A TOPCon battery and a front passivation process method thereof

By introducing hydrogen ions on the front of the silicon wafer, and depositing SiNx or SiOxNy film layers, the problem of insufficient passivation performance of solar cells is solved, the density and uniformity of the passivation layer are improved, and the photoelectric conversion is improved. efficiency.

CN118825133BActive Publication Date: 2024-11-19MIANYANG XINHAO NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411287665.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-19
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

The passivation performance of existing solar cells is insufficient, resulting in low photoelectric conversion efficiency and poor film-forming density and uniformity of existing passivation layers.

Method used

A stable Si-H bond layer was prepared by introducing hydrogen ions (H+) on the front of the silicon wafer. As a basis, SiNx or SiOxNy film layers were deposited in sequence to improve the density and uniformity of the passivation layer.

Benefits of technology

Effectively passivate the surface defects of the silicon wafer, provide a flatter surface, improve the deposition quality and stability of the SiNx or SiOxNy film layer, enhance the passivation effect, and improve the photoelectric conversion efficiency of solar cells.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of photovoltaic technology, and discloses a TOPCon cell and a front passivation process method thereof, comprising the following steps: sequentially plating a Si-H bond layer, a SiN bond layer, and a Si-H bond layer on the front of a silicon wafer. x Thin film layer, SiO x N y The coating process steps of the Si-H bond layer are as follows: at 430-530°C, a special gas is excited by radio frequency discharge to generate plasma and deposited on the front surface of the silicon wafer. The power of the radio frequency discharge is 13000-15000W, the pressure is 900-1100mtorr, and the time is 60-90s; the special gas is: 5000-8000sccm of ammonia and 5000-8000sccm of nitrous oxide. The present invention introduces hydrogen ions (H + ), and then prepare a stable Si-H bond layer, which can effectively reduce the surface recombination center, reduce the surface recombination rate, and improve the photoelectric conversion efficiency of solar cells, paving the way for the subsequent SiN x or SiO x N y The film deposition provides a smoother and cleaner surface, which not only makes SiN x or SiO x N y The film layer is easier to deposit, and its density and uniformity are improved, so it can better bond with the silicon wafer to form a more stable structure, further improving the passivation effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photovoltaic cells, and in particular to a TOPCon cell and a front passivation process method thereof. Background Art

[0002] In the photovoltaic field, improving the efficiency of solar cells has always been a top priority in research and design. In order to improve the efficiency of solar cells, silicon nitride film or silicon oxynitride film is widely used as a passivation layer of solar cells in the manufacturing process of solar cells. Usually, its passivation effect and adjustable refractive index characteristics are used to reduce the surface recombination of solar cells and reduce reflection, thereby increasing the light incidence.

[0003] As the requirements for solar cell efficiency become higher and higher, the requirements for the passivation performance of the passivation layer of solar cells are also getting higher and higher. At present, the front passivation of the battery is usually carried out by first preparing an aluminum oxide layer on the front of the silicon wafer, and then depositing a silicon nitride film layer and a silicon oxynitride film layer in sequence. However, this direct deposition method has poor film density and uniformity, resulting in poor passivation effect.

[0004] Therefore, how to improve the passivation performance of the passivation layer of solar cells is an important issue that needs to be solved urgently in the industry.

[0005] In view of this, this application is hereby filed. Summary of the invention

[0006] The problem of the prior art is that the passivation performance of the existing solar cells is still defective, resulting in low photoelectric conversion efficiency of the solar cells. In order to solve the above problem, the present invention provides a TOPCon cell and a front passivation process method thereof, by introducing hydrogen ions (H + ), and then prepare a stable Si-H bond layer. The Si-H bond layer can effectively passivate the surface defects of the silicon wafer, reduce the surface recombination center and reduce the surface energy of the silicon wafer surface, thus providing a basis for the subsequent SiN x or SiO x N y The film deposition provides a smoother and cleaner surface, which not only makes SiN x or SiO x N y The film layer is easier to deposit, and its density and uniformity are improved, so it can better bond with the silicon wafer to form a more stable structure, further improving the passivation effect.

[0007] The present invention is achieved through the following technical solutions:

[0008] In a first aspect, the present invention provides a front passivation process for a TOPCon cell, comprising the following steps: sequentially plating a Si-H bond layer, a SiN bond layer, and a Si-H bond layer on the front side of a silicon wafer.x Thin film layer, SiO x N y Thin film layer;

[0009] The plating process steps of the Si-H bond layer are as follows: at a temperature of 430~530°C, a special gas is excited by radio frequency discharge to generate plasma deposited on the front surface of the silicon wafer, the power of the radio frequency discharge is 13000~15000W, the pressure is 900~1100mtorr, and the time is 60~90s; the special gas is: ammonia 5000~8000sccm, nitrous oxide 5000~8000sccm.

