 .
[0074] As an optional implementation, the thermal expansion coefficient of the carrier 3 is no more than 60% of the thermal expansion coefficient of the wafer 1 .
[0075] In the embodiment of the present application, it is also necessary to control the WARP (warpage) of the bonding sheet formed by the above-mentioned wafer 1, bonding medium layer 2 and carrier 3 to avoid that the subsequent grinding process effect during the thinning process of the wafer 1 is seriously affected due to excessive warpage, and the subsequent debonding process will also cause a greater risk of breakage due to uneven force. Therefore, it is necessary to select the materials of the wafer 1 and the carrier 3 based on the thermal expansion coefficient.
[0076] Please refer to Figure 5 , which is a schematic diagram of the thermal expansion coefficients of silicon materials and common carrier materials. Since the wafer 1, the bonding medium layer 2 and the carrier 3 have different thermal expansion coefficients, the materials with different thermal expansion coefficients are bonded in pairs, which will cause the wafer 1, the bonding medium layer 2 and the carrier 3 to form a bonded sheet. Under the action of thermodynamics, the wafer 1 is forced to undergo a large warping change by the deformation of the carrier 3. Therefore, it is preferred to select a carrier material with a thermal expansion coefficient close to that of the wafer material in order to effectively reduce the warping of the bonded sheet after bonding.
[0077] Preferably, the thermal expansion coefficient of the carrier 3 needs to be controlled not to exceed 60% of the thermal expansion coefficient of the wafer 1 .
[0078] Please refer to Figure 6 ,for Figure 5 The schematic diagram of the warpage of the bonding wafer formed by the silicon material and the common carrier material is shown. In order to further determine the impact of the difference in thermal expansion coefficients between the wafer material and the carrier material on the warpage of the bonding wafer, the present application selects a 150mm Si wafer 1 for bonding with a common carrier material in the prior art, and detects the warpage of the bonding wafer after bonding.
[0079] in, Figure 6The bonding medium 20260 is a high-temperature bonding glue with a bonding temperature of 260°C; the bonding medium 12160 is a low-temperature bonding glue with a bonding temperature of 160°C; a is sapphire as the carrier material, and high-temperature bonding glue is selected for bonding; b is sapphire as the carrier material, and low-temperature bonding glue is selected for bonding; c is quartz glass as the carrier material, and high-temperature bonding glue is selected for bonding; d is quartz glass as the carrier material, and low-temperature bonding glue is selected for bonding; e is borosilicate glass as the carrier material, and high-temperature bonding glue is selected for bonding; and f is borosilicate glass as the carrier material, and low-temperature bonding glue is selected for bonding.
[0080] Please refer to Figure 7 ,for Figure 1 The schematic diagram of the structure of the bonding sheet formed in the temporary bonding and debonding method shown in FIG. Figure 6 It can be observed that in cf, the warping of the bonded sheet formed after the silicon wafer 1 is bonded with the quartz glass and borosilicate glass is small. However, since quartz glass is harder than borosilicate glass, which is an amorphous inorganic non-metallic material, it has poor stability in a high-temperature environment and is prone to thermal stress cracking during high-temperature debonding. Borosilicate glass has good stability in a high-temperature environment and does not undergo thermal stress cracking during high-temperature debonding. Therefore, the present application preferably uses borosilicate glass as the carrier material for thermal bonding with the silicon wafer 1.
[0081] Furthermore, it can be observed that the thermal expansion coefficient of the silicon wafer 1 is 2.6 / (1×10 -6 .K -1 ), the thermal expansion coefficient of borosilicate glass is 3.3 / (1×10 -6 .K -1 ), the thermal expansion coefficients of the two are closest, and the warping of the bonded sheet after bonding is small. By comparing the thermal expansion coefficients of the two, it is preferred to control the thermal expansion coefficient of the carrier 3 not to exceed 60% of the thermal expansion coefficient of the wafer 1.
[0082] Of course, wafers 1 of other materials can also be selected according to actual preparation requirements, as long as the thermal expansion coefficient of the selected carrier 3 does not exceed 60% of the thermal expansion coefficient of wafer 1. This application does not impose further restrictions on the specific setting materials of wafer 1 and carrier 3, and technical personnel in this field can make corresponding adjustments according to actual preparation requirements.
