Carrier-assisted method for separating crystalline material along laser-damaged region
By forming a laser-damaged region under the surface of the crystal material and using a rigid carrier and adhesive to bond it together, the problems of large kerf loss, reduced material strength and long processing time in the separation of thin wafers in the prior art are solved, and efficient and reliable crystal material separation is achieved.
Patent Information
- Application Number
- CN202410848398.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-02-12
- Filing Date
- 2019-12-27
- Publication Date
- 2024-10-22
AI Technical Summary
Existing technologies for removing thin layers from crystalline materials suffer from problems such as large kerf loss, reduced material strength, long processing time, bending caused by polymer layer interface fracture, and high cost, making it difficult to achieve efficient and reliable thin wafer separation.
A rigid carrier is bonded to the surface of the crystal material with an adhesive, and fracture is achieved by using the laser-damaged area under the surface. Combined with methods such as ultrasonic energy, difference in thermal expansion coefficient, or mechanical force, reliable separation of the crystal material is achieved, avoiding the use of additional stress layers and polymer layers.
It reduces kerf loss, improves material strength and processing efficiency, reduces processing time and cost, and provides a more reliable method for separating thin wafers.
Smart Images

Figure CN118824948A_ABST
Abstract
Description
[0001] This application is a divisional application of the invention patent application with the application date of December 27, 2019, application number 201980087197.8, and invention name “Carrier-assisted method for separating crystal materials along laser damaged areas”.
[0002] Citations of Related Applications
[0003] This application claims priority to U.S. Patent Application No. 16274,045 filed on March 5, 2019, U.S. Provisional Patent Application No. 62803,333 filed on February 8, 2019, and U.S. Provisional Patent Application No. 62786,335 filed on December 29, 2018, the entire disclosures of the foregoing applications are incorporated herein by reference. Technical Field
[0004] The present disclosure relates to methods for processing crystalline materials, and more particularly to carrier-assisted methods for separating or removing relatively thin layers of crystalline materials from substrates, such as boules or wafers, having subsurface laser damaged regions therein. Background Art
[0005] Various microelectronic, optoelectronic and microfabrication applications require thin layers of crystalline materials as starting structures for making various useful systems. Conventional methods for cutting thin layers (e.g., wafers) from large diameter crystal ingots of crystalline materials involve the use of wire saws. Wire saw technology has been applied to various crystalline materials, such as silicon, sapphire and silicon carbide. The wire saw tool includes an ultra-fine steel wire (typically having a diameter of 0.2 mm or less) passing through the grooves of one or more guide rollers. There are two slicing methods, namely loose abrasive slicing and fixed abrasive slicing. Loose abrasive slicing involves applying a slurry (usually an abrasive suspension in oil) to a steel wire running at high speed, whereby the rolling motion of the abrasive between the steel wire and the workpiece causes the cutting of the ingot. Unfortunately, the environmental impact of the slurry is considerable. In order to reduce this impact, a wire fixed with diamond abrasive can be used in a fixed abrasive slicing method that only requires a water-soluble coolant (not a slurry). Highly efficient parallel slicing allows a large number of wafers to be produced in a single slicing process. Figure 1 A conventional wire saw tool 1 is shown, comprising parallel wire segments 3 extending between rollers 4A-4C and arranged to simultaneously saw an ingot 2 into a plurality of thin segments (e.g., wafers 8A-8G), each thin segment having a face generally parallel to an end face 6 of the ingot 2. During the sawing process, the wire segments 3 supported by the rollers 4A-4C may be pressed in a downward direction 5 toward a holder 7 below the ingot 2. If the end face 6 is parallel to the crystallographic c-plane of the ingot 2, and the wire segments 3 saw through the ingot 2 parallel to the end face 6, each resulting wafer 8A-8G will have a "coaxial" end face 6' parallel to the crystallographic c-plane.
[0006] It is also possible to produce ortho (also called beveled or "off-axis") wafers with end faces that are not parallel to the crystallographic c-plane. Ortho wafers (e.g., of SiC) with a 4 degree bevel are often used as growth substrates for high-quality epitaxial growth of other materials (e.g., AlN and other Group III nitrides). Ortho wafers can be produced by growing an ingot in a direction away from the c-axis (e.g., growing on ortho seed material) and sawing the ingot perpendicular to the ingot sidewalls, or by growing an ingot starting with an on-axis seed material and sawing the ingot at an angle that deviates from perpendicular to the ingot sidewalls.
[0007] Wire sawing of crystalline materials involves various limitations. Kerf loss based on the width of material removed with each cut is inherent to saw cutting and represents a significant loss of crystalline material. Wire saw cutting applies moderately high stresses to the wafer, resulting in non-zero bow and warp characteristics. The processing time for a single ingot (or ingot) is very long, and events like wire breakage increase processing time and result in undesirable material loss. Wafer strength can be reduced by flaking and cracking on the cut surface of the wafer. At the end of the wire saw process, the resulting wafer must be cleaned of debris.
[0008] In the case of silicon carbide (SiC), which has high wear resistance (and hardness comparable to diamond and boron nitride), wire saws can require a lot of time and resources, thus requiring a lot of production costs. SiC substrates enable the manufacture of desired power electronics, radio frequency devices, and optoelectronic devices. SiC exists in many different crystal structures called polytypes, some of which (e.g., 4H-SiC and 6H-SiC) have a hexagonal crystal structure.
[0009] Figure 2 is a first stereogram showing a coordinate system of an isohexagonal crystal such as 4H-SiC, in which the c-plane ((0001) plane, corresponding to the
[0001] (vertical) direction of epitaxial crystal growth) is perpendicular to the m-plane ( plane) and a plane ( plane), where Plane perpendicular to direction, and Plane perpendicular to direction. Figure 3 is a second stereoscopic crystal plan view of a hexagonal crystal, showing an ortho plane 9 that is not parallel to the c-plane, wherein a vector 10 (perpendicular to the ortho plane 9) is tilted away from the
[0001] direction by a tilt angle β, wherein the tilt angle β is (slightly) directed toward Tilt direction. Figure 4A1 is a perspective view wafer orientation diagram showing the orientation of adjacent wafer 11A relative to the c-plane ((0001) plane), wherein vector 10A (perpendicular to wafer face 9A) is tilted away from the
[0001] direction by an angle β. This tilt angle β is equal to the orthogonal tilt (or orientation bias angle) β spanned between the (0001) plane and projection 12A of wafer face 9A. Figure 4B is a simplified cross-sectional view of a neighboring wafer 11A superimposed over a portion of an ingot 14A (eg, a coaxial ingot having end faces 6A parallel to the (0001) plane) from which the neighboring wafer 11A is defined. Figure 4B The wafer surface 9A of the adjacent wafer 11A is shown to be offset by a tilt angle β with respect to the (0001) plane.
[0010] Figure 5 is a top plan view of an exemplary SiC wafer 25 including an upper surface 26 (e.g., parallel to the (0001) plane (c-plane) and perpendicular to the
[0001] direction) and laterally bounded by a generally circular edge 27 (having a diameter D) including a portion perpendicular to the
[0001] direction. The main flat portion 28 of the plane has a length LF and is parallel to direction.
[0011] Due to the difficulties associated with manufacturing and processing SiC, SiC device wafers are relatively costly relative to wafers of various other crystalline materials. Typical kerf losses obtained from wire sawing SiC can be about 250 microns or more per wafer, which is significant considering that wafers produced by the wire saw process can be about 350 microns thick and are subsequently thinned (by grinding) to a final thickness of about 100 to 180 microns (depending on the end use). Slicing wafers thinner than about 350 microns is impractical given the wire saw and device manufacturing issues.
[0012] In an effort to address limitations associated with wire saws, alternative techniques have been developed for removing thin layers of crystalline material from bulk crystals. One technique, known as controlled exfoliation, introduces a crack near the edge of a substrate (e.g., Ge(001)) by depositing a tensile stress layer (e.g., nickel) on the surface of the substrate, and mechanically guiding the crack (e.g., using a flexible handling layer such as tape) as a single fracture front along the surface (see Bedell et al., J. Phys. D: Appl. Phys. 46 (2013)). However, this technique can result in the application of very high stresses and excessive bending of the removed layer. Another technique involving the removal of silicon carbide layers from larger crystals is described in Kim et al., “4H-SiC wafer slicing by using femtosecond laser double pulses,” Optical Materials Express 2450, Vol. 7, No. 7 (2017). This technique involves forming a laser-written track by striking the silicon carbide with a laser pulse to induce subsurface damage, followed by adhering the crystal to a locking fixture and applying tension to achieve fracture along the subsurface damaged area. The use of a laser to weaken specific areas in the material, followed by fracture between these areas, reduces laser scanning time. However, it is questionable whether the aforementioned fracture technique can be used to reliably remove thin wafers from ingots without breakage and / or whether it can be scaled up to a commercial scale. Another technique known in the art for achieving fracture along laser-induced subsurface damaged areas of crystalline materials involves applying ultrasonic energy to the crystalline material, but the reliability of this method for obtaining thin wafers (e.g., 350 microns or less) has been questioned because ultrasonic fracture requires a higher degree of laser damage and may result in higher wafer breakage rates when applied to thin wafers.
[0013] Another technique disclosed in U.S. Patent Application Publication No. 2010 / 0289189A1 includes applying a polymer layer (e.g., poly(dimethylsiloxane) (PDMS)) over a solid material, and exposing the solid material and polymer layer (initially at no greater than 300° C.) to a temperature below room temperature (or a temperature below about −20° C.). This cooling causes the polymer layer to shrink, thereby inducing mechanical stresses in the solid material that cause the material to break along planes at depth in the material. PDMS is a cross-linked polymer, and its hardness can be controlled by varying the cross-link density (e.g., by varying the weight ratio of the curing agent to the prepolymer, and by varying the curing conditions). Even with efforts to improve its mechanical properties, PDMS is reported to have a Young's modulus value of less than about 4 MPa. See, e.g., Kim et al., J. Micromech. Microeng. 23 (2013) 095024.
[0014] A further technique for removing a thin layer of crystalline material from a bulk crystal is disclosed in U.S. Patent Application Publication No. 2018 / 0126484A1. Laser radiation is irradiated on the solid material to produce a detachment zone or multiple partial detachment zones, followed by formation of a polymer receiving layer (e.g., PDMS) and cooling (optionally combined with high-speed rotation) to induce mechanical stress that causes the thin layer of solid material to separate from the rest of the material along the detachment zone.
[0015] One disadvantage of techniques that rely on polymer layer interface fracture is that the resulting wafer may exhibit an undesirably high level of bow. Another disadvantage of techniques that rely on polymer layer interface fracture is that it may take a considerable amount of time (e.g., 30 minutes or more) to apply and cure the polymer layer on the solid material, and additional time to remove the polymer material from the resulting wafer. Another limitation of techniques that require a polymer layer is that such a polymer layer may not be suitable for withstanding subsequent wafer processing steps that may require precise dimensions.
[0016] Another technique for removing a thin layer of crystalline material from a bulk crystal is disclosed in U.S. Patent Application Publication No. 2018 / 0243944A1. Laser radiation is irradiated on a donor substrate to specify a crack path, a carrier substrate (i.e., having a thickness of less than 800 microns) is disposed on the carrier substrate via a bonding layer, a stress generating layer (e.g., a PDMS layer), and the stress generating layer is thermally loaded (i.e., cooled with a coolant, particularly liquid nitrogen) to transfer stress through the carrier substrate and the bonding layer, thereby generating stress in the donor substrate to trigger a crack that propagates on the crack path to remove the solid layer (and the carrier substrate bonded thereto) from the donor substrate. The donor substrate and the carrier substrate are preferably composed of the same material, but may be composed of different materials. The limited maximum thickness of the carrier substrate appears to be necessary to enable the stress to propagate from the stress generating layer to the donor substrate. One limitation of the above technique is the need to provide at least three layers on the donor substrate. Another limitation is that the technique appears to be limited to thermally induced cooling at very low (e.g., liquid nitrogen) temperatures. Yet another limitation is that the maximum thickness of the carrier substrate cannot exceed 800 microns, thereby potentially limiting the rigidity of the bonded assembly after separation from the donor substrate. Yet another limitation is that reusing the carrier substrate would require removing residual materials of different composition (i.e., bonding layer material and stress-generating layer material) from its opposing sides.
[0017] Accordingly, the art continues to seek improved methods for separating or removing relatively thin layers of crystalline material from substrates that address the problems associated with conventional methods. Summary of the invention
[0018] The present disclosure relates in various aspects to a method for processing a crystalline material, the method comprising bonding a carrier (e.g., a rigid carrier) to a surface of a crystalline material having subsurface laser damage at a non-zero depth relative to the surface, followed by fracture of the crystalline material along the subsurface laser damage region. This fracture produces a bonded assembly comprising a substrate and a portion of the crystalline material removed from the substrate. The fracture is performed without the need for a separate stress-generating layer disposed above the carrier. The foregoing steps may be repeated to sequentially remove thin layers of crystalline material from an ingot to form a wafer. In certain embodiments, the carrier may be crystalline in nature. In certain embodiments, the rigid carrier may be bonded to the surface of the crystalline material by adhesive bonding, the rigid carrier may have a thickness greater than 800 microns, and the rigid carrier may have an elastic modulus of at least 20 GPa (or another threshold value disclosed herein). In certain embodiments, the adhesive material has a glass transition temperature Tg greater than 25° C. (or another threshold value specified herein). A portion of the crystalline material removed from the substrate (which may be embodied as a wafer) may be used to undergo further processing steps while the portion remains part of the bonded assembly. In some embodiments, the first rigid carrier and the second rigid carrier can be bonded to opposite sides of the substrate prior to fracture. In some implementations, fracture of the crystalline material can be facilitated by: (i) applying a mechanical force proximate to at least one edge of the carrier (e.g., optionally positioned at one or more points) to impart a bending moment in at least a portion of the carrier; (ii) cooling the carrier in the event that the carrier has a greater coefficient of thermal expansion than the crystalline material; and / or (iii) applying ultrasonic energy to the crystalline material.
[0019] In one aspect, the present disclosure relates to a method of processing a crystalline material, the method comprising temporarily bonding a rigid carrier to a surface of the crystalline material with an intermediate bonding material, wherein the crystalline material comprises a substrate having a subsurface laser damaged region at a depth relative to a first surface of the substrate, and wherein the bonding material has a glass transition temperature, Tg, greater than 25° C. (or another threshold value specified herein). The method further comprises fracturing the crystalline material along or proximate to the subsurface laser damaged region to produce a bonded assembly comprising the rigid carrier, the bonding material, and a portion of the crystalline material removed from the substrate.
[0020] In certain embodiments, the rigid carrier has a thickness greater than 800 microns; the rigid carrier has an elastic modulus of at least 20 GPa, and in the combined assembly, the portion of the crystalline material removed from the substrate comprises at least 160μm Thickness.
[0021] In certain embodiments, the bonding material comprises a thermoplastic material.In certain embodiments, the bonding material has a glass transition temperature, Tg, of at least 35°C, at least 50°C, at least 60°C, or another threshold value specified herein.
[0022] In certain embodiments, the bonding material has a Shore D hardness value of at least about 70 when the bonding material is at 25° C. In certain embodiments, the bonding material has an elastic modulus of at least about 7 MPa when the bonding material is at 25° C.
[0023] In certain embodiments, the rigid support has a thickness greater than 800 microns. In certain embodiments, the rigid support has an elastic modulus of at least 20 GPa, at least 100 GPa, or another threshold value specified herein. In certain embodiments, the rigid support comprises a crystalline material.
[0024] In certain embodiments, the rigid carrier includes a first side and a second side opposite the first side; the adhesive material is disposed in contact with the first side; and the second side is free of any adhesive material and free of any stress-generating material.
[0025] In some embodiments, the rigid carrier has a coefficient of thermal expansion (CTE) greater than the CTE of the substrate at 25° C. In some embodiments, breaking includes at least cooling the rigid carrier to promote breaking of the crystalline material along or proximate to the subsurface laser damaged region.
[0026] In certain embodiments, disrupting comprises applying ultrasonic energy to at least one of the rigid carrier or the substrate.
[0027] In some embodiments, at least one of a maximum length or a maximum width of at least a portion of the rigid carrier exceeds a corresponding maximum length or maximum width of the substrate. In some embodiments, the substrate includes a notch or a flat along at least one edge of the substrate, and at least a portion of at least one edge of the rigid carrier extends laterally beyond the notch or the flat. In some embodiments, the fracture includes applying a mechanical force proximate to at least one edge of the rigid carrier, and wherein the mechanical force is configured to impart a bending moment in at least a portion of the rigid carrier.
[0028] In certain embodiments, the crystalline material comprises a hexagonal crystal structure; and the bending moment is in the vertical
[0029] Hexagonal crystal structure Orientation within ±5 degrees of direction.
[0030] In certain embodiments, the method further comprises performing at least one additional processing step on a portion of the crystalline material while the portion of the crystalline material is still part of the bonded assembly.
[0031] In certain embodiments, the method further comprises bonding an additional rigid support to a second surface of the crystalline material opposite the first surface prior to fracturing.
[0032] In certain embodiments, the subsurface laser damaged region includes a plurality of substantially parallel subsurface laser damaged lines.