[0010] The present invention uses a mixture of NH3 and N2O to react under overglow discharge conditions to introduce hydrogen ions (H + ), and then prepare a stable Si-H bond layer. The main ionization and reaction processes are as follows:

[0011] 1. Ammonia molecules dissociate to produce NH2 free radicals and H atoms:

[0012]

[0013] 2. Ammonia molecules are ionized to produce ammonia molecular ions and free electrons:

[0014] ;

[0015] 3. Ammonia molecular ions are further ionized to produce NH2 + and H + :

[0016] ;

[0017] 4. NH2 + Continue to ionize to produce NH + and H + :

[0018] ;

[0019] 5. NH + Finally, ionization is carried out to produce N + and H + :

[0020] ;

[0021] 6. Laughing gas molecules are ionized to produce laughing gas molecular ions and free electrons:

[0022] ;

[0023] 7. Laughing gas molecular ions dissociate to produce N2 and O+ :

[0024] ;

[0025] 8. Generated O + The ions may react with the H atoms produced by the dissociation of ammonia to produce OH + :

[0026] ;

[0027] 9. OH + Further dissociation produces O and H + :

[0028] ;

[0029] The above equations are idealized and do not represent that only the above reactions actually occur and the above intermediates and by-products are produced.

[0030] In a specific embodiment, the SiN x The coating process steps of the thin film layer are as follows: at a temperature of 430~530℃, radio frequency discharge is used to excite special gas 2 to generate plasma deposition on the Si-H bond layer. The power of radio frequency discharge is 13000~18000W, the pressure is 1700~1900mtorr, and the time is 450~550s; special gas 2 is: ammonia 9000~11000sccm, silane 1000~2000sccm.

[0031] In a specific embodiment, the SiO x N y The coating process steps of the thin film layer are as follows: at a temperature of 430~530℃, a special gas is excited by radio frequency discharge to generate plasma and deposit on SiN x On the thin film layer, the power of RF discharge is 13000~15000W, the pressure is 1200~1400mtorr, and the time is 200~300s; special gas three is: ammonia 9000~11000sccm, silane 1100~1500sccm; nitrous oxide 7000~10000sccm.

[0032] In a specific embodiment, in the Si-H bond layer deposition process, the power of the RF discharge is any one of 13000 W, 13200 W, 13400 W, 13600 W, 13800 W, 14000 W, 14200 W, 14400 W, 14600 W, 14800 W and 15000 W, or a range between any two of them.

[0033] In a specific embodiment, in the Si-H bond layer deposition process, the pressure is any one of 900mtorr, 920mtorr, 940mtorr, 960mtorr, 980mtorr, 1000mtorr, 1020mtorr, 1040mtorr, 1060mtorr, 1080mtorr and 1100mtorr, or a range between any two of them.

[0034] In a specific embodiment, in the Si-H bond layer deposition process, the deposition time is 60s, 65s, 70s, 75s, 80s or 85s.

[0035] In a specific embodiment, in the Si-H bond layer deposition process, the special gas one is: ammonia: 5000sccm, 5500sccm, 6000sccm, 6500sccm, 7000sccm, 7500sccm or 8000sccm; nitrous oxide: 5000sccm, 5500sccm, 6000sccm, 6500sccm, 7000sccm, 7500sccm or 8000sccm.

[0036] In a specific embodiment, preferably, in the Si-H bond layer deposition process, the power of the RF discharge is 13000 W, the pressure is 900 mtorr, and the time is 60 s; special gas 1: ammonia: 5000 sccm, nitrous oxide: 5000 sccm.

[0037] In a specific embodiment, SiN xIn the deposition process of the thin film layer, the power of the RF discharge is any one of 13000W, 13500W, 14000W, 14500W, 15000W, 15500W, 16000W, 16500W, 17000W, 17500W and 18000W or a range between any two thereof; the pressure is 1700mtorr, 1720mtorr, 1740mtorr, 1760mtorr, 1780mtorr, 1800mtorr, 1820mtorr, 1840mtorr, 1860mtorr, 1880 Either mtorr and 1900mtorr or the range between any two; the deposition time is 450s, 460s, 470s, 480s, 490s, 500s, 510s, 520s, 530s, 540s or 550s; special gas two is: ammonia: 9000sccm, 9500sccm, 10000sccm, 10500sccm or 11000sccms; silane: 1000sccm, 1200sccm, 1400sccm, 1600sccm, 1800sccm or 2000sccms.