[0083] In a specific embodiment provided in the present application, the wafer 1 can be set to be a silicon wafer 1, and the carrier 3 can be correspondingly set to be borosilicate glass.
[0084] Step S4: grinding the wafer 1 to reduce the thickness of the wafer 1 to a preset thickness value;
[0085] As an optional implementation manner, the above-mentioned grinding of the wafer 1 to reduce the thickness of the wafer 1 to a preset thickness value includes:
[0086] The wafer 1 is mechanically ground to reduce the thickness of the wafer 1 to 100 μm or less.
[0087] After the wafer 1, bonding medium layer 2 and carrier 3 are hot-pressed and bonded to form a bonding sheet, the carrier 3 can support the wafer 1, and then the wafer is ground by mechanical grinding to reduce the thickness of the wafer 1 to 100μm or less, that is, the preset thickness value does not exceed 100μm.
[0088] Since directly thinning the wafer 1 will increase the fragmentation rate of the wafer 1 during the production process, the present application uses a carrier 3 to fix the wafer 1 and provide strength support to prevent the wafer 1 from being damaged or fragmented during the grinding process.
[0089] Step S5: a porous suction cup is arranged on the side of the wafer 1 facing away from the carrier 3, and the wafer 1 and the carrier 3 are debonded by thermal decomposition and sliding, so as to separate the wafer 1 from the carrier 3;
[0090] As an optional implementation, please refer to Figure 8 ,for Figure 1 The flowchart of separating the wafer and the carrier in the temporary bonding and debonding method shown in the figure, wherein a porous suction cup is arranged on the side of the wafer 1 facing away from the carrier 3, and the wafer 1 and the carrier 3 are debonded by thermal decomposition and sliding to separate the wafer 1 from the carrier 3, comprising:
[0091] Step S50: adsorbing the porous suction cup on the side of the wafer 1 facing away from the carrier, and adsorbing the vacuum suction cup on the side of the carrier 3 facing away from the wafer 1;
[0092] Step S51: heating the wafer 1, the bonding medium layer 2 and the carrier 3, so that the bonding medium layer 2 is heated and melted;
[0093] Step S52: Move the carrier 3 in a horizontal direction to separate the wafer 1 from the carrier 3 .
[0094] As an optional implementation, the porous suction cup is adsorbed on the side of the wafer 1 facing away from the carrier through a silicon carbide porous carrier, and the vacuum suction cup is adsorbed on the side of the carrier 3 facing away from the wafer 1.
[0095] In the embodiment of the present application, since mechanical grinding is used to reduce the thickness of the wafer 1 to 100 μm or less, it is difficult to directly separate the wafer 1 and the carrier 3 after the process is completed. In order to achieve the thermal decomposition and sliding debonding of the above-mentioned ultra-thin wafer 1 and the carrier 3, it is preferred to use a SiC (silicon carbide) porous carrier to support the entire surface of the ultra-thin wafer 1. The silicon carbide porous carrier is a device that can vacuum adsorb and support the wafer 1. For the specific structure of the above-mentioned silicon carbide porous carrier, please refer to the description of the porous carrier in the relevant technology, and the present application will not go into details here.
[0096] The porous suction cup is adsorbed on the side of the round wafer facing away from the carrier through the silicon carbide porous carrier. Since the porous suction cup has a certain air permeability, the wafer 1 can be adsorbed by drawing a vacuum to form a support for the round wafer, thereby avoiding hidden cracks in the too thin round wafer during the process of thermal decomposition and sliding debonding with the carrier 3.
[0097] Furthermore, the silicon carbide porous carrier is also correspondingly provided with a vacuum suction cup, which is arranged opposite to the through-hole suction cup, and the carrier 3 is adsorbed by the vacuum suction cup, that is, the vacuum suction cup is adsorbed on the side of the carrier 3 facing away from the wafer. At this time, the porous suction cup and the vacuum suction cup are respectively adsorbed on the wafer 1 and the carrier 3.
[0098] As an optional implementation, the bonding sheet needs to be heated so that the bonding medium layer 2 in the bonding sheet is heated and melted. Since the wafer 1 is adsorbed by the porous suction cup relatively set at the bottom, and the carrier 3 is adsorbed by the vacuum suction cup relatively set at the top, when the bonding medium layer 2 is heated and melted, the carrier 3 is moved horizontally by the vacuum suction cup until it is dragged out of the outer edge of the wafer, thereby realizing the separation of the wafer 1 and the carrier 3.
