Temperature-sensitive material, molded body, and method for producing temperature-sensitive material
By using a compound with a high flash point and a combination of a porous inorganic compound and a thermoplastic resin in the thermochromic material, the problems of insufficient heat resistance and bleeding of thermochromic materials in the existing technology are solved, and non-bleeding at high temperatures is achieved. The resulting molded body has excellent thermochromic properties, brittleness resistance and light weight.
Patent Information
- Application Number
- CN202380025179.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-07
- Filing Date
- 2023-03-01
- Publication Date
- 2024-10-22
AI Technical Summary
Existing thermochromic materials exhibit insufficient heat resistance in high heat-resistant applications, easily bleed out during melting and mixing with thermoplastic resins, and their brittleness resistance and lightweight properties have not been fully studied.
A resin composition is used, including a compound with a flash point of 155°C or above, a porous inorganic compound with an oil absorption of 4.0g/g or above, and a thermoplastic resin. Through specific composition ratios and process conditions, it is ensured that the composition does not Bleed out, and has excellent thermochromic properties, brittleness resistance and lightweight.
A thermochromic material that adapts to process heat resistance at high temperatures and does not bleed out in the molded body was realized, and a molded body with excellent thermochromic properties, brittleness resistance, and lightweight was obtained.
Smart Images

Figure BDA0005024364730000131 
Figure BDA0005024364730000141
Abstract
Description
Technical Field
[0001] The present disclosure relates to a temperature-sensitive material, a formed body, and a method for manufacturing the temperature-sensitive material. Background Art
[0002] The phenomenon of thermochromism, in which the color of a substance changes due to a temperature change, is known, and substances having such a property (thermochromic property), namely, thermochromic materials, are known. Such thermochromic materials are widely used in various fields.
[0003] Patent Document 1 discloses a technique for detecting a temperature change in an environment using a temperature sensor including a resin composition having a thermochromic pigment and a solar cell covered with the composition.
[0004] In addition, Patent Document 2 discloses a technology for determining whether a patch preparation has been attached to an individual using a patch preparation device that is laminated with a temperature change component having a thermochromic pigment and is equipped with a patch preparation and a sensor, wherein the patch preparation is used to be attached to an individual having body temperature, and the sensor detects temperature changes caused by the attachment of the patch preparation to the individual.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent No. 6679377
[0008] Patent Document 2: Japanese Patent No. 6847585 Summary of the invention
[0009] Problems to be solved by the invention
[0010] Thermochromic materials and resin compositions containing the same are required to have high heat resistance depending on the application. However, conventional thermochromic materials represented by the thermochromic pigments described in Patent Documents 1 and 2 do not have sufficient heat resistance and are difficult to use in applications requiring high heat resistance.
[0011] In addition, when using a thermoplastic resin with high heat resistance, the thermochromic material and the thermoplastic resin are sometimes melt-kneaded at a relatively high temperature. Therefore, the thermochromic material is required to have heat resistance that can adapt to the process temperature when melt-kneading with the resin. However, no thermochromic material that satisfies this heat resistance has been known so far.
[0012] Furthermore, the obtained molded body is required to have properties such as no leakage (no seepage) of the thermochromic material from the thermoplastic resin, and also to have brittleness resistance and lightness, etc. However, such studies have not been sufficiently conducted in the prior art.
[0013] The present disclosure provides a resin composition and a molded body including the resin composition, wherein the resin composition contains a thermochromic material having process heat resistance that can be adapted even when melt-kneading is performed at a relatively high temperature and having the property that the material does not leak out (does not seep out) from the resin when the molded body is formed, and can obtain a molded body having thermochromic properties and excellent brittleness resistance and lightness.
[0014] Methods for solving problems
[0015] The above-mentioned problems can be solved, for example, by the following means.
[0016] [1] A temperature-sensitive material comprising:
[0017] 100 parts by mass of a thermoplastic resin (A) satisfying the following requirements (a-1) to (a-3),
[0018] 10 to 100 parts by mass of a compound (B) having a flash point of 155° C. or higher (different from the above-mentioned component (A)), and
[0019] 1.5 to 20 parts by weight of a porous inorganic compound (C) having an oil absorption of 4.0 g / g or more,
[0020] When the content of the porous inorganic compound (C) is 100 parts by mass, the content of the compound (B) is more than 200 parts by mass and less than 700 parts by mass,
[0021] When the total light transmittance at 1600 to 300 nm at a temperature 5°C lower than the phase transition temperature of the compound (B) is T1(%), and the total light transmittance at 1600 to 300 nm at a temperature 5°C higher than the phase transition temperature of the compound (B) is T2(%), and ΔT=T2-T1(%),
[0022] The average ΔT value at 1600-300nm is more than 10%,
[0023] (a-1) Density measured according to the method described in ASTM D 1505 is 0.80 to 1.0 g / cm 3 scope;
[0024] (a-2) a melt flow rate (MFR) measured at 230°C and 10 kg load according to the method described in ISO 1133 in the range of 0.1 to 100 g / 10 min;
[0025] (a-3) The durometer A hardness (instantaneous value) measured according to the method described in ISO 7619 is in the range of 50 to 100.