[0038] In a specific embodiment, preferably, SiN x In the deposition process of the thin film layer, the power of the RF discharge is 13000W, the pressure is 1700mtorr, and the time is 450s; special gas 2: ammonia: 9000sccm, silane: 1000sccm.

[0039] In a specific embodiment, SiO x N yIn the deposition process of the thin film layer, the power of the RF discharge is any one of 13000W, 13200W, 13400W, 13600W, 13800W, 14000W, 14200W, 14400W, 14600W, 14800W and 15000W, or a range between any two of them; the pressure is any one of 1200mtorr, 1220mtorr, 1240mtorr, 1260mtorr, 1280mtorr, 1300mtorr, 1320mtorr, 1340mtorr, 1360mtorr, 1380mtorr and 1400mtorr, or a range between any two of them. range; deposition time is 200s, 210s, 220s, 230s, 240s, 250s, 260s, 270s, 280s, 290s or 300s; special gas three is: ammonia: 9000sccm, 9500sccm, 10000sccm, 10500sccm or 11000sccms; silane: 1100sccm, 1200sccm, 1300sccm, 1400sccm or 1500sccm; nitrous oxide: 7000sccm, 7500sccm, 8000sccm, 8500sccm, 9000sccm, 9500sccm or 10000sccms.

[0040] In a specific embodiment, preferably, SiO x N y In the deposition process of the thin film layer, the power of the RF discharge is 13000W, the pressure is 900mtorr, and the time is 200s; special gas three: ammonia: 9000sccm, silane: 1100sccm, nitrous oxide: 7000sccm.

[0041] In a second aspect, the present invention provides a TOPCon battery, which is prepared by the front passivation process of the battery, wherein the front passivation structure of the battery comprises a Si-H bond layer, a SiN bond layer and a Si-H bond layer deposited sequentially on the front surface of the silicon wafer. x Layer and SiO x N y layer.

[0042] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0043] The embodiment of the present invention provides a TOPCon battery and a front passivation process method thereof, by introducing hydrogen ions (H + ), and then prepare a stable Si-H bond layer, which can effectively passivate the surface defects of the silicon wafer, reduce the surface recombination center and reduce the surface energy of the silicon wafer. x or SiOx N y The film deposition provides a smoother and cleaner surface, which not only makes SiN x or SiO x N y The film layer is easier to deposit, and its density and uniformity are improved, so it can better bond with the silicon wafer to form a more stable structure, further improving the passivation effect. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The illustrative embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.

[0045] In the following description, a large number of specific details are set forth in order to provide a thorough understanding of the present invention. However, it is apparent to one of ordinary skill in the art that these specific details need not be employed to practice the present invention. In other embodiments, in order to avoid obscuring the present invention, well-known materials or methods are not specifically described.

[0046] Throughout the specification, references to "one embodiment," "an embodiment," "an example," or "an example" mean that a particular feature, structure, or characteristic described in conjunction with the embodiment or example is included in at least one embodiment of the present invention. Therefore, the phrases "one embodiment," "an embodiment," "an example," or "an example" appearing in various places throughout the specification do not necessarily all refer to the same embodiment or example. In addition, particular features, structures, or characteristics may be combined in one or more embodiments or examples in any suitable combination and / or subcombination. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0047] The "range" disclosed in this application is defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be combined arbitrarily, that is, any lower limit can be combined with any upper limit to form a range. In this application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers.

[0048] In a first aspect, the present invention provides a front passivation process for a TOPCon cell, comprising the following steps: sequentially plating a Si-H bond layer, a SiN bond layer, and a Si-H bond layer on the front side of a silicon wafer. x Thin film layer, SiO x N y Thin film layer;

[0049] The plating process steps of the Si-H bond layer are as follows: at a temperature of 430~530°C, a special gas is excited by radio frequency discharge to generate plasma deposited on the front surface of the silicon wafer, the power of the radio frequency discharge is 13000~15000W, the pressure is 900~1100mtorr, and the time is 60~90s; the special gas is: ammonia 5000~8000sccm, nitrous oxide 5000~8000sccm.