[0099] As an optional implementation manner, after the wafer 1 is separated from the carrier 3, the method further includes:
[0100] The separated wafer 1 is cleaned to remove the residual bonding medium layer 2 on the wafer 1 .
[0101] In the embodiment of the present application, after the wafer 1 completes thermal decomposition and sliding debonding, since part of the bonding medium layer 2 remains on the wafer 1, the wafer 1 needs to be cleaned.
[0102] Furthermore, at this time, the porous suction cup is adsorbed on the wafer 1, so the porous suction cup and the wafer 1 can be transferred as a whole to the single-chip wafer 1 cleaning machine to clean the surface of the wafer 1, thereby avoiding direct cleaning of the wafer 1 causing the wafer 1 to fall or break during the cleaning process.
[0103] Optionally, the wafer 1 may be cleaned with an organic solvent such as acetone or isopropanol to remove residual wax and other impurities on the bonding medium layer 2. Of course, the wafer 1 may also be cleaned with other solvents, as long as the porous suction cup is adsorbed on the wafer 1 to provide support for the wafer 1. This application does not impose any further restrictions on the solvents used in the above cleaning process.
[0104] Step S6: blowing air to the porous suction cup to separate the wafer 1 from the porous suction cup.
[0105] As an optional implementation, please refer to Fig. 9 ,for Figure 1 The flowchart of separating the wafer and the porous chuck in the temporary bonding and debonding method shown in the figure, wherein the blowing on the porous chuck comprises:
[0106] Step S60: placing the separated wafer 1 and the porous suction cup upside down on dust-free paper or dust-free cloth;
[0107] Step S61: blowing air through a plurality of air guide holes provided on the porous suction cup to release the vacuum between the wafer 1 and the porous suction cup, so as to separate the wafer 1 from the porous suction cup.
[0108] In the related art, the wafer 1 and the porous suction cup are often separated by lightly picking up or lifting the edge of the wafer 1, but this method can easily damage the wafer 1 and cause fragments; or the wafer 1 and the porous suction cup are placed in a PMMA (PolyMethyl Methacrylate) solution. Although this method can separate the porous suction cup and the wafer 1, it will cause marks on the surface of the wafer 1 and contaminate the surface of the wafer 1, so the separation effect is not good.
[0109] In the embodiment of the present application, since a plurality of air guide holes are provided on the porous suction cup, and the porous suction cup is arranged on the side of the wafer 1 away from the carrier 3, the separated wafer 1 and the porous suction cup can be turned upside down on a dust-free cloth or dust-free paper to avoid contamination of the surface of the wafer 1, thereby facilitating direct blowing operation on the porous suction cup.
[0110] Preferably, the plurality of air guide holes may be arranged along the circumference of the porous suction cup.
[0111] After placing wafer 1 and the porous suction cup upside down on the dust-free cloth or dust-free paper, gently press the porous suction cup and the wafer, and blow air through several air guide holes set on the edge of the porous suction cup to release the vacuum between the porous suction cup and wafer 1, so that wafer 1 automatically falls off the porous suction cup to avoid damage to wafer 1 caused by external force. In addition, a dust-free cloth or dust-free paper is laid under the wafer to effectively avoid contamination of the wafer surface.
[0112] The present application provides a temporary bonding and debonding method, which comprises the following steps: preparing a bonding dielectric layer on a wafer, pre-baking and curing the bonding dielectric layer and the wafer, and providing a negative pressure vacuum. By adjusting the temperature, air and pressure during the vacuum hot pressing process, the void bubbles in the bonding dielectric layer are moved to the edge of the wafer for discharge, and the bubbles generated in the center and edge of the bonding dielectric layer can be effectively removed to avoid uneven thickness of the bonding dielectric layer or hollowing caused by the bubbles, which results in the area with bubbles being unable to support the wafer, causing the wafer to break due to local loss of support during thinning. The invention can also avoid the infiltration of waste generated during the thinning process due to insufficient edge sealing of the bonding dielectric layer, resulting in unremovable contamination on the wafer surface. The thermal expansion coefficient of the carrier is set not to exceed 60% of the thermal expansion coefficient of the wafer, so as to avoid the subsequent grinding process effect during the wafer thinning process being seriously affected by excessive warping of the bonding sheet, and to avoid a greater risk of breakage due to uneven force during the subsequent debonding process, thereby improving the reliability of the temporary bonding and debonding process.