[0033] In certain embodiments, the method further comprises removing a portion of the crystalline material from the bonded assembly.
[0034] In certain embodiments, the crystalline material comprises SiC.
[0035] In certain embodiments, the method further comprises roughening, texturing and / or etching at least one of (i) the first surface of the crystalline material or (ii) an adjacent surface of the rigid carrier prior to temporarily bonding the rigid carrier to the first surface of the crystalline material with the adhesive material.
[0036] In certain embodiments, the crystalline material comprises a thickness of at least 500 microns prior to fracturing the crystalline material along or proximate to the subsurface laser damaged region.
[0037] In some embodiments, the portion of the crystalline material removed from the substrate comprises a self-supporting wafer configured to grow at least one epitaxial layer thereon. In some embodiments, the portion of the crystalline material removed from the substrate comprises a device wafer comprising at least one epitaxial layer grown thereon.
[0038] In another aspect, the present disclosure relates to a method for processing a crystalline material, the method comprising: bonding a first crystal carrier to a first surface of a crystalline material, wherein the crystalline material comprises a substrate having a subsurface laser damaged region at a depth relative to the first surface of the substrate; bonding a second crystal carrier to the second surface of the crystalline material; and after the bonding step, fracturing the crystalline material along the subsurface laser damaged region or close to the subsurface laser damaged region to produce a bonded assembly comprising the first crystal carrier and a portion of the crystalline material removed from the substrate.
[0039] In certain embodiments, at least one of the first crystal support or the second crystal support comprises an elastic modulus of at least 100 GPa. In certain embodiments, at least one of the first crystal support or the second crystal support comprises a thickness greater than 800 microns.
[0040] In some embodiments, at 25° C., the coefficient of thermal expansion (CTE) of the first crystalline carrier is greater than the CTE of the substrate; and breaking includes cooling at least the first crystalline material carrier to promote breaking of the crystalline material along or near the subsurface laser damaged region.
[0041] In certain embodiments, fracturing of the crystalline material along or proximate to the subsurface laser damaged region comprises applying ultrasonic energy to at least one of the first crystal carrier or the substrate.
[0042] In certain embodiments, at least one of a maximum length or a maximum width of at least a portion of the first crystal carrier exceeds a corresponding maximum length or maximum width of the substrate.
[0043] In certain embodiments, the substrate includes a notch or flat along at least one edge of the substrate, and at least a portion of at least one edge of the first crystal carrier extends laterally beyond the notch or flat.
[0044] In certain embodiments, the fracturing of the crystalline material along or proximate to the subsurface laser damaged region comprises applying a mechanical force proximate to at least one edge of the first crystal carrier, and the mechanical force is configured to impart a bending moment in at least a portion of the first crystal carrier. In certain embodiments, the crystalline material comprises a hexagonal crystal structure; and the bending moment
[0045] In the perpendicular direction of the hexagonal crystal structure The hexagonal crystal structure is oriented within ±5 degrees of the substrate surface.
[0046] In certain embodiments, at least one of bonding the first crystal support to the first surface of the crystalline material or bonding the second crystal support to the second surface of the crystalline material comprises anodic bonding.
[0047] In certain embodiments, at least one of bonding the first crystal support to the first surface of the crystal material or bonding the second crystal support to the second surface of the crystal support comprises adhesive bonding using an adhesive material.
[0048] In certain embodiments, the bonding material has a glass transition temperature, Tg, greater than 25°C.
[0049] In certain embodiments, the first crystal carrier includes a first face and a second face opposite the first face; the bonding material is disposed in contact with the first face; and the second face is free of any bonding material and free of any stress-generating material.
[0050] In certain embodiments, the adhesive material comprises a thermoplastic material.
[0051] In certain embodiments, the bonding material has a Shore D hardness value of at least about 70 when the bonding material is at 25°C.
[0052] In certain embodiments, the bonding material has an elastic modulus of at least about 7 MPa when the bonding material is at 25°C.
[0053] In certain embodiments, the method further comprises performing at least one additional processing step on a portion of the crystalline material while the portion of the crystalline material is still part of the bonded assembly.
[0054] In certain embodiments, the subsurface laser damaged region includes a plurality of substantially parallel subsurface laser damaged lines.
[0055] In certain embodiments, the method further comprises removing a portion of the crystalline material from the bonded assembly.
[0056] In certain embodiments, the crystalline material comprises SiC.
[0057] In some embodiments, the portion of the crystalline material removed from the substrate comprises a self-supporting wafer configured to grow at least one epitaxial layer thereon. In some embodiments, the portion of the crystalline material removed from the substrate comprises a device wafer comprising at least one epitaxial layer grown thereon.
[0058] In another aspect, the present disclosure is directed to a method of processing a crystalline material, the method comprising: bonding a rigid carrier to a first surface of the crystalline material, wherein the crystalline material comprises a substrate having a subsurface laser damaged region at a depth relative to the first surface, and at least a portion of at least one edge of the rigid carrier extends laterally beyond a corresponding at least one edge of the substrate. The method further comprises applying a mechanical force proximate to at least one edge of the rigid carrier to impart a bending moment in at least a portion of the rigid carrier, and fracturing the crystalline material along or proximate to the subsurface laser damaged region to produce a bonded assembly comprising the rigid carrier and a portion of the crystalline material removed from the substrate.
[0059] In certain embodiments, applying the mechanical force proximate to at least one edge of the rigid carrier consists of locally applying the mechanical force at a single location proximate to at least one edge of the rigid carrier.
[0060] In certain embodiments, applying a mechanical force proximate to at least one edge of the rigid carrier includes: locally applying the mechanical force at a plurality of spatially divided locations proximate to at least one edge of the rigid carrier; and applying an opposing mechanical force at a central location of the rigid carrier.
[0061] In certain embodiments, at least a portion of at least one edge of the rigid carrier extends laterally beyond a corresponding at least one edge of the substrate by at least about 100 microns, or at least about 500 microns (or another distance threshold disclosed herein).
[0062] In certain embodiments, the substrate includes a notch or flat along at least one edge of the substrate, and at least a portion of at least one edge of the rigid carrier extends laterally beyond the notch or flat.
[0063] In certain embodiments, the crystalline material comprises a hexagonal crystal structure; and the bending moment is in the vertical
[0064] Hexagonal crystal structure The hexagonal crystal structure is oriented within ±5 degrees of the substrate surface.
[0065] In certain embodiments, bonding the rigid carrier to the surface of the crystalline material includes adhesive bonding using an adhesive material disposed between the rigid carrier and the surface of the crystalline material.
[0066] In some embodiments, the method further comprises bonding an additional rigid support to a second surface of the crystalline material opposite the first surface prior to applying the mechanical force. In some embodiments, applying the mechanical force comprises applying a local pulling force between the first rigid support and the additional rigid support to increase the spacing between the first rigid support and the additional rigid support.
[0067] In some embodiments, the portion of the crystalline material removed from the substrate comprises a self-supporting wafer configured to grow at least one epitaxial layer thereon. In some embodiments, the portion of the crystalline material removed from the substrate comprises a device wafer comprising at least one epitaxial layer grown thereon.
[0068] In another aspect, the present disclosure relates to a method for processing a crystalline material, the method comprising: bonding a rigid carrier to a first surface of the crystalline material, wherein the crystalline material comprises a substrate having a subsurface laser damaged region at a depth relative to the first surface, the rigid carrier comprises a thickness greater than 850 microns, and the rigid carrier comprises at least one of the following features (i) or (ii): (i) the carrier comprises a crystalline carrier; or (ii) the carrier has an elastic modulus of at least 20 GPa; and fracturing the crystalline material along or proximate to the subsurface laser damaged region to produce a bonded assembly comprising the rigid carrier and a portion of the crystalline material removed from the substrate.
[0069] In some embodiments, the rigid carrier comprises a crystalline carrier. In some embodiments, the carrier has an elastic modulus of at least 20 GPa, at least 100 GPa, or another threshold value specified herein. In some embodiments, bonding the rigid carrier to the crystalline material comprises adhesive bonding using an adhesive material disposed between the rigid carrier and the crystalline material.
[0070] In certain embodiments, the bonding material has a glass transition temperature Tg greater than 25° C. In certain embodiments, the bonding material has a Shore D hardness value of at least about 70 when the bonding material is at 25° C. In certain embodiments, the bonding material has an elastic modulus of at least about 7 MPa when the bonding material is at 25° C.
[0071] In certain embodiments, the rigid carrier includes a first side and a second side opposite the first side; the adhesive material is disposed in contact with the first side; and the second side is free of any adhesive material and free of any stress-generating material.
[0072] In certain embodiments, the coefficient of thermal expansion (CTE) of the rigid carrier is greater than the CTE of the substrate at 25°C.
[0073] In certain embodiments, fracturing includes cooling at least the rigid carrier to promote fracturing of the crystalline material along or proximate to the subsurface laser damaged region.
[0074] In certain embodiments, wherein disrupting comprises applying ultrasonic energy to at least one of the rigid carrier or the substrate.
[0075] In some embodiments, at least one of a maximum length or a maximum width of at least a portion of the rigid carrier exceeds a corresponding maximum length or maximum width of the substrate. In some embodiments, the substrate includes a notch or a flat along at least one edge of the substrate, and at least a portion of at least one edge of the rigid carrier extends laterally beyond the notch or the flat.
[0076] In certain embodiments, fracturing comprises applying a mechanical force proximate to at least one edge of the rigid carrier, and wherein the mechanical force is configured to impart a bending moment in at least a portion of the rigid carrier.
[0077] In certain embodiments, the crystalline material comprises a hexagonal crystal structure; and the bending moment is in the vertical
[0078] Hexagonal crystal structure Orientation within ±5 degrees of direction.
[0079] In certain embodiments, the method further comprises performing at least one additional processing step on a portion of the crystalline material while the portion of the crystalline material is still part of the bonded assembly.
[0080] In certain embodiments, the method further comprises bonding an additional rigid support to a second surface of the crystalline material opposite the first surface prior to breaking. In certain embodiments, the method further comprises removing a portion of the crystalline material from the bonded assembly.
[0081] In certain embodiments, the crystalline material comprises SiC.
[0082] In certain embodiments, the portion of the crystalline material removed from the substrate comprises a free-standing wafer configured to grow at least one epitaxial layer thereon.
[0083] In certain embodiments, the portion of the crystalline material removed from the substrate comprises a device wafer including at least one epitaxial layer grown thereon.
[0084] In another aspect, the present disclosure relates to a method comprising: grinding an edge of a thick wafer of crystalline material to eliminate a non-vertical edge profile and to form a vertical edge profile, wherein the thick wafer comprises a first surface, a second surface opposite the first surface, and at least one epitaxial layer deposited on or above the first surface, and wherein a rigid first carrier is temporarily bonded over the at least one epitaxial layer with an adhesive material disposed between the rigid first carrier and the at least one epitaxial layer; and after forming the vertical edge profile, impinging a laser shot through the second surface of the thick wafer to form a subsurface laser damaged region within the thick wafer.
[0085] In some embodiments, the method also includes bonding a rigid second carrier to the second surface of the thick wafer; and breaking the thick wafer along a laser damaged region beneath the surface or proximate to the laser damaged region beneath the surface to produce: (i) a first bonded assembly comprising a rigid first carrier, an adhesive material, at least one epitaxial layer, and a first thin wafer severed from the thick wafer; and (ii) a second bonded assembly comprising a rigid second carrier and a second thin wafer severed from the thick wafer.
[0086] In some embodiments, the method also includes: bonding a rigid first carrier to a major surface of a crystalline material, wherein the crystalline material includes a substrate having an initial subsurface laser damage region at a depth relative to the major surface; breaking the crystalline material along or near the initial subsurface laser damage region to produce an initial bonded assembly including the rigid first carrier and a portion of the crystalline material removed from the substrate; and removing a portion of the crystalline material from the first bonded assembly to produce a thick wafer, wherein the thick wafer includes a portion of the crystalline material.
[0087] In certain embodiments, the method further includes: forming a non-vertical wafer edge of the thick wafer; and epitaxially growing at least one epitaxial layer on or over the first surface of the thick wafer after generating the non-vertical wafer edge.
[0088] In certain embodiments, at least one of the first thin wafer or the second thin wafer comprises a thickness of less than 250 microns. In certain embodiments, the crystalline material comprises SiC.
[0089] In another aspect, the present disclosure relates to a method for processing a crystalline material wafer, the crystalline material wafer comprising a first surface having surface damage thereon, the first surface being defined by an edge, the method comprising: grinding the first surface with at least one first grinding device to remove a first portion of the surface damage; after grinding the first surface with the at least one first grinding device, edge grinding the edge to form a chamfered or rounded edge profile; and after edge grinding, grinding the first surface with at least one second grinding device to remove a second portion of the surface damage, the second portion being sufficient to make the first surface suitable for further processing by chemical mechanical planarization.
[0090] In certain embodiments, the method further includes: processing the first surface by chemical mechanical planarization to epitaxially grow one or more layers of semiconductor material on the first surface after grinding the first surface with at least one second grinding device.
[0091] In certain embodiments, at least one first grinding device includes at least one grinding wheel having a grinding surface of less than 5000 grit (e.g., 1000 grit, 1400 grit, 2000 grit, 3000 grit, 4000 grit, etc.), and at least one second grinding device includes at least one grinding wheel having a grinding surface of at least 5000 grit (e.g., 5000 grit, 7000 grit, 8000 grit, 10,000 grit, 15,000 grit, 20,000 grit, 25,000 grit, 30,000 grit, etc.).
[0092] In certain embodiments, grinding the first surface with at least one first grinding device includes removing crystalline material having a thickness of 20 to 100 microns (e.g., 20 to 80 microns, 40 to 80 microns, 40 to 60 microns, etc.), and grinding the second surface with at least one second grinding device includes removing crystalline material having a thickness of 3 to 15 microns (e.g., 5 to 10 microns).
[0093] In certain embodiments, the surface damage includes laser damage and fracture damage.
[0094] In certain embodiments, the crystalline material comprises a silicon carbide material, and the first surface comprises a Si-terminated facet of the silicon carbide material.
[0095] On the other hand, the present disclosure relates to a method for processing a crystalline material wafer, the crystalline material wafer including a first surface having surface damage thereon, the first surface being defined by an edge, the method comprising: grinding the first surface with at least one first grinding device to remove a first portion of the surface damage; after grinding the first surface with at least one first grinding device, grinding the first surface with at least one second grinding device to remove a second portion of the surface damage, the second portion being sufficient to make the first surface suitable for further processing by chemical mechanical planarization; after grinding the first surface with at least one second grinding device, forming a protective coating on the first surface; after depositing a sacrificial material on the first surface, edge grinding the edge to form a chamfered or rounded edge profile; and after edge grinding, removing the protective coating from the first surface.
[0096] In certain embodiments, the method further includes, after removing the sacrificial material from the first surface, processing the first surface by chemical mechanical planarization to prepare the first surface for epitaxial growth of one or more layers of semiconductor material thereon.
[0097] In certain embodiments, at least one first grinding device includes at least one grinding wheel having a grinding surface with a grit of less than 5000, and at least one second grinding device includes at least one grinding wheel having a grinding surface with a grit of at least 5000.
[0098] In certain embodiments, grinding the first surface with at least one first grinding device comprises removing crystalline material to a thickness of 20 microns to 100 microns, and grinding the second surface with at least one second grinding device comprises removing crystalline material to a thickness of 3 microns to 15 microns.
[0099] In certain embodiments, the protective coating comprises a photoresist.
[0100] In certain embodiments, the surface damage includes laser damage and fracture damage.
[0101] In certain embodiments, the crystalline material comprises a silicon carbide material, and the first surface comprises a Si-terminated facet of the silicon carbide material.
[0102] On the other hand, the present disclosure relates to a material processing device, comprising: a laser processing station, which is configured to form a subsurface laser damage area in a crystal material substrate supplied to the laser processing station; a fracture station, which is arranged to receive the crystal material substrate processed by the laser processing station, and is configured to fracture the crystal material substrate along the subsurface laser damage area to form a crystal material portion removed from the crystal material substrate, wherein each crystal material portion includes surface damage; a plurality of rough grinding stations, which are arranged in parallel downstream of the fracture station and are configured to remove a first portion of the surface damage from the crystal material portion, wherein at least a first rough grinding station and a second rough grinding station of the plurality of rough grinding stations are configured to operate simultaneously to remove a first portion of the surface damage of different crystal material portions; and at least one fine grinding station, which is arranged downstream of the plurality of rough grinding stations and is configured to remove a second portion of the surface damage from the crystal material portion, the second portion being sufficient to make at least one surface of each crystal material portion suitable for further processing by chemical mechanical planarization.
[0103] In certain embodiments, the apparatus further comprises at least one chemical mechanical planarization station disposed downstream of the at least one fine grinding station and configured to render at least one surface of each crystalline material portion suitable for further processing by chemical mechanical planarization.
[0104] In certain embodiments, the apparatus further comprises at least one edge grinding station configured to grind an edge of each crystalline material portion to form a beveled or rounded edge profile.
[0105] In certain embodiments, each rough grinding station includes at least one grinding wheel having a grinding surface with a grit of less than 5000, and at least one fine grinding station includes at least one grinding wheel having a grinding surface with a grit of at least 5000.