[0050] In a specific embodiment, the SiN x The coating process steps of the thin film layer are as follows: at a temperature of 430~530℃, radio frequency discharge is used to excite special gas 2 to generate plasma deposition on the Si-H bond layer. The power of radio frequency discharge is 13000~18000W, the pressure is 1700~1900mtorr, and the time is 450~550s; special gas 2 is: ammonia 9000~11000sccm, silane 1000~2000sccm.

[0051] In a specific embodiment, the SiO x N y The coating process steps of the thin film layer are as follows: at a temperature of 430~530℃, a special gas is excited by radio frequency discharge to generate plasma and deposit on SiN x On the thin film layer, the power of RF discharge is 13000~15000W, the pressure is 1200~1400mtorr, and the time is 200~300s; special gas three is: ammonia 9000~11000sccm, silane 1100~1500sccm; nitrous oxide 7000~10000sccm.

[0052] In a specific embodiment, in the Si-H bond layer deposition process, the power of the RF discharge is any one of 13000 W, 13200 W, 13400 W, 13600 W, 13800 W, 14000 W, 14200 W, 14400 W, 14600 W, 14800 W and 15000 W, or a range between any two of them.

[0053] In a specific embodiment, in the Si-H bond layer deposition process, the pressure is any one of 900mtorr, 920mtorr, 940mtorr, 960mtorr, 980mtorr, 1000mtorr, 1020mtorr, 1040mtorr, 1060mtorr, 1080mtorr and 1100mtorr, or a range between any two of them.

[0054] In a specific embodiment, in the Si-H bond layer deposition process, the deposition time is 60s, 65s, 70s, 75s, 80s or 85s.

[0055] In a specific embodiment, in the Si-H bond layer deposition process, the special gas one is: ammonia: 5000sccm, 5500sccm, 6000sccm, 6500sccm, 7000sccm, 7500sccm or 8000sccm; nitrous oxide: 5000sccm, 5500sccm, 6000sccm, 6500sccm, 7000sccm, 7500sccm or 8000sccm.

[0056] In a specific embodiment, preferably, in the Si-H bond layer deposition process, the power of the RF discharge is 13000 W, the pressure is 900 mtorr, and the time is 60 s; special gas 1: ammonia: 5000 sccm, nitrous oxide: 5000 sccm.

[0057] In a specific embodiment, further preferably, the ratio of ammonia to nitrous oxide is 1:1.

[0058] In a specific embodiment, SiN x In the deposition process of the thin film layer, the power of the RF discharge is any one of 13000W, 13500W, 14000W, 14500W, 15000W, 15500W, 16000W, 16500W, 17000W, 17500W and 18000W or a range between any two thereof; the pressure is 1700mtorr, 1720mtorr, 1740mtorr, 1760mtorr, 1780mtorr, 1800mtorr, 1820mtorr, 1840mtorr, 1860mtorr, 1880 Either mtorr and 1900mtorr or the range between any two; the deposition time is 450s, 460s, 470s, 480s, 490s, 500s, 510s, 520s, 530s, 540s or 550s; special gas two is: ammonia: 9000sccm, 9500sccm, 10000sccm, 10500sccm or 11000sccms; silane: 1000sccm, 1200sccm, 1400sccm, 1600sccm, 1800sccm or 2000sccms.

[0059] In a specific embodiment, preferably, SiN xIn the deposition process of the thin film layer, the power of the RF discharge is 13000W, the pressure is 1700mtorr, and the time is 450s; special gas 2: ammonia: 9000sccm, silane: 1000sccm.

[0060] In a specific embodiment, SiO x N y In the deposition process of the thin film layer, the power of the RF discharge is any one of 13000W, 13200W, 13400W, 13600W, 13800W, 14000W, 14200W, 14400W, 14600W, 14800W and 15000W, or a range between any two of them; the pressure is any one of 1200mtorr, 1220mtorr, 1240mtorr, 1260mtorr, 1280mtorr, 1300mtorr, 1320mtorr, 1340mtorr, 1360mtorr, 1380mtorr and 1400mtorr, or a range between any two of them. range; deposition time is 200s, 210s, 220s, 230s, 240s, 250s, 260s, 270s, 280s, 290s or 300s; special gas three is: ammonia: 9000sccm, 9500sccm, 10000sccm, 10500sccm or 11000sccms; silane: 1100sccm, 1200sccm, 1300sccm, 1400sccm or 1500sccm; nitrous oxide: 7000sccm, 7500sccm, 8000sccm, 8500sccm, 9000sccm, 9500sccm or 10000sccms.