[0026] [2] The temperature sensitive material according to item [1], wherein the compound (B) is a fatty acid ester.
[0027] [3] The temperature sensitive material according to item [2], wherein the fatty acid ester is an ester compound of a monovalent aliphatic carboxylic acid having 10 to 25 carbon atoms and a monovalent aliphatic alcohol having 10 to 25 carbon atoms.
[0028] [4] The temperature-sensitive material according to item [2] or [3], wherein the fatty acid ester is at least one compound selected from the group consisting of stearyl stearate, myristyl myristate, cetyl myristate and behenyl behenate.
[0029] [5] The temperature-sensitive material according to any one of items [1] to [4], wherein the content of the compound (B) is 20 to 70 parts by mass based on 100 parts by mass of the thermoplastic resin (A).
[0030] [6] The temperature sensitive material according to any one of items [1] to [5], wherein the oil absorption of the porous inorganic compound (C) is 4.5 g / g or more and 10.0 g / g or less.
[0031] [7] The temperature sensitive material according to any one of items [1] to [6], wherein the porous inorganic compound (C) is hydrophobic silica.
[0032] [8] The temperature-sensitive material according to any one of items [1] to [7], wherein the content of the porous inorganic compound (C) is 3 to 16 parts by mass relative to 100 parts by mass of the thermoplastic resin (A).
[0033] [9] A formed body comprising the temperature sensitive material according to any one of items [1] to [8].
[0034]
[10] A method for producing a temperature-sensitive material, which is the method for producing a temperature-sensitive material according to any one of items [1] to [8], comprising the step of kneading a thermoplastic resin (A), a compound (B) and a porous inorganic compound (C) at a temperature of 150° C. or higher.
[0035] Effects of the Invention
[0036] According to the present disclosure, a resin composition and a molded body including the resin composition can be provided, wherein the resin composition contains a thermochromic material having process heat resistance that can be adapted even when melt-kneading is performed at a relatively high temperature and having the property that the material will not leak out (bleed out) from the resin when the molded body is formed, and a molded body having thermochromic properties and excellent brittleness resistance and lightness can be obtained. DETAILED DESCRIPTION
[0037] Hereinafter, the present disclosure will be described in detail.
[0038] In the present disclosure, unless otherwise specified, the description "XX or more and YY or less" and "XX to YY" indicating a numerical range means a numerical range including the lower limit and the upper limit as endpoints.
[0039] Moreover, when describing a numerical range in stages, the upper limit and the lower limit of each numerical range can be arbitrarily combined.
[0040] Furthermore, the description of "A and / or B" is a concept that includes the case of A, the case of B, and the case of both A and B.
[0041] <Thermoplastic resin (A)>
[0042] The thermoplastic resin (A) used in the present disclosure satisfies the following requirements (a-1) to (a-3).
[0043] (a-1) Density measured according to the method described in ASTM D 1505 is 0.80 to 1.0 g / cm 3 range.
[0044] (a-2) The melt flow rate (MFR) measured at 230°C and 10 kg load in accordance with the method described in ISO 1133 is in the range of 0.1 to 100 g / 10 min.
[0045] (a-3) The durometer A hardness (instantaneous value) measured according to the method described in ISO 7619 is in the range of 50 to 100.
[0046] The density in requirement (a-1) is preferably 0.81 to 0.97 g / cm 3 , more preferably 0.82 to 0.94 g / cm 3 When the density of the thermoplastic resin (A) is within the above range, a molded product having excellent lightness can be obtained.
[0047] The MFR in the requirement (a-2) is preferably 0.5 to 80 g / 10 min, more preferably 1 to 50 g / 10 min. When the MFR of the thermoplastic resin (A) is within the above range, the obtained resin composition has excellent moldability.
[0048] The durometer A hardness (instantaneous value) in requirement (a-3) is preferably 50 to 90, more preferably 50 to 85, and even more preferably 50 to 80. When the durometer A hardness (instantaneous value) of the thermoplastic resin (A) is within the above range, the thermochromic material is unlikely to bleed out of the thermoplastic resin.
[0049] As the thermoplastic resin (A) as described above, there is no particular limitation as long as it is a thermoplastic resin that satisfies the above requirements (a-1) to (a-3), and examples thereof include olefin resins, styrene resins, acrylic resins, polyester resins, polyvinyl chloride resins, polyamide resins, polycarbonate resins, polylactic acid resins, polyimide resins, polysulfone resins, aromatic polyketone resins, etc. These resins may be used alone or in combination of two or more, and commercial products may also be used. Among the above, olefin resins are preferred, and olefin thermoplastic elastomers are more preferred.
[0050] Preferred examples of olefin-based thermoplastic elastomers include dynamically crosslinked products of an ethylene-α-olefin-non-conjugated polyene copolymer [I] having 3 to 20 carbon atoms (hereinafter also referred to as “ethylene-α-olefin-non-conjugated polyene copolymer [I]”) and a polyolefin resin [II].