[0106] In certain embodiments, each rough grinding station is configured to remove 20 microns to 100 microns of crystalline material thickness from each crystalline material portion, and each fine grinding station is configured to remove 3 microns to 15 microns of crystalline material thickness from each crystalline material portion.
[0107] In certain embodiments, the laser processing station is configured to simultaneously form subsurface laser damaged regions in a plurality of crystalline material substrates.
[0108] On the other hand, any of the aforementioned aspects, and / or various individual aspects and features as described herein can be combined for additional advantage. Unless otherwise indicated herein, any of the various features and elements disclosed herein can be combined with one or more other disclosed features and elements.
[0109] Other aspects, features and embodiments of the present disclosure will be more fully apparent from the ensuing disclosure and appended claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0110] The accompanying drawings, which are incorporated in and form a part of this specification, illustrate several aspects of the disclosure, and together with the description, serve to explain the principles of the disclosure.
[0111] Figure 1 Included are a first frame providing a perspective view of an ingot received by a conventional wire saw tool and subjected to a wire saw process and a second frame providing a perspective view of a plurality of wafers obtained by the wire saw process.
[0112] Figure 2 is a first stereogram showing a coordinate system of a hexagonal crystal such as 4H-SiC.
[0113] Figure 3 is a second perspective crystal plan view for a hexagonal crystal, showing ortho planes that are not parallel to the c-plane.
[0114] Figure 4A is a perspective view of a wafer orientation diagram showing the orientation of adjacent wafers relative to the c-plane.
[0115] Figure 4B It is superimposed on a part of the ingot. Figure 4A Simplified cross-section of an adjacent wafer.
[0116] Figure 5 is a top plan view of an exemplary SiC wafer with superimposed arrows showing the crystallographic orientation direction.
[0117] Fig. 6A is a schematic side view of a coaxial ingot of crystalline material.
[0118] Figure 6B yes Fig. 6A Schematic side view of an ingot rotated 4 degrees with an overlaid pattern for cutting the end of the ingot.
[0119] Figure 6C is a schematic side view of an ingot after the end portion has been removed to provide an end surface that is not perpendicular to the c-direction.
[0120] Figure 7 is a schematic perspective view of a movable laser tool configured to focus laser emission within a crystalline material to form subsurface lesions.
[0121] FIG. 8A to FIG. 8D An exemplary laser tool travel path relative to a crystalline material for forming subsurface damage within the crystalline material is provided. Fig.8D Includes display of subsurface lines relative to
[0122] Hexagonal crystal structure of crystalline materials Superimposed arrows of orientation in the direction where the lines are also parallel to the surface of the crystalline material.
[0123] Fig. 9 is a side cross-sectional schematic diagram of an assembly including a crystalline material substrate having subsurface laser damage and bonded to a rigid carrier via an intermediately disposed adhesive material and including an exposed adhesive lip surrounding at least a portion of a perimeter of the crystalline material along an interface with the rigid carrier.
[0124] Fig. 10A is a schematic side cross-sectional view of a rigid carrier having an adhesive material bonded to its surface.
[0125] Fig. 10B yes Fig. 10A A schematic cross-sectional view of an assembly of a rigid carrier and bonding material bonded to a crystalline material substrate having a laser damaged region proximate to the surface of the bonding material, wherein the assembly is similar to Fig. 9 The assembly shown but lacking the exposed bonding lip.
[0126] Fig. 10C yes Fig. 10B Schematic cross-section of an assembly in which a surface of a rigid carrier is positioned on a cooling device in the form of a liquid cooling chuck.
[0127] Fig. 10D is a schematic cross-sectional view of a substantial portion of a crystalline material substrate separated from a bonded assembly (atop a liquid cooled chuck) comprising a rigid carrier and a portion of the crystalline material removed from the substrate after fracturing the crystalline material along a subsurface laser damaged region.
[0128] Fig. 10E yes Fig. 10D Schematic cross-section of the bonded assembly after removal from the liquid-cooled chuck, with residual laser damage along the upward-facing surface.
[0129] Fig.10F is a schematic cross-sectional view of a portion of a crystalline material supported by a heated vacuum chuck, wherein a rigid carrier and bonding material are laterally translated away from the crystalline material portion following thermal softening and release of the bonding material.
[0130] Fig.11 is based on Fig. 10C Schematic cross-sectional view of components on a cooling device in the form of a liquid-cooled chuck arranged in a bath of liquid coolant.
[0131] Fig.12is a perspective view of a cooling apparatus including a vacuum chuck disposed proximate a bottom wall of a container arranged to receive a liquid cryogen (eg, methanol, liquid nitrogen, etc. received from an evaporative cooling system).
[0132] FIG. 13A to FIG. 13E is a top view of a bonded assembly including carriers of different shapes each bonded to a substrate of crystalline material.
[0133] Fig.13F and Figure 13G Provided separately Fig.13D and Fig.13E A side cross-sectional schematic diagram of a combined assembly.
[0134] Fig.14 is a schematic cross-sectional view of a crystalline material having subsurface laser damage and bonded to a rigid carrier, wherein the crystalline material and the carrier are arranged in a liquid bath of an ultrasonic generator.
[0135] FIG. 15A to FIG. 15D is a schematic cross-sectional view showing steps for fracturing a crystalline material having subsurface laser damage, including applying a mechanical force proximate one edge of a carrier to impart a bending moment in at least a portion of the carrier.
[0136] Fig.16A is a cross-sectional schematic diagram of an apparatus for fracturing a crystalline material to which a substrate having subsurface laser damage is bonded by applying mechanical forces along opposite edges of the carrier to impart a bending moment in portions of the carrier.
[0137] Fig. 16B is used Fig.16A Schematic cross-sectional view of a device separated from bulk crystalline material including a bonded assembly of a rigid carrier and a substrate.
[0138] FIG. 17A to FIG. 17D Schematic cross-sectional views of forming subsurface laser damage in a substrate of crystalline material by focusing laser emission into a bare substrate, through the surface of a substrate supported by a carrier, through the carrier and adhesive layer into the substrate, and through the carrier into the substrate, respectively.
[0139] FIG. 18A to FIG. 18O is a cross-sectional schematic diagram illustrating steps of a device wafer splitting process, according to which a thick wafer is broken from a crystalline material, at least one epitaxial layer is grown on the thick wafer, and the thick wafer is broken to form a first bonded assembly and a second bonded assembly, the first bonded assembly and the second bonded assembly each including a carrier and a thin wafer separated from the thick wafer, wherein the first bonded assembly includes at least one epitaxial layer as part of an operable semiconductor-based device.
[0140] Fig.19is a flow chart schematically illustrating the steps for producing subsurface laser damage and bonding a rigid carrier to an ingot of crystalline (e.g., SiC) material, followed by laser separation of the bonded assembly including the carrier and a portion of the crystalline material, followed by further processing of the bonded assembly and forming an epitaxial layer on a device wafer, returning the ingot and rigid carrier to the beginning of the process.
[0141] Fig. 20 yes Fig.19 Schematic cross-section of a portion of a crystalline material substrate showing subsurface laser damage with superimposed dashed lines identifying the expected kerf loss material area due to laser damage and subsequent surface processing (e.g., grinding and polishing).
[0142] Fig.21 is a schematic diagram of a material processing apparatus according to one embodiment, the apparatus comprising a laser processing station, a material breaking station, a plurality of rough grinding stations arranged in parallel, a fine grinding station, and a CMP station.
[0143] Fig. 22 is based on Fig.21 A schematic diagram of a material processing apparatus of a similar embodiment, but wherein the edge grinding station is arranged between the fine grinding station and the rough grinding station.
[0144] Fig.23 is a schematic diagram of a material processing apparatus according to one embodiment, the apparatus comprising a laser processing station, a material breaking station, a plurality of rough grinding stations arranged in parallel, a fine grinding station, a surface coating station, an edge grinding station, a coating removal station, and a CMP station.
[0145] Fig.24A is a schematic side cross-sectional view of a first apparatus for holding an ingot having end surfaces that are non-perpendicular to its sidewalls according to one embodiment.
[0146] Fig. 24B is a schematic side cross-sectional view of a second apparatus for holding an ingot having an end surface that is non-perpendicular to its sidewalls according to one embodiment.
[0147] Fig.25 is a line graph that plots the linear coefficient of thermal expansion for sapphire as a function of temperature.
[0148] Fig.26 is a line graph plotting the linear coefficient of thermal expansion for SiC as a function of temperature.
[0149] Fig. 27 is a bar graph providing a comparison of the linear thermal expansion coefficients for various crystalline materials and metals.
[0150] Fig.28is a graph plotting elastic modulus (Young's modulus) values for various materials divided into three groups: (1) metals and alloys; (2) graphite, ceramics, and semiconductors; and (3) polymers. DETAILED DESCRIPTION
[0151] Various aspects of the present disclosure provide a method for processing a crystalline material, wherein a carrier (e.g., a rigid carrier) is bonded to a surface of a crystalline material having subsurface laser damage at a depth, and the crystalline material is fractured along the subsurface laser damage region, providing a bonded assembly including the carrier and a portion of the crystalline material removed from the substrate. The fracture is performed without the need for a separate stress-generating layer disposed above the carrier. The foregoing steps may be repeated to sequentially remove thin layers of crystalline material from an ingot to form a wafer. In certain embodiments, the carrier comprises a crystalline material. In certain embodiments, the rigid carrier may be bonded to the surface of the crystalline material by an adhesive bond, and the rigid carrier may have an elastic modulus of at least 20 GPa. The adhesive material may have a glass transition temperature Tg greater than 25°C (or another threshold value specified herein). A portion of the crystalline material removed from the substrate (which may be embodied as a wafer) may be used to undergo further processing steps while the portion remains part of the bonded assembly. In certain embodiments, fracture of the crystalline material can be facilitated by: (i) applying a mechanical force proximate to at least one edge of the carrier (e.g., optionally positioned at one or more points) to impart a bending moment in at least a portion of the carrier; (ii) cooling the carrier in the event that the carrier has a greater coefficient of thermal expansion than the crystalline material; and / or (iii) applying ultrasonic energy to at least a portion of the bonded assembly.
[0152] The embodiments set forth below represent necessary information to enable those skilled in the art to practice the embodiments and to illustrate the best mode for practicing the embodiments. When reading the following description in conjunction with the accompanying drawings, those skilled in the art will understand the concepts of the present disclosure and will recognize the applications of these concepts that are not specifically addressed herein. It should be understood that these concepts and applications fall within the scope of the present disclosure and the appended claims.
[0153] It will be understood that although the terms first, second, etc. can be used to describe various elements in this article, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. For example, without departing from the scope of the present disclosure, the first element can be referred to as the second element, and similarly, the second element can be referred to as the first element. As used herein, the term "and / or" includes any and all combinations of one or more associated listed items.
[0154] It should be understood that when an element such as a layer, region or substrate is referred to as "on another element" or "extending onto another element", it can be directly on another element or directly extended to another element, or there can also be an intermediate element. On the contrary, when an element is opposite, when an element is referred to as "directly on" or "directly extending to" another element, there is no intermediate element. Similarly, it should be understood that when an element such as a layer, region or substrate is referred to as "above another element" or extending "on another element", it can be directly above another element or directly extended to another element, or there can also be an intermediate element. On the contrary, when an element is referred to as "directly above another element" or "directly extending to another element", there is no intermediate element. It should be understood that when an element is referred to as "connected" or "coupled" to another element, it can be directly connected or coupled to another element, or there can be an intermediate element. On the contrary, when an element is referred to as "directly connected" or "directly coupled" to another element, there is no intermediate element.
[0155] Relative terms such as "below" or "above" or "upper" or "lower" or "horizontal" or "vertical" may be used herein to describe one element, layer or region relative to another element, layer or region as shown in the figures. It should be understood that these terms and those discussed above are intended to encompass different orientations of the device in addition to the orientation depicted in the figures.
[0156] The terms used herein are only used for the purpose of describing specific embodiments and are not intended to limit the present disclosure. As used herein, the singular forms "a", "a kind of" and "the" are also intended to include plural forms unless the context clearly indicates otherwise. It should be further understood that the terms "include", "comprise", "contain", and / or "contain" specify the presence of stated features, integers, steps, operations, elements and / or parts when used herein, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or their groups.
[0157] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the present disclosure belongs. It should be further understood that the terms used herein should be interpreted as having the same meaning as they have in the context of this specification and the relevant art, and will not be interpreted in an idealized or overly formal sense unless explicitly defined as such herein.
[0158] As used herein, "substrate" refers to a crystalline material (such as an ingot or wafer) that can be divided into at least two thinner parts, the at least two thinner parts having substantially the same lateral dimensions (e.g., diameter, or length and width) as the substrate, and having sufficient thickness (i) to support epitaxial deposition of one or more layers of crystalline material for surface treatment (e.g., grinding and polishing), and optionally (ii) if self-supporting when separated from a rigid carrier. In certain embodiments, the substrate can have a generally cylindrical shape, and / or can have a thickness of at least about one or more of the following thicknesses: 300 μm, 350 μm, 500 μm, 750 μm, 1 mm, 2 mm, 3 mm, 5 mm, 1 cm, 2 cm, 5 cm, 10 cm, 20 cm, 30 cm, or greater. In certain embodiments, the substrate can include a thicker wafer that can be divided into two thinner wafers. In some embodiments, the substrate can be part of a thicker wafer having one or more epitaxial layers disposed thereon (optionally in combination with one or more metal contacts) as part of a device wafer having a plurality of electrically operational devices. The device wafer can be segmented according to aspects of the present disclosure to produce a thinner device wafer and a second thinner wafer on which one or more epitaxial layers (optionally in combination with one or more metal contacts) can be subsequently formed. In some embodiments, the substrate can include a diameter of 150 mm or more, or 200 mm or more.
[0159] The methods disclosed herein can be applied to substrates of various crystalline materials, single crystal and polycrystalline varieties. In certain embodiments, the methods disclosed herein can utilize cubic, hexagonal and other crystal structures, and can involve crystalline materials with coaxial and off-axis crystal orientations. In certain embodiments, the methods disclosed herein can be applied to semiconductor materials and / or wide bandgap materials. Exemplary materials include, but are not limited to, Si, GaAs and diamond. In certain embodiments, such methods can utilize single crystal semiconductor materials with hexagonal crystal structures, such as 4H-SiC, 6H-SiC or III-group nitride materials (e.g., GaN, AlN, InN, InGaN, AlGaN, or AlInGaN). The various illustrative embodiments described below generally refer to SiC or specifically to 4H-SiC, but it should be understood that any suitable crystalline material can be used. Among various SiC polytypes, 4H-SiC polytypes are particularly attractive to power electronics due to their high thermal conductivity, wide bandgap and isotropic electron mobility. Bulk SiC can be grown on-axis (i.e., with no intentional angular deviation from its c-plane, suitable for forming undoped or semi-insulating materials) or off-axis (typically at a non-zero angle, typically in the range of from 0.5 to 10 degrees (or a sub-range thereof, such as 2 to 6 degrees), from a growth axis (such as the c-axis), as may be suitable for forming N-doped or highly conductive materials). The embodiments disclosed herein may be applied to on-axis and off-axis crystalline materials, as well as doped and unintentionally doped crystalline materials. Certain embodiments disclosed herein may utilize on-axis 4H-SiC or vicinal (off-axis) 4H-SiC with a bevel in the range of 1 to 10 degrees, or 2 to 6 degrees, or about 4 degrees.
[0160] Fig. 6A and Figure 6C On-axis and off-axis crystalline substrates in ingot form that can be used with the methods disclosed herein are schematically shown. Fig. 6A is a schematic side view of a coaxial ingot 15 of crystalline material having a first end face 16 and a second end face 17 perpendicular to the c-direction (ie, the
[0001] direction of a hexagonal crystal structure material such as 4H-SiC). Figure 6B yes Fig. 6A A schematic side view of an ingot 15 rotated four degrees is shown, wherein there is an overlay pattern 18 (shown by a dotted line) for cutting and removing the ends of the ingot 15 close to the end faces 16, 17. Figure 6C After the end portions are removed to provide new end faces 16A, 17A which are not perpendicular to the c direction, Figure 6BA side view schematic diagram of an off-axis ingot 15A formed from an ingot 15. If a laser shot of a first depth is supplied through an end face 16 of the ingot 15 to form subsurface laser damage, a carrier (not shown) is bonded to the end face 16, and the ingot 15 is fractured along the subsurface laser damage, an on-axis wafer can be formed. Conversely, if a laser shot of a first depth is supplied through an end face 16A of the off-axis ingot 15A to form subsurface laser damage, a carrier (not shown) is bonded to the end face 16A, and the ingot 15A is fractured along the subsurface laser damage, an off-axis wafer can be formed.
[0161] Although various substrates, carriers, adhesives, and rupture techniques are disclosed herein, it should be understood that, depending on the various arrangements of substrates, carriers, and / or bonding methods, one or more rupture techniques may be used alone, or any combination of rupture techniques may be used simultaneously and / or sequentially to achieve the desired separation.