[0061] In a specific embodiment, preferably, SiO x N y In the deposition process of the thin film layer, the power of the RF discharge is 13000W, the pressure is 900mtorr, and the time is 200s; special gas three: ammonia: 9000sccm, silane: 1100sccm, nitrous oxide: 7000sccm.

[0062] In a second aspect, the present invention provides a TOPCon battery, which is prepared by the front passivation process of the battery, wherein the front passivation structure of the battery comprises a Si-H bond layer, a SiN bond layer and a Si-H bond layer deposited sequentially on the front surface of the silicon wafer. x Layer and SiO x N y layer.

[0063] Example 1

[0064] The embodiment of the present invention provides a front passivation process method of a TOPCon battery, comprising the following steps:

[0065] (1) Place the silicon wafer to be produced into the graphite boat and treat it for 120 seconds;

[0066] (2) Raise the temperature to 450°C within 300 seconds and keep it at this temperature for 400 seconds;

[0067] (3) The first vacuum treatment is performed for 120 seconds, and then the pressure is maintained for leak detection for 60 seconds. The pressure change is less than 60mtorr;

[0068] (4) The second vacuum treatment was performed for 40 seconds, and then SiH4 gas 1480sccm and NH3 gas 6550sccm were introduced; the pressure was kept constant at 900mtorr;

[0069] (5) Radio frequency discharge is used to excite the special gas for re-plating to generate plasma which is deposited on the positive surface of the silicon wafer to form Si-H bond layer, SiN x Thin film layer, SiO x N y Thin film layer,

[0070] The power of the RF discharge for Si-H bond layer deposition is 13000W, the pressure is 900mtorr, and the time is 60s; special gases: ammonia: 5000sccm; nitrous oxide: 5000sccm;

[0071] S N x The power of the RF discharge for thin film deposition is 13000W, the pressure is 1700mtorr, and the time is 450s; special gases: ammonia: 9000sccm; silane: 1000sccm;

[0072] SiO x N y The power of the RF discharge for thin film deposition is 13000W, the pressure is 1200mtorr, and the time is 200s; special gases: ammonia: 9000sccm; silane: 1100sccm; nitrous oxide: 7000sccm;

[0073] (6) The fourth vacuum treatment was performed for 30 seconds, and then the furnace tube was cleaned by nitrogen filling for 50 seconds;

[0074] (7) The fifth vacuum treatment is performed for 30 seconds, and then the vacuum is broken;

[0075] (8) Unloading and processing for 120 seconds.

[0076] Example 2

[0077] The embodiment of the present invention provides a front passivation process method of a TOPCon battery, comprising the following steps:

[0078] (1) Place the silicon wafer to be produced into the graphite boat and treat it for 120 seconds;

[0079] (2) Raise the temperature to 450°C within 300 seconds and keep it at this temperature for 400 seconds;

[0080] (3) The first vacuum treatment is performed for 120 seconds, and then the pressure is maintained for leak detection for 60 seconds. The pressure change is less than 60mtorr;

[0081] (4) The second vacuum treatment was performed for 40 seconds, and then SiH4 gas 1480sccm and NH3 gas 6550sccm were introduced; the pressure was 900mtorr for constant pressure;

[0082] (5) Radio frequency discharge is used to excite the special gas for re-plating to generate plasma which is deposited on the positive surface of the silicon wafer to form Si-H bond layer, SiN x Thin film layer, SiO x N y Thin film layer,

[0083] The power of the RF discharge for Si-H bond layer deposition is 13200W, the pressure is 920mtorr, and the time is 60s; special gases: ammonia: 6500sccm; nitrous oxide: 6500sccm;

[0084] S N x The power of the RF discharge for thin film deposition is 13500W, the pressure is 1720mtorr, and the time is 450s; special gases: ammonia: 9500sccm; silane: 1200sccm;

[0085] SiO x N y The power of the RF discharge for thin film deposition is 13000W, the pressure is 1220mtorr, and the time is 210s; special gases: ammonia: 9500sccm; silane: 1200sccm; nitrous oxide: 7000sccm;

[0086] (6) The fourth vacuum treatment was performed for 30 seconds, and then the furnace tube was cleaned by nitrogen filling for 50 seconds;

[0087] (7) The fifth vacuum treatment is performed for 30 seconds, and then the vacuum is broken;

[0088] (8) Unloading and processing for 120 seconds.