[0113] The embodiments described above are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be included in the protection scope of the present invention.
Claims
1. A method for temporary bonding and debonding, It is characterized in that The following steps are involved: preparing a bonding dielectric layer on the wafer; Pre-baking and curing the wafer and the bonding medium layer, and providing negative pressure vacuum; Arranging a carrier on the bonding medium layer, and performing thermal compression bonding on the wafer and the carrier; Grinding the wafer to reduce the thickness of the wafer to a preset thickness value; A porous suction cup is arranged on the side of the wafer facing away from the carrier, and the wafer and the carrier are subjected to thermal decomposition and sliding debonding to separate the wafer from the carrier; Air is blown to the porous suction cup to separate the wafer from the porous suction cup.
2. The temporary bonding and debonding method according to claim 1, It is characterized in that The step of preparing a bonding dielectric layer on a wafer comprises: coating liquid wax or liquid glue on the wafer; Controlling the wafer to rotate at a first speed so that the liquid wax or liquid glue is evenly covered on the wafer; Allowing the wafer to stand still so that bubbles in the liquid wax or liquid glue can burst; The wafer is controlled to rotate at a second speed to form the bonding preparation layer on the wafer; wherein the second speed is greater than the first speed.
3. The temporary bonding and debonding method according to claim 1, It is characterized in that The step of performing thermal compression bonding on the wafer and the carrier comprises: The carrier is aligned with a wafer provided with the bonding medium layer, and the wafer and the carrier are bonded by heat pressing; wherein, the temperature, air and pressure during the vacuum heat pressing process are adjusted so that the void bubbles in the bonding medium layer are moved to the edge of the wafer and discharged.
4. The temporary bonding and debonding method according to claim 1, It is characterized in that The thermal expansion coefficient of the carrier does not exceed 60% of the thermal expansion coefficient of the wafer.
5. The temporary bonding and debonding method according to claim 1, It is characterized in that The step of grinding the wafer to reduce the thickness of the wafer to a preset thickness value includes: The wafer is mechanically ground to reduce the thickness of the wafer to 100 μm or less.
6. The temporary bonding and debonding method according to claim 1, It is characterized in that The method comprises: arranging a porous suction cup on the side of the wafer facing away from the carrier, performing thermal decomposition and sliding debonding on the wafer and the carrier to separate the wafer from the carrier, comprising: Adsorbing the porous suction cup on the side of the wafer facing away from the carrier, and adsorbing the vacuum suction cup on the side of the carrier facing away from the wafer; heating the wafer, the bonding medium layer and the carrier so that the bonding medium layer is heated and melted; The carrier is moved in a horizontal direction to separate the wafer from the carrier.
7. The temporary bonding and debonding method according to claim 6, It is characterized in that The porous suction cup is adsorbed on the side of the wafer facing away from the carrier through the silicon carbide porous carrier, and the vacuum suction cup is adsorbed on the side of the carrier facing away from the wafer.
8. The temporary bonding and debonding method according to claim 1, It is characterized in that After the wafer is separated from the carrier, the method further comprises: The separated wafer is cleaned to remove the residual bonding medium layer on the wafer.
9. The temporary bonding and debonding method according to claim 1, It is characterized in that The method of blowing air to the porous suction cup comprises: Place the separated wafer and the porous suction cup upside down on dust-free paper or dust-free cloth; Blow air through a plurality of air guide holes provided on the porous suction cup to release the vacuum between the wafer and the porous suction cup, so as to separate the wafer from the porous suction cup.
10. The temporary bonding and debonding method according to any one of claims 1 to 9, It is characterized in that The wafer is a silicon wafer, and the carrier is borosilicate glass.
Citation Information
Patent Citations
Device for wafer bonding and de-bonding and wafer bonding and de-bonding method
CN112670215A
Wafer bonding method and bonding structure
CN115863241A
Wafer and wafer thinning process processing technology thereof
CN116072533A
Temporary bonding method, processing method, structure and chip of high pattern structure wafer