[0162] Carrier characteristics
[0163] It is contemplated that supports are used with various support-assisted methods for separating crystalline materials along the subsurface laser damaged regions disclosed herein. Given the different methods disclosed herein for separating (ie, breaking) crystalline materials, the desired support properties may vary depending on the specific breaking method.
[0164] Various embodiments relate to carriers that are rigid in nature. In certain embodiments, at least a portion of the carrier close to the crystalline material to be separated or the entire rigid carrier comprises an elastic modulus (a / k / a Young's modulus) of at least about 20 GPa, at least about 50 GPa, at least about 100 GPa, at least about 200 GPa, or at least about 300 GPa. For example, sapphire has an elastic modulus of 345 GPa. The elastic modulus is a mechanical property that measures the stiffness of a solid material. It defines the relationship between stress (force per unit area) and strain (proportional deformation) in a material in a linear elastic state of uniaxial deformation.
[0165] Without wishing to be bound by any particular theory, the reason for the improved results of the separation methods disclosed herein relative to conventional methods (e.g., using low rigidity interface materials such as PDMS or silicone and low temperature fracture) is that it is believed that when a relatively rigid or hard (i.e., high elastic modulus) carrier is bonded to the crystalline material to fracture along the subsurface laser damaged region, the carrier can reduce wafer bending and / or fracture while providing repeatable crystalline material separation results. In addition to the mechanical aspects required for separation (e.g., by mechanical, CTE mismatch and / or ultrasonic means), the carrier also provides mechanical support during and after separation. This is useful for post-separation processes because the separated crystalline material can be ground, polished, etc. while remaining attached to and supported by a rigid carrier. This avoids the need to bond the wafer to a rigid carrier after fracture in order to perform one or more post-separation processing steps.
[0166] When a rigid carrier is bonded to a substrate with an adhesive, in certain embodiments, the carrier can include a wider range of materials, typically including semiconductors, inorganic materials, metals, metalloids, non-metals, ceramics, crystalline materials (e.g., single crystal or polycrystalline in nature), amorphous materials, polymeric materials, glasses, and composite materials. In certain embodiments, the carrier can include two or more materials bonded or joined together by various conventional means. As will be appreciated by those skilled in the art, other materials can be used.
[0167] When a rigid carrier is not limited to being bonded to a substrate with an adhesive, a narrower range of carrier materials may be desired. In certain embodiments, carriers that are not necessarily adhesively bonded to a rigid carrier may include single crystalline materials (e.g., single crystal or polycrystalline in nature), semiconductor materials, ceramic materials, metalloids, inorganic materials, and composite materials.
[0168] In certain embodiments, the thickness of the rigid carrier may exceed one, two, three, four, or five times the depth of the laser damage below the surface of the crystalline material bonded to the rigid carrier. In various embodiments, the rigid carrier may include a thickness less than, equal to, or greater than the thickness of the (pre-separated) crystalline material bonded to the rigid carrier. In certain embodiments, the rigid carrier may have a thickness of at least 500 μm, greater than 800 μm, at least 850 μm, at least 900 μm, at least 1 mm, at least 1.5 mm, at least 2 mm, or at least 3 mm, wherein the foregoing ranges are optionally bounded by upper limits of 1 mm, 2 mm, 3 mm, 4 mm, or 5 mm, as appropriate. In certain embodiments, the rigid carrier can have a thickness in the range of 0.5 mm to 5 mm, or 0.5 mm to 3 mm, or 0.5 mm to 2 mm, or 0.8 mm to 5 mm, or 0.8 mm to 3 mm, or 0.8 mm to 2 mm, or 0.85 mm to 5 mm, or 0.9 mm to 5 mm, or 1 mm to 4 mm, or 1 mm to 3 mm, or 1 to 2 mm.
[0169] In certain embodiments, the rigid carrier may desirably have a lateral extent (e.g., diameter, or length and width) that is at least as large as or exceeds the corresponding dimensions of the substrate to which it is bonded. It is believed that providing a rigid carrier having a diameter at least as large as (or larger than) the crystalline substrate helps to induce fracture during the various fracture processes described herein.
[0170] In some embodiments, at least one of the maximum length or maximum width of at least a portion of the rigid carrier exceeds the corresponding maximum length or maximum width of the substrate. In some embodiments, at least a portion of at least one edge of the rigid carrier can extend laterally beyond the corresponding at least one edge of the substrate by at least about 100 microns, at least about 200 microns, at least about 500 microns, at least about 1 mm, or at least about 2 mm. Such lateral superposition may be particularly desirable in embodiments utilizing mechanical separation, as the superposition may receive at least a portion of a tool suitable for applying a torque on the rigid carrier to induce fracture. In some embodiments, the substrate includes a notch or flat along at least one edge of the substrate, and at least a portion of the edge (or at least one edge) of the rigid carrier extends laterally beyond the notch or flat.
[0171] Embodiments including single and dual carriers are disclosed herein. As the substrate to be separated becomes thinner (e.g., less than about 5 mm thick), dual carriers become a practical need. A carrier arranged close to the laser damaged area below the surface may be referred to as a front carrier to distinguish it from a rear carrier arranged away from the laser damaged area below the surface. According to certain embodiments disclosed herein, the front carrier is specifically intended to promote the separation of crystalline materials along the laser damaged area below the surface or close to the laser damaged area below the surface. In contrast, the rear carrier is not intended to promote the separation of the substrate during the fracture process. To this end, when the CTE mismatch between the carrier and the substrate is used to promote the fracture of the substrate along the damaged area below the surface, the rear carrier may have a different CTE from the front carrier. In some embodiments, the rear carrier may have a smaller CTE mismatch relative to the substrate than the front carrier. In some embodiments, the rear carrier may be CTE matched or nearly CTE matched with the substrate.
[0172] CTE properties of carriers relative to crystalline materials
[0173] In certain embodiments, a rigid carrier having a first coefficient of thermal expansion, or CTE1, is bonded or joined to a surface of a crystalline material having subsurface laser damage and having a second coefficient of thermal expansion, or CTE2, wherein CTE1 is greater than CTE2 at a desired temperature (e.g., at 25° C.) or within a desired temperature range. Thereafter, at least the carrier is cooled such that the carrier shrinks more rapidly in size than the crystalline material due to the CTE difference. This differential shrinkage creates stresses (e.g., shear stresses) in the carrier as well as the crystalline material, and such stresses cause the crystalline material to fracture along the subsurface laser damaged region. Although the inventors have extensively tested SiC substrates in combination with sapphire carriers, other CTE-mismatched material combinations can be readily determined by one skilled in the art with the benefit of this disclosure.
[0174] In order to impart sufficient stress on the substrate, the CTE mismatched substrate according to various embodiments disclosed herein can be rigid in nature, taking into account not only the mechanical properties (e.g., elastic modulus) of the carrier material, but also the carrier thickness. In certain embodiments, the rigid carrier can include a thickness greater than 800 microns, at least 850 microns, at least 900 microns, at least 1 mm, at least 1.5 mm, or another threshold value disclosed herein.
[0175] For various materials, the CTE can vary with temperature. For a rigid carrier having a CTE greater than the CTE of a crystalline material, in certain embodiments, the rigid carrier can include a material having a CTE greater than the CTE of the crystalline material at a desired temperature (e.g., at 25°C, 100°C, 200°C, 300°C, 0°C, and / or -100°C) or within a desired temperature range (e.g., a range of -100°C to 300°C, a range of -100°C to 200°C, a range of -100°C to 100°C, a range of 0°C to 200°C, a range of 50°C to 150°C, or any other suitable temperature range or sub-range disclosed herein).
[0176] In certain embodiments, the CTE of the rigid carrier (to be disposed proximate to the subsurface damage region in the crystalline material substrate) is less than 5 times, no more than about 4 times, no more than about 3 times, no more than about 2 times, no more than about 1.5 times the CTE of the crystalline material substrate. In certain embodiments, the CTE of the rigid carrier is a multiplication factor in the range of about 1.25 to about 4 over the CTE of the crystalline material substrate. It is believed that some or all of the aforementioned CTE mismatch ratios are significantly less than the CTE mismatch ratios of materials used in conventional nickel-based or polymer-based exfoliation (separation) technologies (e.g., as described in the background section of the present disclosure). For example, the CTE mismatch ratio between nickel or nickel-containing metal (which can be used as a carrier) and SiC (which can be used as a crystalline material) can be at least 5 or more, and the CTE mismatch ratio between a polymer and SiC can be about 10 to 100 or more.
[0177] Although reference has been made to a rigid carrier having a CTE greater than and bonded to a crystalline material having subsurface damage, in certain embodiments, the crystalline material having subsurface laser damage may be disposed between a first rigid carrier and a second rigid carrier. In such embodiments, the first rigid carrier is bonded to a first surface of the crystalline material proximate to the subsurface laser damage, and the second rigid carrier is bonded to a second surface of the crystalline material opposite the first surface and away from the subsurface laser damage. In certain embodiments, both the first rigid carrier and the second rigid carrier may have a CTE value that exceeds the CTE of the crystalline material. In other embodiments, the CTE of the first rigid carrier is greater than the CTE of the crystalline material, while the CTE of the second rigid carrier is less than or equal to the CTE of the crystalline material. For example, in certain embodiments, the front side carrier for a SiC substrate may be sapphire, which exhibits a significant CTE mismatch relative to SiC, while the back side carrier may be SiC with no CTE mismatch relative to the CTE carrier. Alternatively, the front side carrier for a SiC wafer may be sapphire (which has a CTE greater than SiC), while the back side carrier may be SiC (with no CTE mismatch with the SiC wafer).
[0178] In certain embodiments where CTE mismatch is utilized to facilitate fracture, it may be desirable to provide the minimum amount of CTE mismatch required to achieve the desired separation in order to reduce the bowing of the bonded assembly (i.e., the carrier and the fractured substrate portion bonded thereto) after separation. When using SiC substrates and sapphire carriers, bowing of about 200 microns has been observed for 150 mm diameter SiC wafers. This degree of bowing is within a range that can be easily addressed via grinding due to both the mechanical forces applied by the vacuum chuck used during grinding and the grinding forces used to flatten the bonded assembly during processing. In contrast, excessive bowing is a major problem encountered with prior art processes.
[0179] One or more carriers combined with crystalline materials
[0180] Various methods can be used to bond or join a rigid carrier to the surface of a crystalline material having subsurface damage to promote fracture along the subsurface damage. One method includes adhesive bonding, which can involve applying an adhesive material to the proximal surface of the rigid carrier, matching the adhesive to the surface of the crystalline material having subsurface laser damage, and curing the adhesive (e.g., by subjecting the carrier / adhesive / crystalline material stack to elevated temperature and pressure).
[0181] In certain embodiments, the bond between the rigid carrier and the crystalline material having subsurface laser damage can be temporary in nature, such as by using an adhesive material that will maintain adhesion during certain conditions (e.g., room temperature) but will exhibit reduced adhesion during removal conditions (e.g., at temperatures sufficient to cause the adhesive material to flow and / or exposure to a chemical agent configured to weaken or dissolve the adhesive material). The use of a temporary bonding medium allows the crystalline material to be bonded to the carrier to achieve fracture according to the methods disclosed herein (e.g., thermally induced fracture at low temperatures, fracture induced by application of mechanical forces, and / or fracture induced by application of ultrasonic energy), but allows the removed portion of the crystalline material adhered to the rigid carrier to be removed thereafter (optionally, after one or more other processing steps are performed on the crystalline material portion while attached to the rigid carrier). The desired properties of the adhesive material that can be used in various embodiments of the present disclosure can depend in part on the method used to induce fracture of the crystalline material.
[0182] Important parameters of temporary bonding materials may include (a) cohesive strength, (b) adhesive strength, (c) elastic modulus, (d) glass transition temperature, and (e) thickness. Suitable temporary bonding materials (e.g., temporary adhesives) should have an appropriate combination of the foregoing parameters to effectively transfer separation forces between the carrier and the crystalline material to achieve fracture along the subsurface damaged area, wherein and such bonding materials are still easily removed, destroyed or inoperable under certain conditions (e.g., chemical degradation, photon degradation, thermal degradation, etc.) - preferably without excessive effort to remove the residue.
[0183] In terms of cohesive strength, the desired bonding material should have a sufficiently high cohesive strength so that the bonding material maintains its integrity and does not separate when subjected to the force required to destroy the crystalline material having subsurface laser damage. The bonding strength of the bonding material should be high enough to maintain adhesion to the surrounding material (e.g., the carrier or crystalline material) when the bonding material is subjected to the force required to destroy the crystalline material having subsurface laser damage. It should be noted that some bonding materials exhibit reduced adhesive and cohesive strengths at lower temperatures, so it may be desirable to employ a fracture technique involving relatively higher temperatures.
[0184] With respect to the elastic modulus and thickness of the bonding material, the desired bonding material should be used to appropriately transfer an appropriate amount of stress from the carrier to the crystalline material without requiring the bonding material to absorb an excessive amount of stress required to achieve fracture of the crystalline material. This tends to favor relatively high modulus (i.e., relatively hard) bonding materials present in relatively thin layers to promote stress transfer while inhibiting the bonding material from absorbing stress.
[0185] With respect to the glass transition temperature (Tg), the lower the Tg value, the lower the temperature to which the carrier must be cooled to achieve fracture (e.g., spontaneous fracture) of the crystalline material along the subsurface laser damaged region when relying on the CTE mismatch between the carrier and the crystalline material. For example, if the Tg of the bonding material is 0°C, and a temperature change of 70°C is desired to introduce sufficient stress, the carrier must be cooled to -70°C. Unfortunately, at very low temperatures, bonding material properties (including stress transfer efficiency) may deteriorate. Therefore, bonding materials exhibiting relatively high Tg values may be preferred for use in embodiments of the present disclosure.
[0186] In some embodiments, the adhesive material may include an adhesive that is compatible with high temperature hot press adhesive bonding. For high temperature hot press bonding, a lower glass transition temperature (Tg) is desirable to avoid very high temperature bonding requirements and prevent the separated crystalline material portion / rigid carrier assembly from having excessive bending at room temperature. However, in some embodiments, the Tg of the adhesive material should not be too low, particularly when used in embodiments that utilize cooling in conjunction with substrate / carrier CTE mismatch to achieve crystalline material fracture, because the low Tg material may undesirably absorb excessive substrate / carrier CTE mismatch stresses upon cooling before the Tg crosses. The glass transition temperature of a polymer material is the temperature region where the polymer transforms from a hard, glassy material to a soft, rubbery material.
[0187] In some embodiments, the adhesive material may include an adhesive that can be cured with ultraviolet (UV) light. For such adhesives, a higher Tg may be used because the adhesive bond can be formed at room temperature (e.g., about 25° C.), thereby minimizing any residual stress in the resulting separated material at room temperature. In some embodiments, a UV-curable adhesive bond can be formed above room temperature so as to produce a desired level of residual stress at room temperature in embodiments where a cooling bonding substrate / carrier CTE mismatch is used to achieve crystalline material fracture. In such embodiments, residual stress may be desirable to reduce the temperature difference required to achieve separation through a CTE mismatch between the carrier and the portion of the crystalline material adhered thereto.
[0188] In certain embodiments where the fracture is achieved by cooling and CTE mismatch between the carrier and the crystalline material adhered thereto, the bonding material may have a glass transition temperature (Tg) of about 25°C or greater, greater than 50°C, greater than 75°C, greater than 100°C, or greater than 150°C, taking into account different adhesive bonding and / or curing processes. In certain embodiments, the aforementioned lower threshold may be bounded from above (where appropriate) by an upper threshold of less than about 250°C, less than about 200°C, less than about 150°C, less than about 125°C, or less than about 100°C. Further, in certain embodiments, the bonding material may have a melting point of greater than 50°C, greater than 100°C, greater than 150°C, or greater than 200°C, taking into account different adhesive bonding and / or curing processes.
[0189] In certain embodiments, the adhesive material comprises a thermoplastic adhesive. At least some thermoplastic adhesives can exhibit desired mechanical and adhesive properties (relatively high Tg, high elastic modulus, high cohesive strength, high adhesion strength to desired carriers and crystalline materials, and hardness in a desired temperature range (e.g., near room temperature)), while still being easily removable when heated to elevated temperatures and / or exposed to solvents. Examples of adhesive materials that may be suitable for use with the methods disclosed herein may include commercially available from Brewer Science, Inc. (Rolla, Missouri, USA). 220, HT-10.10 and 305 thermoplastic adhesive and Crystalbond commercially available from Aremco Products (Valley Cottage, NY, USA) TM 509 Thermoplastic Adhesives. Selected thermal and mechanical property values for these adhesives are shown in the table below.