[0089] Example 3

[0090] The embodiment of the present invention provides a front passivation process method of a TOPCon battery, comprising the following steps:

[0091] (1) Place the silicon wafer to be produced into the graphite boat and treat it for 120 seconds;

[0092] (2) Raise the temperature to 450°C within 300 seconds and keep it at this temperature for 400 seconds;

[0093] (3) The first vacuum treatment is performed for 120 seconds, and then the pressure is maintained for leak detection for 60 seconds. The pressure change is less than 60mtorr;

[0094] (4) The second vacuum treatment was performed for 40 seconds, and then SiH4 gas 1480sccm and NH3 gas 6550sccm were introduced; the pressure was 900mtorr for constant pressure;

[0095] (5) Radio frequency discharge is used to excite the special gas for re-plating to generate plasma which is deposited on the positive surface of the silicon wafer to form Si-H bond layer, SiN x Thin film layer, SiO x N y Thin film layer,

[0096] The power of the RF discharge for Si-H bond layer deposition is 15000W, the pressure is 1100mtorr, and the time is 85s; special gases: ammonia: 8000sccm; nitrous oxide: 8000sccm;

[0097] S N x The power of the RF discharge for thin film deposition is 18000W, the pressure is 1900mtorr, and the time is 550s; special gases: ammonia: 11000sccm; silane: 2000sccm;

[0098] SiO x N y The power of the RF discharge for thin film deposition is 15000W, the pressure is 1400mtorr, and the time is 300s; special gases: ammonia: 11000sccm; silane: 1500sccm; nitrous oxide: 10000sccm;

[0099] (6) The fourth vacuum treatment was performed for 30 seconds, and then the furnace tube was cleaned by nitrogen filling for 50 seconds;

[0100] (7) The fifth vacuum treatment is performed for 30 seconds, and then the vacuum is broken;

[0101] (8) Unloading and processing for 120 seconds.

[0102] Comparative Example 1

[0103] This comparative example provides a front passivation process method for a TOPCon battery, comprising the following steps:

[0104] (1) Place the silicon wafer to be produced into the graphite boat and treat it for 120 seconds;

[0105] (2) Raise the temperature to 450°C within 300 seconds and keep it at this temperature for 400 seconds;

[0106] (3) The first vacuum treatment is performed for 120 seconds, and then the pressure is maintained for leak detection for 60 seconds. The pressure change is less than 60mtorr;

[0107] (4) The second vacuum treatment was performed for 40 seconds, and then SiH4 gas 1480sccm and NH3 gas 6550sccm were introduced; the pressure was 900mtorr for constant pressure;

[0108] (5) Use radio frequency discharge to stimulate the special gas for plating to generate plasma, which is deposited on the front surface of the silicon wafer to form SiN x Thin film layer, SiO x N y Thin film layer,

[0109] S N x The power of the RF discharge for thin film deposition is 13000W, the pressure is 1700mtorr, and the time is 450s; special gases: ammonia: 9000sccm; silane: 1000sccm;

[0110] SiO x N y The power of the RF discharge for thin film deposition is 13000W, the pressure is 1200mtorr, the time is 200s, and the special gases are: ammonia: 9000sccm; silane: 1100sccm; nitrous oxide: 7000sccm;

[0111] (6) The fourth vacuum treatment was performed for 30 seconds, and then the furnace tube was cleaned by nitrogen filling for 50 seconds;

[0112] (7) The fifth vacuum treatment is performed for 30 seconds, and then the vacuum is broken;

[0113] (8) Unloading and processing for 120 seconds.

[0114] Comparative Example 2

[0115] This comparative example provides a front passivation process method for a TOPCon battery, comprising the following steps:

[0116] (1) Place the silicon wafer to be produced into the graphite boat and treat it for 120 seconds;

[0117] (2) Raise the temperature to 450°C within 300 seconds and keep it at this temperature for 400 seconds;

[0118] (3) The first vacuum treatment is performed for 120 seconds, and then the pressure is maintained for leak detection for 60 seconds. The pressure change is less than 60mtorr;

[0119] (4) The second vacuum treatment was performed for 40 seconds, and then SiH4 gas 1480sccm and NH3 gas 6550sccm were introduced; the pressure was 900mtorr for constant pressure;

[0120] (5) Radio frequency discharge is used to excite the special gas for re-plating to generate plasma which is deposited on the positive surface of the silicon wafer to form Si-H bond layer, SiN x Thin film layer, SiO x N y Thin film layer,

[0121] The power of the RF discharge for Si-H bond layer deposition is 13000W, the pressure is 900mtorr, and the time is 60s; special gases: ammonia: 7000sccm; nitrous oxide: 3000sccm;

[0122] S N x The power of the RF discharge for thin film deposition is 13000W, the pressure is 1700mtorr, and the time is 450s; special gases: ammonia: 9000sccm; silane: 1000sccm;

[0123] SiO x N y The power of the RF discharge for thin film deposition is 13000W, the pressure is 1200mtorr, and the time is 200s; special gases: ammonia: 9000sccm; silane: 1100sccm; nitrous oxide: 7000sccm;

[0124] (6) The fourth vacuum treatment was performed for 30 seconds, and then the furnace tube was cleaned by nitrogen filling for 50 seconds;

[0125] (7) The fifth vacuum treatment is performed for 30 seconds, and then the vacuum is broken;

[0126] (8) Unloading and processing for 120 seconds.