[0190]
[0191] In the above table, the hardness values of the films of the first adhesive and the second adhesive are provided by the manufacturer, wherein such values are typically determined using the value expressed in Pascals (e.g., MPa or GPa) using the nanoindenter method, and the hardness value of the fourth adhesive is expressed as the hardness determined by the applicant using the Shore D method. The applicant calculates the elastic modulus value of the fourth adhesive from the Shore D durometer value. Although there is no direct theoretical relationship between the scale of Shore modulus and Young's modulus, there is an empirically derived mathematical formula that is useful for conversion between them. The formula used by the applicant (using Microsoft Excel) is "EXP ((Durometer + 50) * 0.0235-0.6403)", wherein Durometer refers to the Shore D durometer value. The fourth adhesive material (Crystalbond TM509) has a Shore D durometer value of 73.2, which is between solid truck tires (having a Shore D value of about 50) and high-density polyethylene safety covers (having a Shore D value of about 75) and Shore D durometer values. In addition, the Shore D hardness value of the fourth adhesive material is significantly higher than the Shore D hardness of 50.51 and 54.25 measured by the wax tested by the applicant (i.e., SHIFTWAX 7607 commercially available from NIKKA Seiko and Galaxy Wax commercially available from Galaxy Technologies, respectively), and it is determined using the thermally induced spontaneous separation method and the mechanically induced separation method described herein that it is not suitable for inducing the fracture of crystalline materials along the damaged area under the surface. It is determined that the wax material has a cohesive strength that is not enough to cause fracture, wherein the wax material is observed to separate within the wax itself. This is consistent with the online description, indicating that the wax has a very weak intermolecular attraction (London force) so that it cannot be held very strongly on other molecules.
[0192] Other adhesives other than the thermoplastic materials described above can be used, as will be recognized by those of ordinary skill in the art after reviewing the present disclosure. In certain embodiments, the adhesive material may include a glass transition temperature greater than 0°C, greater than 5°C, greater than 10°C, greater than 20°C, greater than 25°C, greater than 30°C, greater than 35°C, or any suitable higher threshold. In certain embodiments, the aforementioned lower threshold can be defined from above (where appropriate) by an upper threshold less than about 250°C, less than about 200°C, less than about 150°C, less than about 125°C, or less than about 100°C. Such adhesive materials can avoid the need to be cooled to significantly low temperatures (e.g., less than -75°C or less than -100°C, requiring liquid nitrogen or similar coolants). When using liquid nitrogen to reach very low temperatures below negative 100°C, the inventors have observed catastrophic adhesive failures using thermoplastic adhesive materials previously disclosed herein, depending on exposure time. Such thermoplastic materials appear to experience cracking and crazing at very low temperatures, indicating that significantly low temperatures (eg, minus 100° C. or lower) should be avoided.
[0193] One class of bonding materials that need to be cooled to significantly low temperatures is silicone (including PDMS), which has a glass transition temperature (Tg) range of -110°C to -140°C. Silicone may be difficult to remove easily. Silicone exhibits a very low elastic modulus above its glass transition temperature, but when the material is cooled below its glass transition temperature, this modulus changes by orders of magnitude to the GPa range. The inventors tested silicone as a bonding material between a SiC ingot and a sapphire carrier, attempting to induce spontaneous fracture due to CTE mismatch along the subsurface laser damaged area by cooling the carrier to a temperature of about -110°C. Fracture was not successfully achieved. It is speculated that during the cooling of the sapphire carrier, the bonding material, and the SiC ingot, the silicone material acts as a stress absorber, and when the Tg of the silicone is reached, the CTE mismatch between the carrier and the crystalline material is not high enough. Although the CTE mismatch between the sapphire carrier and the SiC ingot is significant at room temperature, the CTE mismatch is reduced to a relatively small value at a low temperature of -110°C. That is, even assuming that silicone does exhibit effective stress transfer properties, it may still be beneficial to avoid the ultra-low temperatures (e.g., liquid nitrogen temperatures) used to separate device wafers, as exposure to ultra-low temperatures may cause damage to the devices.
[0194] In certain embodiments, the bonding material may include a chemically cross-linked adhesive such as an epoxy. In certain embodiments, a multi-part reactive catalyst-type binder (eg, a two-part epoxy) may be used to bond the rigid carrier and the crystalline material substrate.
[0195] Although any suitable thickness of adhesive material layer can be used, in certain embodiments, the adhesive layer can be relatively thin (e.g., less than about 100 microns, less than about 50 microns, less than about 40 microns, less than about 30 microns, less than about 20 microns, or less than about 10 microns (where any of the above upper thresholds are optionally limited by lower thresholds of at least about 2 microns, at least about 5 microns, or at least about 10 microns, as appropriate)). Providing a thin adhesive layer can facilitate a more direct transfer of shear stresses between the rigid carrier and the crystalline material during fracture, thereby reducing the force and time required to complete the fracture. However, the optimal adhesive thickness can depend on multiple factors, such as, the elastic modulus of the adhesive, the bonding method, the separation technique, etc.
[0196] Given that there are different types of adhesives that can be used to join the rigid carrier and the crystalline material, a variety of adhesive bonding methods can be employed. In certain embodiments, hot pressing (involving the application of compressive forces at elevated temperatures) can be used. In one example, a force of 1800N to 3000N can be applied to a 150mm diameter crystalline material substrate (e.g., 4HSiC) secured to a rigid carrier (e.g., of single crystal sapphire) by an adhesive during exposure to a temperature of 180°C. In certain embodiments, a compressive force can be applied during UV emission of a UV-curable adhesive material between the rigid carrier and the crystalline material substrate. When a liquid or flowable bonding medium is used, in certain embodiments, the bonding medium can partially extend upward along the sidewalls of the crystalline material substrate (and along the proximal surface of the rigid carrier) when squeezed out during bonding to form a peripheral lip around at least a portion (or all) of the periphery of the crystalline material, wherein such a peripheral lip can be used to slightly increase the bonding strength between the substrate and the carrier.
[0197] In certain embodiments, plasma activated anodic bonding or any other suitable anodic bonding process may be used to bond the rigid carrier and the crystalline material substrate. For all purposes, details regarding anodic bonding between the crystalline material substrate and the carrier are disclosed in U.S. Patent Application Publication No. 2016 / 0189954, the contents of which are incorporated herein by reference.
[0198] In some embodiments, to facilitate bonding, the proximal surface of the rigid support and / or crystalline material may be roughened, textured, and / or surface activated by any suitable method prior to bonding (e.g., including adhesive bonding). Examples of surface treatments that may be performed include, but are not limited to, micropatterning, mechanical abrasion, chemical etching, reactive ion etching, and plasma treatment. In some embodiments, the rigid support may include single crystal sapphire having a micropatterned surface.
[0199] In certain embodiments, the rigid carrier may include one or more features configured to facilitate debonding when it is desired to remove a (previously separated) portion of a crystal adhered to the carrier. Examples of such features may include perforations and / or micropatterned surfaces to provide holes or cavities disposed proximal to and / or allowing fluid communication with the proximal surface of the rigid carrier.
[0200] Various processes can be used to promote the debonding between a (previously separated) portion of the crystalline material and the rigid carrier. In some embodiments, thermal debonding, mechanical debonding, chemical debonding and / or photonic debonding can be used. In some embodiments, debonding can be performed by thermal slippage, which involves heating the adhesive bonding assembly to a temperature sufficient to soften and / or flow the adhesive material, and when the rigid carrier is fixed in place (e.g., held by a vacuum chuck), an external shear stress can be applied to the portion of the crystalline material to cause the portion to slide laterally away from the rigid carrier. In some embodiments, the adhesive can include a UV absorbing material, whereby the impact of UV emission on the adhesive after separation can be used to cause degradation of the adhesive between the crystalline material portion and the carrier (e.g., by heating), thereby allowing the crystalline material portion to be removed. The chemical removal of the adhesive can utilize any suitable one or more chemical reagents sufficient to reduce adhesion and / or dissolve the adhesive material. If chemical debonding is used, one or more access openings (e.g., perforations) can be provided in the carrier to enable chemicals to contact the adhesive material.
[0201] Subsurface laser damage formation
[0202] Tools for forming laser subsurface damage in crystalline materials are known in the art and are commercially available from various suppliers, such as Disco Corporation (Tokyo, Japan). Such tools allow laser emission to be focused within the interior of a crystalline material substrate and enable the laser to be moved laterally relative to the substrate. Typical laser damage patterns include the formation of parallel lines that are laterally spaced relative to each other at a depth within the crystalline material substrate. Parameters such as focus depth, laser power, translation speed, and subsurface damage line spacing can be adjusted to impart laser damage, but adjustment of certain factors requires trade-offs. Increasing laser power tends to impart greater subsurface damage, which may increase the ease of fracture (e.g., by reducing the stress required to complete the fracture), but greater subsurface damage increases surface irregularities along the surfaces exposed by the fracture, such that additional processing may be required to smooth these surfaces sufficiently for subsequent processing (e.g., for incorporation into electronic devices). Reducing the lateral spacing between subsurface laser damage lines can also increase the ease of fracture, but reducing the spacing between laser damage lines increases the number of translation passes between the substrate and the laser, thereby reducing tool throughput.
[0203] Figure 7is a perspective schematic diagram of an example of a laser tool 29 configured to focus laser emissions within a crystalline material 30 to form subsurface damage 40. The crystalline material 30 includes an upper surface 32 and an opposing lower surface 34, and the subsurface damage 40 is formed in the interior of the crystalline material 30 between the upper surface 32 and the lower surface 34. If the crystalline material includes SiC, the upper surface 32 through which the laser emissions are directed may be a C-terminated surface. The laser emissions 36 are focused with a lens assembly 35 to produce a focused beam 38, wherein its focus is within the interior of the crystalline material 30. Such laser emissions 36 may be pulsed at any suitable frequency (typically in the nanosecond, picosecond, or femtosecond range) and beam intensity, wherein the wavelength is below the band gap of the crystalline material 30 to allow the laser emissions 36 to be focused at a target depth below its surface. At the focus, the beam size and short pulse width result in a highly localized absorption of energy density high enough to result in the formation of subsurface damage. One or more characteristics of the lens assembly 35 may be varied to adjust the focus of the focused beam 38 to a desired depth within the crystalline material 30. Relative lateral movement (e.g., lateral translation) between the lens assembly 35 and the crystal material 30 can be achieved to propagate the subsurface damage 40 in a desired direction, as schematically shown by the dashed line 42. This lateral movement can be repeated in various patterns, such as FIG. 8A to FIG. 8D shown.
[0204] FIG. 8A to FIG. 8D An exemplary laser tool travel path relative to a crystal material is provided for forming subsurface damage within the crystal material. In some embodiments, a laser tool portion (e.g., including a lens assembly) can be configured to move while the crystal material is stationary; in other embodiments, the laser tool portion can remain stationary while the crystal material moves relative to the tool portion. Fig. 8A A y-direction linear scanning motion 52 suitable for patterning subsurface damage in laterally spaced parallel lines within the first crystalline material 50A is shown. Figure 8B Y- and x-direction linear scanning movements 52, 54 are shown which are adapted to form subsurface damage in a pattern of a first set of laterally spaced parallel lines that intersects a second set of laterally spaced parallel lines within the second crystalline material 50B. Figure 8C Circular movement 56 suitable for forming subsurface damage in a concentric circular pattern within the third crystalline material 50C is shown. Fig.8D A y-direction linear scanning motion 56 is shown over (and beyond) the entire surface of the crystalline material 50D, which is sufficient to form a subsurface parallel laser damage line distributed through the crystalline material 50D, wherein the damage line is perpendicular to the hexagonal crystal structure of the crystalline material 50D. Other subsurface damage patterns (e.g., spiral, honeycomb, herringbone, etc.) can be formed if desired.
[0205] In certain embodiments, the crystalline material processing method as disclosed herein may include some or all of the following items and / or steps. A second carrier wafer may be attached to the bottom side of a crystalline material substrate (e.g., an ingot). Thereafter, the top side of the crystalline material substrate is ground or polished to provide an average surface roughness Ra of less than about 5 nanometers, thereby preparing a surface for transmitting laser energy. Then, laser damage may be applied at one or more depths required within the crystalline material substrate, wherein the spacing and direction of the laser damage traces depend on the crystal orientation of the crystalline material substrate as appropriate. The first carrier is bonded to the top side of the crystalline material substrate. An identification code or other information linked to the first carrier is associated with the wafer to be obtained from the crystalline material substrate. Alternatively, a laser mark may be applied to the wafer (not the carrier) before separation to facilitate traceability of the wafer during and after manufacturing. The crystalline material substrate is then broken along the subsurface laser damage region (using one or more methods described herein) to provide a portion of the crystalline material substrate bonded to the first carrier and the remainder of the crystalline material substrate bonded to the second carrier. The removed portion of the crystalline material substrate and the remainder of the crystalline material substrate are ground smooth and cleaned as needed to remove residual subsurface laser damage. The removed portion of the crystalline material substrate can be separated from the carrier. After this, the process can be repeated using the remaining portion of the crystalline material substrate.
[0206] While wire sawing of SiC wafers typically requires a kerf loss of at least about 250 microns per wafer, the laser and carrier assisted separation methods disclosed herein and applied to SiC can achieve kerf losses in the range of 80 to 140 microns per wafer.
[0207] Fig. 9is a side cross-sectional schematic diagram of an assembly 58 including a crystalline material substrate 60 having a subsurface laser damage 66 and bonded to a rigid carrier 72 via an intermediately disposed adhesive material layer 68. The assembly 58 is adapted to facilitate removal of a portion of the crystalline material substrate 60 along the subsurface laser damage 66 by fracturing the crystalline material substrate 60 along the subsurface laser damage 66 using any one or more of the methods disclosed herein. The crystalline material substrate 60 includes a first surface 62 proximate to the adhesive material 68 and includes an opposing second surface 64, wherein the subsurface laser damage 66 is closer to the first surface 62 than the second surface 64. The rigid carrier 72 also includes a first surface 73 proximate to the adhesive material 68 and a second surface 74 opposing the first surface 73. The adhesive material 68 extends between the first surface 62 of the crystalline substrate 60 and the first surface 73 of the rigid carrier 72. As shown, an exposed adhesive lip 70 is disposed around at least a portion (or optionally, all) of the perimeter of the crystalline material substrate 60, proximate to the first surface 62 of the crystalline material substrate 60. In some embodiments, the rigid carrier 72 includes a material having a CTE greater than the CTE of the crystalline material substrate 60 within a desired temperature range, and fracture of the crystalline material 60 can be induced by exposing at least the rigid carrier 72 (or the carrier and substrate 60) to a cryogenic medium (e.g., a cooling liquid) or conditions.
[0208] Rigid carrier fracture with carrier / substrate CTE mismatch by cooling
[0209] FIG. 10A to FIG. 10F Steps of a semiconductor processing method utilizing a CTE-mismatched rigid carrier bonded to a crystalline material are shown according to one embodiment of the present disclosure. Fig. 10A is a schematic side cross-sectional view of a rigid carrier 72 having an adhesive material layer 68 bonded to a first surface 73 of the rigid carrier 72 and having a second surface 74 opposite the first surface 73. To promote better adhesion to the first surface 73, such surface may be etched (e.g., by reactive ion etching) prior to applying the adhesive material 68. The adhesive material 68 may be applied by any suitable method, such as spin coating, spray coating, dip coating, roller coating, etc.
[0210] Fig. 10B Yes Fig. 10A Schematic cross-sectional view of an assembly 58' of a rigid carrier 72 and bonding material 68 bonded to a crystalline material substrate 60 having a subsurface laser damaged region 66 therein. As shown, the rigid carrier 72 has a larger diameter or lateral extent than the crystalline material substrate 60. Fig. 10B The component 58' is similar to Fig. 9 Components shown, but missing Fig. 9 Exposed adhesive lip shown. Continue to reference Fig. 10B, the crystalline material substrate 60 includes a first surface 62 proximate to the bonding material 68, and includes an opposing second surface 64, wherein the subsurface laser damage 66 is closer to the first surface 62 than the second surface 64 of the substrate 60. The rigid carrier 72 also includes a first surface 73 proximate to the bonding material 68, such that the bonding material 68 extends between the first surface 62 of the crystalline substrate 60 and the first surface 73 of the rigid carrier 72. The bonding material 68 can be cured according to the requirements of the selected bonding method (e.g., high temperature hot pressure adhesive bonding, compression assisted UV bonding, chemical reaction bonding, etc.). Although the second surface of the crystalline material substrate 60 is shown as being exposed, in some embodiments, a second carrier (not shown) can be bonded (temporarily or permanently) to the second surface 64 of the substrate 60, wherein the second carrier is optionally not wider than the substrate 60 and / or CTE matched to the substrate 60.
[0211] Fig. 10C After positioning the second surface 74 of the rigid carrier 72 on the support surface 78 of the cooling device Fig. 10B FIG. 1 is a cross-sectional schematic diagram of an assembly of a rigid carrier 72, the cooling device being in the form of a cooling chuck 76 configured to receive a cooling liquid. The contact between the rigid carrier 72 and the cooling chuck 76 causes heat to be transferred from the rigid carrier 72 to the cooling chuck 76, causing the rigid carrier 72 to cool rapidly. During this cooling process, the rigid carrier 72 will shrink laterally to a greater extent than the crystalline material substrate 60, thereby applying shear stress on the crystalline material substrate 60. Due to the presence of subsurface laser damage 66 near the adhesive layer 68 that bonds the rigid carrier 72 to the crystalline material substrate 60, the application of shear stress on the substrate 60 causes the crystalline material to fracture along or close to the subsurface laser damage region 66.