[0127] Comparative Example 3

[0128] This comparative example provides a front passivation process method for a TOPCon battery, comprising the following steps:

[0129] (1) Place the silicon wafer to be produced into the graphite boat and treat it for 120 seconds;

[0130] (2) Raise the temperature to 450°C within 300 seconds and keep it at this temperature for 400 seconds;

[0131] (3) The first vacuum treatment is performed for 120 seconds, and then the pressure is maintained for leak detection for 60 seconds. The pressure change is less than 60mtorr;

[0132] (4) The second vacuum treatment was performed for 40 seconds, and then SiH4 gas 1480sccm and NH3 gas 6550sccm were introduced; the pressure was 900mtorr for constant pressure;

[0133] (5) Radio frequency discharge is used to excite the special gas for re-plating to generate plasma which is deposited on the positive surface of the silicon wafer to form Si-H bond layer, SiN x Thin film layer, SiO x N y Thin film layer,

[0134] The power of the RF discharge for Si-H bond layer deposition is 13000W, the pressure is 900mtorr, and the time is 60s; special gases: ammonia: 10000sccm; nitrous oxide: 5000sccm;

[0135] S N x The power of the RF discharge for thin film deposition is 13000W, the pressure is 1700mtorr, and the time is 450s; special gases: ammonia: 9000sccm; silane: 1000sccm;

[0136] SiO x N y The power of the RF discharge for thin film deposition is 13000W, the pressure is 1200mtorr, and the time is 200s; special gases: ammonia: 9000sccm; silane: 1100sccm; nitrous oxide: 7000sccm;

[0137] (6) The fourth vacuum treatment was performed for 30 seconds, and then the furnace tube was cleaned by nitrogen filling for 50 seconds;

[0138] (7) The fifth vacuum treatment is performed for 30 seconds, and then the vacuum is broken;

[0139] (8) Unloading and processing for 120 seconds.

[0140] The battery cells prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to relevant performance tests, and the results are shown in Table 1 below.

[0141] Table 1

[0142] type Count (pcs) Conversion efficiency / Eta(%) Open circuit voltage / Uoc(V) Short circuit current / Isc(A) Fill factor / FF(%) Series resistance / Rser(Ω) Shunt resistance / RshuntDfDr(Ω) Dark current / IRev2 (A) Example 1 2360 25.66058 0.728007 14.01828 84.160 0.000958 1939.905648 0.008468 Example 2 17314 25.70148 0.728334 14.03415 84.161 0.000957 1810.578552 0.01832 Example 3 2132 25.64205 0.728156 14.01163 84.122 0.000964 1575.538203 0.010769 Comparative Example 1 17033 25.60391 0.726551 14.01889 84.139 0.000936 1756.767397 0.022833 Comparative Example 2 2134 25.63852 0.726646 14.01953 84.237 0.00094 1888.289997 0.008442 Comparative Example 3 2001 25.44457 0.722791 13.99303 84.205 0.000944 1721.332508 0.014177

[0143] It can be seen from the above table that the battery cells produced by the battery front passivation process provided by Examples 1 to 3 of the present invention have significantly improved related performance compared with the battery produced by the existing process.

[0144] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A front passivation process for a TOPCon battery, characterized in that: The steps include: sequentially plating Si-H bond layer, SiN x Thin film layer, SiO x N y Thin film layer; The plating process steps of the Si-H bond layer are as follows: at a temperature of 430~530°C, a special gas is excited by radio frequency discharge to generate plasma deposited on the front surface of the silicon wafer, the power of the radio frequency discharge is 13000~15000W, the pressure is 900~1100mtorr, and the time is 60~90s; the special gas is: ammonia 5000~8000sccm, nitrous oxide 5000~8000sccm.