[0212] In some embodiments, the cooling chuck 76 has a smaller diameter than the diameter of the rigid carrier 72. It has been found that only the second surface 74 from the rigid carrier 72 is required, and only the central portion of the rigid carrier 72 may need to be covered. Fig. 10CCooling of the components to produce a temperature difference both laterally (i.e., from the center to the edge) and vertically (i.e., from the crystalline material substrate 60 to the rigid carrier 72). Although the cooling chuck 76 can be supplied with a cooling liquid, the rigid carrier 72 does not have to reach liquid nitrogen temperature (-160°C) to successfully complete the thermal fracture of the crystalline material substrate 60. Favorable separation results have been obtained by fracture of a single SiC material supported by a crystallized sapphire substrate using a cooling chuck maintained at -70°C. Such temperatures can be maintained using various cooling liquids received from a two-phase pumped evaporative cooling system (such as liquid methanol, which remains flowable above its freezing point at -97°C). Favorable separation results have also been obtained by cooling the carrier, adhesive and substrate in a refrigerator maintained at -20°C, where such temperatures can be maintained using a single-phase evaporative cooling system. The ability to use a single-phase evaporative cooling system or a two-phase pumped evaporative cooling system instead of liquid nitrogen significantly reduces operating costs.
[0213] Fig. 10D 6 is a schematic cross-sectional view of the remaining portion of the crystalline material substrate 60A separated from the bonded assembly (on top of the liquid cooling chuck 76) including the rigid carrier 72, the bonding material 68, and a portion of the crystalline material 80 removed from the remaining portion of the substrate 60A after the crystalline material has been fractured along the subsurface laser damaged region. The remaining portion of the crystalline material substrate 60A is defined by a new first surface 63 (with residual laser damage 66A) opposite the second surface 64. Correspondingly, the removed portion of the crystalline material 80 is defined by a new second surface 82 (with residual laser damage 66B) opposite the first surface 62. Thereafter, the bonded assembly 85 including the rigid carrier 72, the bonding material 68, and the removed portion of the crystalline material 80 can be withdrawn from the cooling chuck 76.
[0214] Fig. 10E yes Fig. 10D Schematic cross-sectional view of the bonded assembly 85 after being extracted from the liquid-cooled chuck 76. Remaining the removed portion of the crystalline material 80 attached to the rigid carrier 72 advantageously provides mechanical support for the removed portion of the crystalline material 80 to allow one or more surface processing steps (e.g., grinding, polishing, etc.) to be performed on the new surface 82 to remove the residual laser damage 66B and achieve the desired thickness of the crystalline material 80 (e.g., by grinding, optionally followed by chemical mechanical planarization (CMP) and / or various polishing steps). In some embodiments, laser damage removal and thinning can include sequential grinding / polishing operations with a 2000 grit polishing pad and a 7000 grit polishing pad, as well as any appropriate polishing and cleaning steps to prepare the new surface 82 for subsequent operations (e.g., surface implantation, laser marking (e.g., close to the wafer plane), formation of epitaxial layers, metallization, etc.).
[0215] Fig.10F8 is a cross-sectional schematic diagram of a removed portion of a crystalline material 80 supported by an upper surface 88 of a heated vacuum chuck 86, wherein a rigid carrier 72 and an adhesive material 68 are laterally translated away from the removed portion of the crystalline material 82 after softening at an elevated temperature and releasing the adhesive material 68. That is, the heated vacuum chuck 86 can heat the adhesive material 68 to a sufficient temperature to soften and / or flow so that when an external shear stress is applied to the second surface 74 of the rigid carrier 72, the rigid carrier 72 is allowed to laterally translate away from the removed portion of the crystalline material 82 temporarily held in place by the heated vacuum chuck 86. Thereafter, the heated vacuum chuck 86 can be deactivated and the removed portion of the crystalline material 82 is embodied as a self-supporting material. If desired, any residue from the adhesive 68 can be removed and cleaned from the first surface 73 of the rigid carrier 72, and the rigid carrier 72 can optionally be reused for another fracture operation. The removed crystalline material can then be used as a growth substrate for depositing one or more epitaxial layers and conductive metal layers to form a device wafer, which is then singulated to form discrete semiconductor devices.
[0216] In certain embodiments, a cooled chuck may be placed in a coolant bath (e.g., a bath of liquid nitrogen or other coolant liquid such as methanol received from a pumped evaporative cooling system) to achieve thermally induced fracture of a crystalline material substrate supported by a suitably CTE-mismatched rigid carrier.
[0217] Fig.11 is based on Fig. 10C Schematic cross-section of an assembly of on a cooling device in the form of a cooling chuck 76A disposed in a bath of cooling liquid 79 (e.g., methanol or liquid nitrogen received from a pumped evaporative cooling system). An adhesive material 68 is disposed between a rigid carrier 72 and a crystalline material substrate 60 having a subsurface laser damaged region 66, the subsurface laser damaged region being closer to a first surface 62 contacting the adhesive material 68 than an opposing second surface 64 of the substrate 60, and the first surface 62 contacting the adhesive material 68. The rigid carrier 72 includes a first surface 73 contacting the adhesive material 68 and an opposing second surface 74 disposed in contact with a support surface 78A of the cooling chuck 76A. The diameter of the cooling chuck 76A is smaller than the diameter of the rigid carrier 72. The cooling chuck 76A is disposed in a coolant bath (e.g., a liquid nitrogen bath) sufficient to reduce the temperature of the cooling chuck 76A to or near the coolant temperature. In some embodiments, the cooling chuck 76A and the coolant bath 79 can be arranged in a closable insulating container (not shown), whereby the container can be selectively opened to allow a rigid carrier 72 with an attached adhesive material 68 and a crystalline material substrate 60 with subsurface laser damage 66 to be placed in contact with the cooling chuck 76A to rapidly fracture the single crystal material substrate 60 along the subsurface laser damage region 66.
[0218] Fig.12 is a perspective view of a cooling apparatus 90 comprising a container 92 having a cylindrical side wall 94 defined by a bottom wall 96, wherein a chuck 100 is supported above the bottom wall 96 by a thermally conductive spacer 98 (e.g., an aluminum rail). Although the chuck 100 is of a type sufficient to apply suction to a workpiece, it is not necessary to provide a vacuum suction function (provided by a suction port 102 configured to be connected to a vacuum source and perforations 104 arranged along an upper surface 106 of the chuck) during the cooling operation. In use, cooling liquid can be supplied to the container 92 to contact the spacer 98, but not necessarily to contact the entire width of the chuck 100 itself. Heat can be transferred from the chuck 100 to the cooling liquid through the thermally conductive spacer 98. In experiments, a vacuum chuck 100 according to the design shown has been maintained at a temperature of approximately -70°C. As shown Fig. 10B The carrier side of the assembly 58' shown in the figure can be placed on the chuck upper surface 106 to allow the rigid carrier to be rapidly cooled. Due to the CTE mismatch between the carrier and the crystalline material substrate adhered thereto, thermally induced fractures will be induced along the subsurface laser damaged region. In the absence of mechanical intervention, the inventors have observed spontaneous separation of 4H-SiC using the thermoplastic adhesive disclosed herein at temperatures up to about -20°C.
[0219] Support shape and positioning relative to the crystalline material
[0220] As discussed previously, the rigid carrier(s) may desirably have lateral dimensions (e.g., diameter, or length and width) that are at least as large as or greater than corresponding dimensions of a substrate to which they are bonded when used with the methods disclosed herein. FIG. 13A to FIG. 13E is a top view of a bonded assembly comprising carriers of different shapes each bonded to a substrate of a crystalline material, wherein Fig.13F and 13G Provided separately Fig.13D and 13E A side cross-sectional view of a combined assembly. Fig.13A A first bonded assembly 110 is shown including a generally circular substrate 112 having a flat portion 114 and a rounded portion 116 opposite the flat portion 114 , wherein the substrate 112 is bonded to a square carrier 118 that is generally concentric with the substrate 112 . Fig. 13B A second bonded assembly 120 is shown of a generally circular substrate 122 having a flat portion 124 and a rounded portion 126 opposite the flat portion 124, wherein the substrate 122 is bonded to a circular carrier 128 that is generally concentric with the substrate 122. Due to the presence of the flat portion 124 that locally reduces the diameter of the substrate 122, a larger border portion 129 of the carrier 128 is disposed proximate to the flat portion 124. Fig. 13CA third bonded assembly 130 is shown of a generally circular substrate 132 having a flat portion 134 and a rounded portion 136 opposite the flat portion 134, wherein the substrate 132 is bonded to a circular carrier 138 that is not concentric with the substrate 132, such that the rounded portion 136 of the substrate 132 is substantially closer to the edge of the carrier 138 than the remainder of the substrate 132. A larger border portion 139 of the carrier 138 will exist opposite the rounded portion 136 even if the flat portion 134 is not present, but the border portion 139 of the carrier 138 will be even larger than the rounded portion 136 if the flat portion 134 is present. Fig. 13B The presence of a locally enlarged border at one region and a locally reduced border at an opposing region may be advantageous in allowing mechanical breaking of a substrate 132 bonded to a carrier 138 in certain embodiments, wherein the locally enlarged border accommodates the presence of a prying tool (not shown), and the locally reduced border provides a limited overhang that may otherwise resist tilting motion of the upper substrate (depending on the geometry of the separation apparatus).
[0221] Fig.13D and Fig.13F A fourth bonded assembly 140 is shown including a generally circular substrate 142 having a flat portion 144 and a rounded portion 146 opposite the flat portion 144, wherein the substrate 142 is bonded to a primarily circular carrier 148 that is substantially concentric with the substrate 142, but wherein the carrier 148 includes a single laterally protruding lug portion 149 that provides a localized enlarged boundary proximate to the flat portion 144 of the substrate 142. The laterally protruding lug portion 149 of the carrier 148 can be aligned with the flat portion 144 to allow application of a localized mechanical force in such a manner as to apply a bending moment in a direction perpendicular to the flat portion 144 that tends to induce fracture. Fig.13F As shown, a second carrier 148' of the same or different shape may be provided below substrate 142, with subsurface laser damaged region 143 closer to upper carrier 148. The presence of lug portion 149 allows a single prying tool (not shown) to be inserted between carriers 148, 148'.
[0222] Fig.13E and 13GA fourth bonded assembly 150 is shown including a generally circular substrate 152 having a flat portion 154 and a rounded portion 156 opposite the flat portion 154, wherein the substrate 152 is bonded to a primarily circular carrier 158 that is substantially concentric with the substrate 152, but wherein the carrier 158 includes opposing first and second lateral tab portions 159A, 159B that provide locally enlarged border regions, wherein one of the locally enlarged border regions is proximate to the flat portion 154 of the substrate 152. The laterally projecting tab portions 159A, 159B of the carrier 158 may be aligned with the flat portion 154 to allow application of a localized mechanical force in such a manner as to apply a bending moment in a direction perpendicular to the flat portion 154 that tends to induce fracture. Figure 13G As shown, a second carrier 158' of the same or different shape may be provided below the substrate 152, with the subsurface laser damaged region 153 closer to the upper carrier 158. The presence of the laterally protruding lug portions 159A, 159B allows a tool (not shown) to be inserted between the carriers 158, 158' to apply a mechanical force. FIG. 15A to FIG. 15D and FIG. 16A to FIG. 16B Additional details regarding the application of mechanical forces to initiate fracture of crystalline materials along subsurface laser damaged regions are discussed.
[0223] Although Fig.13F and Figure 13G The upper and lower carriers 148, 148', 158, 158' are shown to have lateral dimensions that exceed the lateral dimensions of the substrates 142, 152, it being understood that in some embodiments, the lower carriers 148', 158' are no larger than the corresponding substrates 142, 152 (for example, if the substrates 142, 152 are held by a vacuum chuck or other device) to provide a basis for resisting mechanical forces applied to the upper carriers 148, 158.
[0224] Fragmentation induced by ultrasonic energy
[0225] Another method for achieving fracture along a laser-induced subsurface damaged region of a crystalline material bonded to a rigid carrier involves applying ultrasonic energy to the crystalline material while in the bonded state. Fig.14is a cross-sectional schematic diagram of an assembly 58A including a crystalline material 60A having subsurface laser damage 66A' and bonded to a rigid carrier 72A using an intermediate bonding material 68A, wherein the assembly 58A is disposed in a liquid bath 165 of an ultrasonic generator device 160. The device also includes a container 162 disposed in contact with an ultrasonic generating element 164, wherein the container 162 contains a liquid bath 165. The presence of the rigid carrier 72A can reduce or eliminate the cracking of the crystalline material 60A when subjected to ultrasonic energy, particularly if residual stress remains between the rigid carrier 72A and the crystalline material 60A prior to separation (e.g., due to CTE mismatch). Such residual stress can reduce the amount of ultrasonic energy required to initiate fracture of the crystalline material, thereby reducing the likelihood of fracture of the material. In this regard, it should be noted that a combination of two or more fracture techniques (e.g., CTE mismatch and ultrasonically induced fracture; or CTE mismatch and mechanically induced fracture; or ultrasonically induced and mechanically induced fracture) is particularly contemplated. In certain embodiments, the liquid of the ultrasonic bath can be cooled before or during the application of ultrasonic energy.
[0226] Mechanically induced fracture
[0227] In certain embodiments, fracture of a crystalline material bonded to a rigid carrier can be promoted by applying a mechanical force proximate to at least one edge of the carrier (e.g., optionally positioned at one or more points.) Such a force can impart a bending moment in at least a portion of the carrier that is transferred to the subsurface laser damaged region to initiate fracture.
[0228] As discussed previously herein, a variety of fracture techniques may be used simultaneously or sequentially. Certain embodiments may utilize CTE mismatch in combination with mechanical force. If there is a significant CTE mismatch between the substrate and the carrier and the temperature is appropriately reduced, less (or zero) mechanical force may be required to facilitate separation. Conversely, if there is a low (or zero) degree of CTE mismatch between the substrate and the carrier, more mechanical force may be required to complete the separation.
[0229] exist FIG. 15A to FIG. 15D and FIG. 16A to FIG. 16B An exemplary embodiment of promoting the fracture of a crystalline material having subsurface damage and bonded to a rigid carrier by applying a mechanical force is shown in FIG.
[0230] FIG. 15A to FIG. 15D 1 is a schematic cross-sectional view showing the steps of fracturing a crystalline material substrate 142 having subsurface laser damage 143 by applying a mechanical force proximate to one edge of a carrier 148 to which the substrate 142 is bonded. Fig.13D and Fig.13FThe same bonded assembly 140 shown in FIG. The bonded assembly includes a crystalline material substrate 142 having a subsurface laser damaged region 143 bonded (according to any of the bonding methods disclosed herein) between rigid carriers 148, 148'. Each rigid carrier 148, 148' includes a laterally protruding lug portion 149, 149' aligned with the flat surface 145 of the substrate 142, thereby providing a locally enlarged border area defining a recess 141 into which a tool 166 can be inserted. Fig.15A The state before the tool 166 is inserted into the recess 141 is shown. Fig. 15B 14. The state after inserting the tool 166 into the recess is shown when the tool 166 is tilted upward, thereby applying a prying force in a direction tending to promote separation between the rigid carriers 148, 148', thereby applying a bending moment M on at least one of the carriers 148. In some embodiments, the substrate 142 includes a material having a hexagonal crystal structure (e.g., 4H-SiC), and the bending moment M is oriented in the vertical direction.
[0231] Hexagonal crystal structure The orientation of the bending moment M is particularly desirable if the substrate 142 comprises an off-axis (ortho) material; it may be less important if the substrate 142 comprises an on-axis material. Fig. 15C The crystalline material substrate 142 is shown after initial fracture along the subsurface laser damaged region 143, whereby an upper portion 142A of the crystalline material remains bonded to an upper carrier 148, and a lower portion 142B of the crystalline material remains bonded to a lower carrier 148', with the upper carrier 148 tilted upward relative to the lower 148'. Fig.15D The state is shown after breaking is complete and tool 166 is removed, resulting in a first bonded assembly 168A (comprising upper carrier 148 of crystalline material and upper portion 142A) separated from a second bonded assembly 168B (comprising lower carrier 148' of crystalline material and lower portion 142B).
[0232] In certain embodiments, mechanical forces may be applied proximate opposing edges of a rigid carrier to which the substrate is bonded to promote fracture of crystalline material having subsurface laser damage bonded to the carrier. Fig.16A1 is a schematic cross-sectional view of an apparatus 170 for fracturing a crystalline material substrate 172 along a subsurface laser damaged region 173 by applying mechanical forces along opposite edges of a rigid carrier 176 (bonded to the substrate 172 with an adhesive material 174) to impart bending moments M1, M2 to portions of the carrier 174. A restraining element 171 (e.g., a vacuum chuck, a lower substrate, or other support) may be disposed below the substrate 172. The carrier 176 has a lateral extent (e.g., diameter, or length and width) greater than the substrate 172, wherein the carrier 176 forms opposing laterally protruding lips 179A, 179A that may be received by lifting members 175A, 175B. A central portion of the carrier 176 is restrained from lifting (e.g., pressed downwardly) by a restraining member 177. When the lifting members 175A, 175B apply a vertical lifting force to the laterally protruding edges 179A, 179B, and the limiting member 177 prevents the central portion of the carrier 176 from moving upward, opposite bending moments M1, M2 are applied to the carrier 176, and the bending moments M1, M2 are transmitted to the substrate 172 through the adhesive material 174 to induce fracture of the substrate 172 along the subsurface laser damaged region 173. Thereafter, the limiting member 177 and the lifting members 175A, 175B can be released, and the fracture can be completed. Fig. 16B A state is shown in which the fracture is complete, resulting in a bonded assembly 178 comprising a rigid carrier 176, bonding material 174, and a crystalline material substrate portion 172A separated from the remainder of the crystalline material 172. The exposed surfaces 173A, 173B of the crystalline material substrate portion 172A and the remainder of the crystalline material 172 may exhibit surface irregularities that may be reduced by conventional surface processing steps (e.g., grinding, CMP, and / or polishing). In certain embodiments, such surface processing steps may be performed on the crystalline material substrate portion 172A while such portion remains bonded to the rigid carrier 176.