2. A front passivation process for a TOPCon battery according to claim 1, characterized in that: The SiN x The coating process steps of the thin film layer are as follows: at a temperature of 430~530℃, radio frequency discharge is used to excite special gas 2 to generate plasma deposition on the Si-H bond layer. The power of radio frequency discharge is 13000~18000W, the pressure is 1700~1900mtorr, and the time is 450~550s; special gas 2 is: ammonia 9000~11000sccm, silane 1000~2000sccm.

3. The front passivation process of a TOPCon battery according to claim 1, characterized in that: The SiO x N y The coating process steps of the thin film layer are as follows: at a temperature of 430~530℃, a special gas is excited by radio frequency discharge to generate plasma and deposit on SiN x On the thin film layer, the RF discharge power is 13000~15000W, the pressure is 1200~1400mtorr, and the time is 200~300s; Special gas three is: ammonia 9000~11000sccm, silane 1100~1500sccm; nitrous oxide 7000~10000sccm.

4. The front passivation process of a TOPCon battery according to claim 1, characterized in that: In the Si-H bond layer deposition process, the power of the RF discharge is any one of 13000 W, 13200 W, 13400 W, 13600 W, 13800 W, 14000 W, 14200 W, 14400 W, 14600 W, 14800 W and 15000 W, or a range between any two of them.

5. The front passivation process of a TOPCon battery according to claim 1, characterized in that: In the Si-H bond layer deposition process, the pressure is any one of 900mtorr, 920mtorr, 940mtorr, 960mtorr, 980mtorr, 1000mtorr, 1020mtorr, 1040mtorr, 1060mtorr, 1080mtorr and 1100mtorr, or a range between any two of them.

6. The front passivation process of a TOPCon battery according to claim 1, characterized in that: In the Si-H bond layer deposition process, the deposition time is 60s, 65s, 70s, 75s, 80s or 85s.

7. The front passivation process of a TOPCon battery according to claim 1, characterized in that: In the Si-H bond layer deposition process, the special gas 1 is: ammonia: 5000sccm, 5500sccm, 6000sccm, 6500sccm, 7000sccm, 7500sccm or 8000sccms; nitrous oxide: 5000sccm, 5500sccm, 6000sccm, 6500sccm, 7000sccm, 7500sccm or 8000sccms.

8. The front passivation process of a TOPCon battery according to claim 2, characterized in that: S N x In the deposition process of the thin film layer, the power of the RF discharge is any one of 13000W, 13500W, 14000W, 14500W, 15000W, 15500W, 16000W, 16500W, 17000W, 17500W and 18000W or a range between any two thereof; the pressure is 1700mtorr, 1720mtorr, 1740mtorr, 1760mtorr, 1780mtorr, 1800mtorr, 1820mtorr, torr, 1840mtorr, 1860mtorr, 1880mtorr and 1900mtorr or any range between any two; deposition time is 450s, 460s, 470s, 480s, 490s, 500s, 510s, 520s, 530s, 540s or 550s; special gas 2 is: ammonia: 9000sccm, 9500sccm, 10000sccm, 10500sccm or 11000sccms; Silane: 1000 sccm, 1200 sccm, 1400 sccm, 1600 sccm, 1800 sccm, or 2000 sccm.

9. The front passivation process of a TOPCon battery according to claim 3, characterized in that: SiO x N y In the deposition process of the thin film layer, the power of the RF discharge is any one of 13000W, 13200W, 13400W, 13600W, 13800W, 14000W, 14200W, 14400W, 14600W, 14800W and 15000W or a range between any two thereof; the pressure is 1200mtorr, 1220mtorr, 1240mtorr, 1260mtorr, 1280mtorr, 1300mtorr, 1320mtorr, torr, 1340mtorr, 1360mtorr, 1380mtorr and 1400mtorr, or any range between any two thereof; the deposition time is 200s, 210s, 220s, 230s, 240s, 250s, 260s, 270s, 280s, 290s or 300s; the special gas three is: ammonia: 9000sccm, 9500sccm, 10000sccm, 10500sccm or 11000sccms; Silane: 1100 sccm, 1200 sccm, 1300 sccm, 1400 sccm or 1500 sccm; nitrous oxide: 7000 sccm, 7500 sccm, 8000 sccm, 8500 sccm, 9000 sccm, 9500 sccm or 10000 sccm.

10. A TOPCon battery, characterized in that: The front passivation structure of the battery is prepared by the process method of any one of claims 1 to 9, wherein the front passivation structure of the battery comprises a Si-H bond layer, a SiN bond layer and a Si-H bond layer deposited sequentially on the front surface of the silicon wafer. x Layer and SiO x N y layer.