[0233] although FIG. 15A to FIG. 15D and 16A to Fig. 16B Examples of specific apparatuses are provided that facilitate mechanical fracturing of a substrate along a subsurface laser damaged region, but it is understood that other apparatuses may be used to implement the methods disclosed herein, as would be appreciated by one of ordinary skill in the art.
[0234] Subsurface laser damage formation before or after carrier bonding
[0235] Although previously described herein, laser subsurface damage is formed in a crystalline material substrate prior to bonding to a rigid carrier, in certain embodiments, a rigid carrier transparent to laser emission of a desired wavelength may be bonded to the crystalline material substrate prior to forming the subsurface laser damage. In such embodiments, the laser emission may be transmitted through the rigid carrier to the interior of the crystalline material substrate. 17A to 17C Different carrier-substrate subsurface laser forming configurations are shown. Fig.17A is a schematic diagram of laser emission 181 being focused through the surface of a bare substrate 182 to form subsurface laser lesions 183 within the substrate 182 , whereby a rigid carrier may be secured to the substrate 182 after the subsurface laser lesions are formed. Fig. 17B is a schematic diagram of laser emission 181 focused through the surface of a substrate 182 forming subsurface laser lesions 183 within the substrate 182 , where the substrate 182 has previously been bonded to a rigid carrier 186 using an adhesive material 184 . Fig. 17C 1 is a schematic diagram of laser emission 181 being focused through a rigid carrier 186 and an adhesive 184 to form subsurface laser lesions 183 within a substrate 182 previously bonded to the rigid carrier 186. In certain embodiments, a surface of the substrate 182 remote from the carrier 186 may include one or more epitaxial layers and / or metallization layers, wherein the substrate 182 embodies an operational device prior to forming the subsurface laser lesions 183. Fig.17D is a schematic diagram of laser emission 181 being focused through a rigid carrier 186 into a substrate 182 (without an intervening adhesive layer) to form subsurface laser lesions 183 within the substrate 182 that was previously bonded (e.g., via anodic bonding or other non-adhesive means) to the rigid carrier 186.
[0236] Device wafer segmentation process
[0237] In certain embodiments, laser and carrier assisted separation methods may be applied to the crystalline material after at least one epitaxial layer (and optionally at least one metal layer) is formed on the crystalline material as part of an operable semiconductor-based device. This device wafer singulation process is particularly advantageous for the ability to increase the yield of crystalline material (and reduce waste) by significantly reducing the need to grind away substrate material after device formation.
[0238] FIG. 18A to FIG. 18O is a cross-sectional schematic diagram illustrating steps of a device wafer splitting process, according to which a thick wafer is broken from a crystalline material, at least one epitaxial layer is grown on the thick wafer, and the thick wafer is broken to form a first bonded assembly and a second bonded assembly, the first bonded assembly and the second bonded assembly each including a carrier and a thin wafer separated from the thick wafer, wherein the first bonded assembly includes at least one epitaxial layer as part of an operable semiconductor-based device.
[0239] Fig.18A A crystalline material substrate 190 is shown having a first surface 191 and a subsurface laser damage 193 disposed at a predetermined depth relative to the first surface. Fig.18B After adding adhesive material 194 over first surface 191 Fig.18A substrate 190. Fig. 18C After the rigid carrier 196 is bonded to the substrate 190 using the adhesive material 194, Fig.18B The items depicted in . Fig.18D FIG. 1 shows a substrate 190 after it has been fractured along a subsurface laser damage 193 (eg, using one or more of the methods described herein). Fig.18D , producing the remainder of substrate 190 separated from the combined assembly including carrier 196, bonding material 194, and a portion of crystalline material (e.g., thick wafer) 192 removed from substrate 190. In certain embodiments, thick wafer 192 may have a thickness in the range of approximately 350 to 750 microns. Exposed surfaces 193A, 193B of thick wafer 192 and the remainder of substrate 190, respectively, may exhibit surface irregularities that may be reduced by surface processing steps such as grinding, CMP, polishing, etc. Fig.18E Thick wafer 192 is shown after debonding and removal from carrier 196, where thick wafer 192 includes a vertical edge profile. Vertical edges of wafers are susceptible to fracture, generating unacceptable edge debris and particles during wafer processing. To reduce the risk of fracture, the wafer edge can be edge ground to produce a non-vertical wafer edge with a chamfered or rounded edge. Fig.18F The thick wafer 192 is shown supported by a turntable 198 proximate to a rotating profile grinding tool 199 having a concave cutting surface 199A (eg, impregnated with diamond particles) configured to impart a rounded edge profile 197 to the thick wafer 192 . Figure 18G The thick wafer 192 is shown after edge grinding (also referred to as edge profiling), wherein the thick wafer includes a rounded edge 197 providing a boundary between the first wafer surface 201 and the second wafer surface 202 .
[0240] Fig.18H 2 shows the thick wafer 201 after depositing one or more epitaxial layers 203 on or over the first surface 201. Figure 18G Due to the inherent high temperature incompatibility of adhesives with epitaxy, there is no Fig.18D The vector shown in . Fig.18I The semiconductor device shown in FIG. 1 is a semiconductor device after forming a conductive (eg, metal) contact 204 over the epitaxial layer 203 to form at least one operable semiconductor device. Fig.18H, wherein the thick wafer 192 still has rounded edges 197. Conventionally, grinding would be performed on the second surface 202 to thin the thick wafer 192 to a suitable thickness for the resulting device (e.g., 100 to 200 microns for a Schottky diode or MOSFET). The method disclosed herein reduces the need for wafer grinding and instead utilizes laser and carrier assisted separation to remove a portion of the thick wafer so that it can be surface finished and used to make another operational semiconductor device.
[0241] The inventors have found that the presence of the rounded edge 197 on the thick wafer 192 inhibits the controlled formation of subsurface laser damage close to the edge 197 because the rounded profile negatively affects laser focus and depth control. To address this issue, the rounded edge 197 of the thick wafer 192 can be removed before further laser processing. Fig.18J Shows Fig.18I The structure is subjected to grinding using an edge grinder 206 to grind away the rounded edge 197 and impart a substantially vertical edge 205 extending between a first surface 201 and a second surface 202 of the thick wafer 192, wherein the epitaxial layer 203 and the contacts 204 are arranged above the first surface 201.
[0242] Figure 18K 1 shows the thick wafer 192 after adding a temporary bonding material 207 over the first surface 201, the epitaxial layer 203 and the contacts 204 in preparation for receiving and adhering the first carrier. Fig.18J structure. Figure 18L FIG. 2 shows a first carrier 208 added to the temporary bonding material 207 and after subsurface laser damage 209 is formed in the thick wafer 192 by the impact of the focused laser emission through the second surface 202 of the thick wafer 192. Figure 18K structure. Figure 18M FIG. 2 shows a second surface 202 of a thick wafer 192 after bonding a rigid second carrier 210 to the second surface 202 of the thick wafer 192 proximate to the subsurface laser damage 209. Figure 18L For separation purposes, the rigid second carrier 210 will act as a front side carrier intended to remove a portion (ie, a layer) of the thick wafer 192.
[0243] Fig.18N FIG. 1 shows a schematic diagram of a thick wafer 192 after applying at least one breaking process as disclosed herein to break the thick wafer 192 along the subsurface laser damage 209 to produce first and second bonded subassemblies 212A, 212B. Figure 18M The first combined subassembly 212A includes a first thin wafer portion 192A (with Figure 18MThe second combined subassembly 212B includes the second thin wafer portion 192B (separated from the thick wafer 192), the epitaxial layer 203, the contact 204, the temporary adhesive material, and the first carrier 208. Figure 18M The exposed surfaces 209A, 209B of the thin wafer portions 192A, 192B may exhibit surface irregularities that are reduced by conventional surface processing steps (eg, grinding, CMP, and / or polishing) due to laser damage and / or fracture. Fig.18O An operable semiconductor device 214 is shown resulting from the first bonded subassembly 212A by removing the temporary adhesive 207 and the first carrier 208. This figure also shows the second thinned wafer portion 192B after removing the second carrier 210 to prepare the second thinned wafer portion 192B for further processing (eg, epitaxial growth).
[0244] Exemplary methods including reusing a carrier wafer
[0245] Fig.19 2 is a flow chart schematically illustrating the steps of a method according to the present disclosure. Starting from the upper left, a laser 216 can focus a laser emission below a first surface 222 of a thick crystalline material substrate 220 (e.g., a SiC ingot) to produce a subsurface laser damaged region 218. If the substrate 220 is a SiC material, the laser emission can be irradiated through the C-terminated face of the SiC substrate 220. Thereafter, a carrier wafer 224 can be bonded to the first surface 222 of the crystalline material substrate 220, wherein the carrier wafer 224 includes a first surface 226 (close to the first surface 222 of the substrate 220) and a second surface 228 opposite to the first surface 226 of the carrier wafer 224. Such bonding between the carrier wafer 224 and the crystalline material substrate 220 can be performed by any method disclosed herein, such as adhesive bonding or anodic bonding. Thereafter, a fracture process as disclosed herein is applied (e.g., cooling the CTE mismatched carrier, applying ultrasonic energy, and / or applying mechanical force) to fracture the crystalline material 220 along the subsurface laser damaged region 218, so that the crystalline material portion 230 bonded to the carrier wafer 224 is separated from the rest of the crystalline material substrate 220A. The newly exposed surface 232A of the rest of the crystalline material substrate 220A with the residual laser damage is ground smooth and clean, and returned to the beginning of the process (at Fig.19 ). In addition, the newly exposed surface 234 of the removed crystalline material 230 is ground smooth while being attached to the carrier 224. Thereafter, the carrier wafer 224 can be separated from the removed portion of the crystalline material 230, and the crystalline material 230 can be subjected to epitaxial growth of one or more layers to form an epitaxial device 230', while the carrier wafer 224 is cleaned and returned to the beginning of the process (at Fig.19 ) to achieve removal of another relatively thin portion of the crystalline material substrate 220.
[0246] Fig. 20 The laser damage 218 of the subsurface Fig.19 Schematic cross-sectional view of a portion of a crystalline material substrate (e.g., SiC ingot) 220, wherein the superimposed dashed line identifies an expected kerf loss material region 240. The expected kerf loss material region 240 includes laser damage 218 and material 234 to be mechanically removed (e.g., by grinding and polishing) from a lower surface 238 (e.g., Si-terminated surface) of a crystalline material portion 230 (e.g., SiC wafer) to separate from the substrate 220, plus material 236 to be mechanically removed (e.g., by grinding and polishing) from an upper surface 232A (e.g., C-terminated) surface of a remaining portion 220A of the substrate 220. The lower surface 238 of the crystalline material portion 230 is opposite its upper surface 222. In certain embodiments, for SiC, the entire kerf loss material region may have a thickness in the range of 80 to 120 microns to provide a substrate upper surface 232A and a wafer lower surface 238 sufficient for further processing.
[0247] Material processing / steps with multiple grinding stations
[0248] In certain embodiments, the crystalline material subjected to laser processing and fracture can be further processed with multiple surface grinding steps to remove subsurface damage and edge grinding to impart a chamfered or rounded edge profile, wherein the order of the grinding steps is selected and / or a protective surface coating is used to reduce the likelihood of imparting additional surface damage and to prepare the crystalline material wafer for chemical mechanical planarization. These steps can be performed, for example, using a material processing device according to an embodiment disclosed herein, wherein an exemplary device includes a laser processing station, a fracture station, a plurality of rough grinding stations arranged in parallel downstream of the fracture station, and at least one fine grinding station arranged downstream of the rough grinding station. When processing a wafer cut by a wire saw, edge grinding is typically performed before surface grinding or polishing to remove wire saw surface damage. However, the inventors have found that edge grinding of a substrate portion (e.g., a wafer) having laser damage combined with fracture damage increases the likelihood of cracking of the substrate portion. While not wishing to be bound by any particular theory regarding the cause of this phenomenon, it is believed that if edge grinding is performed before at least some surface processing (grinding and / or polishing), the exposed cleavage planes produced by surface fractures make the surface susceptible to cracking. To this end, it has been found to be beneficial to perform at least some surface processing (eg, grinding and / or polishing) prior to edge grinding.
[0249] It has been found that the rough grinding step (i.e., removing laser damage and fracture damage along the fractured surfaces of the substrate portion and bulk substrate) often requires significantly longer time to complete than the previous laser processing and fracture steps, and significantly longer time to complete than the subsequent fine grinding step. To this end, multiple rough grinding stations are arranged in parallel to eliminate bottlenecks in the manufacture of multiple wafers from bulk crystal material (e.g., ingots). In certain embodiments, robotic processing machines can be arranged upstream and downstream of the multiple rough grinding stations to control the loading and unloading of substrate portions. In certain embodiments, a carrier bonding station can be arranged between the laser processing station and the de-fracture station, and a carrier removal station can be arranged upstream (directly or indirectly) of the edge grinding station. The carrier can ideally remain bonded to the substrate portion during at least some of the surface grinding steps to reduce the possibility of cracking, particularly for thin substrate portions (e.g., wafers); however, it is preferred to remove the carrier prior to edge grinding (or before coating the wafer with a protective coating prior to edge grinding).
[0250] In some embodiments, the carrier bonding station can use a carrier pre-coated with a temporary bonding medium, align and press the carrier to the substrate surface, and subject the bonding medium to the necessary conditions (e.g., heat and pressure) to achieve bonding between the carrier and the substrate. Alternatively, the carrier bonding station can include a coating station that can be used to coat the carrier or substrate as needed.
[0251] Fig.213 is a schematic diagram of a material processing apparatus 300 according to one embodiment, comprising a laser processing station 302, a carrier bonding station 303, a material breaking station 304, a plurality of coarse grinding stations 308A, 308B arranged in parallel, a fine grinding station 312, a carrier removal station 313, and a CMP station 314. The laser processing station 302 comprises at least one laser and a support for at least one substrate, the support being arranged to receive at least one laser beam for forming subsurface laser damage in a crystalline material (e.g., an ingot). The carrier bonding station 303 is configured to bond the crystalline material (having subsurface laser damage therein) to at least one rigid carrier. The breaking station 304 is arranged to receive one or more assemblies (each comprising a substrate bonded to a rigid carrier) from the carrier bonding station 303, and to break at least one substrate along a subsurface laser damage region to remove a substrate portion (which may be similar to a wafer bonded to a carrier). The first and second rough grinding stations 308A, 308B are arranged in parallel downstream of the breaking station 304, wherein the first machining machine 306 is arranged to deliver the substrate portion (as part of the bonded assembly) received from the breaking station 304 alternately to the first rough grinding station 308A or the second rough grinding station 3048B. Downstream of the first and second rough grinding stations 308A, 308B, a second machining machine 310 is provided to deliver the rough ground substrate portion (as part of the bonded assembly) to the fine grinding station 312. The carrier removal station 313 is arranged downstream of the fine grinding station 312 and is used to separate the ground substrate portion from the carrier. The chemical mechanical planarization (CMP) station 314 is arranged downstream of the carrier removal station 313 to prepare the substrate portion for further processing (such as cleaning and epitaxial growth). The CMP station 314 is used to remove the damage remaining after the fine grinding, which itself removes the damage remaining after the rough grinding. In some embodiments, each rough grinding station 308A, 308B includes at least one grinding wheel having a grinding surface with a grit of less than 5000, and the fine grinding station 312 includes at least one grinding wheel having a grinding surface with a grit of at least 5000. In some embodiments, each rough grinding station 308A, 308B is configured to remove a thickness of 20 microns to 100 microns of crystalline material from a crystalline material portion (e.g., a wafer), and the fine grinding station 312 is configured to remove a thickness of 3 microns to 15 microns of crystalline material. In some embodiments, each rough grinding station 308A, 308B and / or the fine grinding station 312 may include multiple grinding substations, wherein different substations include grinding wheels of different grits.
[0252] according to Fig.21The equipment can be modified to accommodate edge grinding to impart a rounded or chamfered edge profile to a crystalline substrate portion (such as a wafer). Such an edge profile will reduce the risk of wafer edge cracking. When the substrate portion is bonded to a carrier, edge grinding may not be performed; therefore, the carrier removal station may be arranged upstream (directly or indirectly) of the edge grinding station.
[0253] Fig. 22 Show that according to similar Fig.21 The material processing apparatus 320 of one embodiment of the present invention includes an edge grinding station 332. The material processing apparatus 320 includes a laser processing station 322, a carrier bonding station 323, a material breaking station 324, a first robot processing machine 326, a plurality of rough grinding stations 328A and 328B arranged in parallel, a second robot processing machine 328, a carrier removal station 331, an edge grinding station 332, a fine grinding station 334, and a CMP station 336. The exemplary edge grinding station 332 can be arranged to clamp a wafer (e.g., such as a wafer) between an upper clamping portion and a lower clamping portion of a turntable having a concave rotating grinding tool. Fig.18F ). Clamping the wafer in this manner may undesirably cause damage to the wafer surface (e.g., the Si-terminated surface of a SiC wafer). Fig. 22 The edge grinding station 332 is shown arranged upstream of the fine grinding station 334 to allow any surface damage produced by the edge grinding station 332 to be removed in the fine grinding station 334. Although the fine grinding station 334 may remove a small degree of wafer thickness, thereby changing the rounded or beveled edge profile produced by the edge grinding station 332, a sufficient degree of rounded or beveled edge profile will remain to inhibit breakage of the wafer edge.
[0254] according to Fig. 22 The apparatus 320 may be used to perform a method for processing a crystalline material wafer including a first surface having surface damage thereon, the crystalline material wafer wherein the first surface is defined by an edge. The method includes grinding the first surface with at least one first grinding apparatus to remove a first portion of the surface damage; after grinding the first surface with the at least one first grinding apparatus, edge grinding the edge to form a chamfered or rounded edge profile; and after the edge grinding, grinding the first surface with at least one second grinding apparatus to remove a second portion of the surface damage sufficient to make the first surface suitable for further processing by chemical mechanical planarization. In certain embodiments, the first grinding apparatus may be embodied in a rough grinding station 328A, 328B, the edge grinding may be performed by an edge grinding station 332, and the second grinding apparatus may be embodied in a fine grinding station 312. In certain embodiments, a carrier removal step may be performed after grinding the first surface with the at least one first grinding apparatus and before edge grinding the edge to form a chamfered or rounded edge profile.
[0255] In certain embodiments, a protective surface coating may be employed to reduce the likelihood of imparting additional surface damage during edge grinding and to prepare the crystalline material wafer for chemical mechanical planarization. Such a surface coating may include a photoresist or any other suitable coating material, may be applied prior to edge grinding, and may be removed after edge grinding.
[0256] Fig.23 is based on Fig.21 Schematic diagram of a material processing apparatus 340 of a similar embodiment, but with a surface coating station 354 incorporated between the fine grinding station 352 and the edge grinding station 356, and a coating removal station 358 incorporated between the edge grinding station 356 and the CMP station 360. The material processing apparatus 340 also includes a laser processing station 342, a material breaking station 344, a first machining device 346, a plurality of rough grinding stations 348A, 348B arranged in parallel, and a second machining device 348 upstream of the fine grinding station 352. The coating station 354 can be configured to apply a protective coating (e.g., a photoresist) by methods such as spin coating, dip coating, spray coating, etc. The protective coating should have sufficient thickness and robustness to absorb any damage that may be generated by the edge grinding station 365. For SiC wafers, the Si termination surface can be coated with a protective coating because the Si termination surface is typically the surface on which epitaxial growth is performed. The coating removal station 358 can be configured to strip the coating by chemical, thermal and / or mechanical means.
[0257] according to Fig.23 The apparatus 340 may be used to perform a method for processing a crystalline material wafer including a first surface having surface damage thereon, wherein the first surface is defined by an edge. The method includes grinding the first surface with at least one first grinding apparatus (e.g., rough grinding stations 348A, 348B) to remove a first portion of the surface damage; then grinding the first surface with at least one second grinding apparatus (e.g., fine grinding station 352) to remove a second portion of the surface damage, the second portion being sufficient to make the first surface suitable for further processing by chemical mechanical planarization; thereafter, forming a protective coating on the first surface (e.g., using a surface coating station 354); then edge grinding the edge (e.g., using an edge grinding station 356) to form a chamfered or rounded edge profile; and thereafter, removing the protective coating from the first surface (e.g., using a coating removal station). Thereafter, the first surface may be processed by chemical mechanical planarization (e.g., by a CMP station 360) to prepare the first surface (e.g., a Si termination surface of the wafer) for subsequent processing (such as surface cleaning and epitaxial growth).
[0258] In some embodiments, the clamping device can be configured to hold an ingot having an end face that is not perpendicular to its side wall to allow subsurface damage to be formed by laser machining the end face. In some embodiments, the clamping effector can conform to an inclined side wall having a circular cross-section when viewed from above. In some embodiments, the clamping effector can include a joint that allows the clamping effector to conform to the inclined side wall.
[0259] Fig.24A 360 is a schematic side cross-sectional view of a first clamping device 362 for holding an ingot 364 having end faces 366, 368 that are not perpendicular to its side wall 370, according to one embodiment. The upper end face 366 is arranged horizontally to receive a laser beam 376. The lower end face 368 can have a carrier 372 attached to the lower end face 368, wherein a chuck 374 (e.g., a vacuum chuck) holds the carrier 372. A clamping effector 378 having a non-vertical face is provided to clamp the side wall 370 of the ingot 364, wherein the clamping effector 378 is arranged at a non-vertical angle A1, A2 relative to a horizontal actuation rod 380. As shown, the ingot 364 is held (e.g., near its bottom) using the clamping device 362 so that the upper end face 366 and the upper portion of the side wall 370 can be used for processing using the methods disclosed herein.
[0260] Fig. 24B is a schematic side cross-sectional view of a second clamping device 362' for holding an ingot 364' having end faces 366', 368' that are not perpendicular to a side wall 370' thereof, according to one embodiment. The upper end face 366' is horizontally arranged to receive a laser beam 376, while the lower end face 368' may have a carrier 372' attached thereto, wherein the carrier 372' is held by a chuck 374'. A clamping effector 378' having a non-perpendicular face is provided to clamp the side wall 370' of the ingot 364', wherein the clamping effector 378' is arranged at a non-perpendicular angle A1, A2 relative to a horizontal actuation rod 380'. A pivot joint 382' is provided between the actuation rod 380' and the clamping effector 378' to facilitate automatic alignment between the clamping effector 378' and the side wall 370' of the ingot 364'.
[0261] Fig.25 Is a line graph that plots the linear coefficient of thermal expansion of sapphire as a function of temperature, with an overlay of the CTE parallel to the sapphire C-axis and the CTE perpendicular to the sapphire C-axis. Fig.26 is a line graph that plots the linear coefficient of thermal expansion of SiC as a function of temperature, with an overlay of the CTE along the SiC c-axis and the SiC a-axis. Fig.25 and Fig.26 ,sapphire( Fig.25 (center) shows a greater CTE variation between the axes than SiC. It can also be seen that sapphire has a greater CTE than SiC over a wide temperature range.
[0262] Fig. 27 is a bar graph providing a comparison of the linear coefficients of thermal expansion of various crystalline materials and metals, believed to be established at 25°C. As can be seen, SiC has a CTE of about 3, while sapphire has a CTE of about 7 (about 2.3 times greater). Fig. 27 , but it has been independently established that the CTE of PDMS polymer is 3.0 x 10 -4 ℃. This value is Fig. 27 Approximately 7.0x 10 of the sapphire shown -6 ℃ CTE value is two orders of magnitude larger.
[0263] Fig.28 is a graph that plots the values of the elastic modulus (Young's modulus) for various materials divided into the following three groups: (1) metals and alloys; (2) graphite, ceramics, and semiconductors; and (3) polymers. The elastic modulus is a mechanical property that measures the stiffness of a solid material and defines the relationship between stress and strain of a material in the linear elastic regime of uniaxial deformation. Fig.28 As can be seen in Figure 2, metals and semiconductors exhibit elastic modulus values that are at least an order of magnitude greater than those of polymers. Fig.28 The exact values are not shown in , but it has been separately established that the elastic modulus of sapphire is 345 GPa, while nickel has an elastic modulus of 190 GPa. In contrast, the polymer PDMS has an elastic modulus range between 0.57 MPa and 3.7 MPa, where such variation depends linearly on the amount of crosslinker present in the polymer.
[0264] The following examples disclose additional non-limiting embodiments of the present disclosure.
[0265] Implementation Method 1
[0266] A 640 μm thick, 150 mm diameter single crystal SiC substrate was used as the starting material. A 10 μm thick SiC epitaxial layer was grown on the first face of the SiC substrate to provide a 650 μm SiC structure. The laser emission was focused from the SiC surface to a depth of 240 μm to produce multiple substantially parallel subsurface laser damage lines at that depth. A single crystal sapphire carrier was adhered to the opposite second side of the SiC substrate using HT-10.10 thermoplastic adhesive (Brewer Science, Inc., Rolla, Missouri, USA), and a thermal compression process (involving the application of a force of 1800 N and maintaining 180°C) was applied until the adhesive was cured. Thermal fracture was performed by contacting the sapphire carrier with a liquid nitrogen-cooled vacuum chuck maintained at -70°C. Fracture produced a 240 μm thick portion of SiC bonded to the sapphire carrier (forming a bonded assembly), separated from a 410 μm thick portion of SiC. Residual laser damage on the 410 μm thick portion of SiC was removed by grinding and CMP to produce a 350 μm thick SiC wafer ready for epitaxy. Separately, the bonded assembly including the 240 μm thick SiC was also subjected to grinding and CMP, whereby the SiC was reduced to a thickness of 180 μm. After this, the bonded assembly is subjected to carrier removal, including contacting the carrier with a heated vacuum chuck to soften the adhesive while applying lateral forces to the SiC according to a hot slip process. The obtained 180 μm thick SiC wafer with SiC epitaxial layer is suitable for MOSFET manufacturing. The result of the process is the formation of a 350 μm thick SiC wafer ready for epitaxy and a 180 μm thick SiC wafer already having a SiC epitaxial layer thereon from a 640 micron thick SiC substrate used as starting material.
[0267] Implementation Method 2
[0268] A single crystal SiC substrate of 570 μm thickness and 150 mm diameter was used as the starting material. A 2 μm thick SiC epitaxial layer was grown on the first face of the SiC substrate to provide a 572 μm SiC structure. The laser emission was focused from the SiC surface to a depth of 160 μm to produce multiple substantially parallel subsurface laser damage lines at this depth. A single crystal sapphire carrier was adhered to the opposite second face of the SiC substrate using the same adhesive process as in Example 1. Thermal fracture was performed by contacting the sapphire carrier with a vacuum chuck cooled by liquid nitrogen maintained at -70°C. The fracture produced a 160 μm thick portion of SiC bonded to the sapphire carrier (forming a bonded assembly), separated from a 412 μm thick portion of SiC. Residual laser damage on the 412 μm thick portion of SiC was removed by grinding and CMP to produce a 350 μm thick SiC wafer ready for epitaxy. Separately, the bonded assembly including the 160 μm thick SiC was also subjected to grinding and CMP, whereby the SiC was reduced to a thickness of 100 μm. After this, the bonded assembly was subjected to carrier removal, including contacting the carrier with a heated vacuum chuck to soften the adhesive while applying lateral forces to the SiC according to a hot slip process. The obtained 100 μm thick SiC wafer with a SiC epitaxial layer is suitable for RF device manufacturing. The result of the process is the formation of a 350 μm thick SiC wafer ready for epitaxy and a 100 μm thick SiC wafer having a SiC epitaxial layer thereon from a 570 micron thick SiC substrate used as a starting material.
[0269] Implementation 3
[0270] A 150 mm diameter single crystal SiC substrate (ingot) with a thickness greater than 10 mm is used as the starting material for producing SiC wafers of 355 microns in thickness. Laser emission is irradiated through the C-terminated surface of the SiC substrate to form subsurface laser damage. A sapphire carrier is bonded to the upper surface of the SiC substrate using a thermoplastic bonding material disclosed herein, and thermal fracture is performed to separate the upper (wafer) portion of the SiC from the rest of the ingot. The Si-terminated surface of the separated wafer portion and the C-terminated surface of the rest of the ingot are coarsely ground using a 2000 grit grinding wheel (e.g., a metal, glass or resin bonded grinding wheel) to remove all visible laser and fracture damage. After this, the Si end faces of the separated wafer portions and the C end faces of the remainder of the ingot are finely ground (e.g., using a vitreous grinding surface) with 7000 or higher grit (e.g., up to 30,000 grit or higher) to produce smoother surfaces, preferably with an average roughness (Ra) of less than 4 nm, more preferably in the range of 1-2 nm Ra. On the remainder of the ingot, a smooth surface is required to avoid any impact on subsequent laser processing. The wafer is ready for CMP and has sufficient smoothness to minimize the amount of CMP removal required, as CMP is typically a higher cost method. During the fine grinding process, typical material removal can be in the range of 5 to 10 microns in thickness to remove all residual subsurface damage and any remaining laser damage (visible and invisible to the naked eye) from the rough grinding. After this, the remainder of the ingot is returned to the laser for further processing, and the wafer is edge ground and subjected to chemical mechanical planarization (CMP) in preparation for epitaxial growth. Edge grinding can be performed between the rough surface grinding and the fine surface grinding to avoid any risk of scratching the precision ground Si face. Material removal during CMP can be in the range of about 2 microns in thickness. The total material consumed from the substrate (ingot) can be less than 475 microns. Given a final wafer thickness of 355 microns, the kerf loss is less than 120 microns.
[0271] Technical benefits that can be obtained by one or more embodiments of the present disclosure may include: reduced kerf loss of crystal material compared to wire saws; reduced processing time and increased yield of crystal material wafers and resulting devices compared to wire saws; reduced bow of the resulting semiconductor wafer compared to conventional post-laser fracture methods; reduced need for consumable liquid nitrogen compared to conventional post-laser fracture methods; and enhanced ability to obtain thin layers of crystal by removing abrasive material (e.g., grinding), reducing the need for thinning.
[0272] Unless indicated to the contrary herein, any of the various features and elements as disclosed herein may be combined with one or more other disclosed features and elements.
[0273] Those skilled in the art will recognize improvements and modifications to the preferred embodiments of the present disclosure. All such improvements and modifications are considered to be within the scope of the concepts disclosed herein and the following claims.
Claims
1. A semiconductor processing method, comprising: temporarily providing an adhesive material on a semiconductor wafer, the semiconductor wafer comprising a substrate and one or more epitaxial layers on a first surface of the substrate, wherein the substrate has a damaged region at a depth in the substrate, wherein the adhesive material is on the one or more epitaxial layers; A carrier is temporarily bonded to the semiconductor wafer using the bonding material, and the substrate is fractured along or proximate to the damaged region to produce a bonded assembly including the carrier, the bonding material, the one or more epitaxial layers, and a portion of the substrate.
2. The semiconductor processing method according to claim 1, further comprising: The carrier is removed from the binding assembly.
3. The semiconductor processing method according to claim 1, further comprising: The adhesive material is removed from the bonded assembly.
4. The semiconductor processing method according to claim 1, wherein breaking the substrate along or close to the damaged region comprises: temporarily bonding a second carrier to a second surface of the semiconductor wafer, the second surface being opposite to the first surface; as well as The substrate is fractured along or proximate to the damaged region to produce a second bonded assembly including the second carrier and a second portion of the substrate.
5. The semiconductor processing method according to claim 4, wherein the method comprises: removing the second carrier from the second binding assembly; as well as One or more second epitaxial layers are formed on a second portion of the substrate. The semiconductor processing method according to claim 1 , wherein the damaged region is a laser damaged region.
7. The semiconductor processing method of claim 1, wherein before temporarily providing an adhesive material on the semiconductor wafer, the method comprises forming one or more conductive contacts on the one or more epitaxial layers.
8. The semiconductor processing method according to claim 1, wherein the method comprises: The damaged region is induced in the substrate using one or more lasers.
9. The semiconductor processing method according to claim 8, wherein the method comprises: Prior to inducing the damaged region in the substrate with one or more lasers, the rounded edges of the substrate are removed.
10. The semiconductor processing method according to claim 1, wherein the substrate comprises silicon carbide.
11. The semiconductor processing method according to claim 1, wherein the adhesive material comprises a thermoplastic material.
12. The semiconductor processing method according to claim 1, wherein the bonding material has a glass transition temperature Tg greater than 25°C.
13. The semiconductor processing method of claim 1, wherein the bonding material has a Shore D hardness value of at least about 70 when the bonding material is at 25°C.
14. The semiconductor processing method of claim 1, wherein the bonding material has an elastic modulus of at least about 7 MPa when the bonding material is at 25°C.
15. The semiconductor processing method according to claim 1, wherein the carrier has an elastic modulus of at least 20 GPa.
16. The semiconductor processing method of claim 1, wherein the carrier comprises a crystalline material.
17. The semiconductor processing method of claim 16, wherein the crystalline material is a polycrystalline material.
18. The semiconductor processing method according to claim 1, wherein the carrier has a thickness of about 800 μm or more.
19. The semiconductor processing method according to claim 1, wherein: At 25° C., a coefficient of thermal expansion (CTE) of the carrier is greater than a CTE of the substrate.
20. The semiconductor processing method of claim 1, wherein breaking the substrate along or proximate to the damaged region to produce a bonded assembly comprises one or more of the following: applying ultrasonic energy to at least one of the carrier or the substrate; or A mechanical force is applied to the carrier.