[0051] The above-mentioned dynamically crosslinked product may be a product obtained by dynamically crosslinking one type of ethylene-α-olefin-non-conjugated polyene copolymer [I] and one type of polyolefin resin [II], or a product obtained by dynamically crosslinking multiple types of ethylene-α-olefin-non-conjugated polyene copolymers [I] and multiple types of polyolefin resins [II].
[0052] In the present specification, dynamic crosslinking means that the ethylene-α-olefin-non-conjugated polyene copolymer [I] and the polyolefin resin [II] are kneaded in a molten state to cause a crosslinking reaction of at least a part of the carbon-carbon double bonds of the ethylene-α-olefin-non-conjugated polyene copolymer [I].
[0053] ·Ethylene-α-olefin-non-conjugated polyene copolymer[I]
[0054] The ethylene-α-olefin-non-conjugated polyene copolymer [I] comprises a structural unit (a) derived from ethylene, a structural unit (b) derived from an α-olefin having 3 to 20 carbon atoms, and a structural unit (c) derived from a non-conjugated polyene.
[0055] The molar ratio (a) / (b) of the structural unit (a) to the structural unit (b) in the ethylene-α-olefin-non-conjugated polyene copolymer [I] is preferably 50 / 50 to 95 / 5, more preferably 60 / 40 to 80 / 20, and even more preferably 65 / 35 to 75 / 25.
[0056] On the other hand, the specific amount of the structural unit (c) derived from the non-conjugated polyene in the ethylene-α-olefin-non-conjugated polyene copolymer [I] is preferably 2 to 20% by mass based on the total amount of the ethylene-α-olefin-non-conjugated polyene copolymer [I].
[0057] Specific examples of the α-olefin having 3 to 20 carbon atoms constituting the ethylene-α-olefin-nonconjugated polyene copolymer [I] include propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-nonadecene, 1-eicosene, 9-methyl-1-decene, 11-methyl-1-dodecene, 12-ethyl-1-tetradecene, and the like.
[0058] Among them, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene are included. The ethylene-α-olefin-non-conjugated polyene copolymer [I] may contain only one type of structural unit (b) derived from α-olefin, or may contain two or more types.
[0059] In addition, the non-conjugated polyene constituting the ethylene-α-olefin-non-conjugated polyene copolymer [I] may be a compound having no conjugated structure and having two or more carbon-carbon double bonds. Specific examples thereof include: chain non-conjugated dienes such as 1,4-hexadiene, 3-methyl-1,4-hexadiene, 4-methyl-1,4-hexadiene, 5-methyl-1,4-hexadiene, 4,5-dimethyl-1,4-hexadiene, 7-methyl-1,6-octadiene, 8-methyl-4-ethylidene-1,7-nonadiene, 4-ethylidene-1,7-undecadiene; methyltetrahydroindene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene Cyclic non-conjugated dienes such as cyclopentadiene, 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, 2-propenyl-2,2-norbornene, and 4-ethylidene-8-methyl-1,7-nonadiene; and trienes such as 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, 2-propenyl-2,2-norbornene, and 4-ethylidene-8-methyl-1,7-nonadiene.
[0060] Among these non-conjugated polyenes, 5-ethylidene-2-norbornene (ENB) and 5-vinyl-2-norbornene (VNB) are particularly preferred. The ethylene-α-olefin-non-conjugated polyene copolymer [I] may contain only one type of structural unit (c) derived from a non-conjugated polyene, or may contain two or more types.
[0061] It should be noted that the ethylene-α-olefin-non-conjugated polyene copolymer [I] may be a so-called oil-extended rubber that is blended with a softener, preferably a mineral oil-based softener, during its production. The mineral oil-based softener may be a conventionally known mineral oil-based softener, examples of which include paraffin-based process oils, etc.
[0062] The above-mentioned ethylene-α-olefin-non-conjugated polyene copolymer [I] can be produced by a conventionally known method.
[0063] ·Polyolefin resin[II]
[0064] The polyolefin resin [II] may be a polyolefin resin having substantially no unsaturated bonds in the main chain. Specific examples thereof include homopolymers of α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene; and copolymers thereof. It should be noted that, when the polyolefin resin [II] is a copolymer, the content of any one α-olefin is preferably 90 mol% or more.
[0065] In addition, the polyolefin resin [II] is particularly preferably a propylene-based polymer (II-1) containing propylene as the main component, or an ethylene-based polymer (II-2) containing ethylene as the main component.
[0066] Examples of propylene polymers (II-1) include: homopolymers of propylene; random copolymers of propylene and α-olefins having 2 to 10 carbon atoms (e.g., ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, etc.); block copolymers of homopolymers of propylene and amorphous or low-crystalline propylene-ethylene random copolymers, etc. Among them, the amount of structural units other than propylene is preferably 10 mol% or less relative to the total amount of structural units.
[0067] The propylene-based polymer (II-1) may be a product obtained by polymerization by a known polymerization method, and may be a manufactured product or a sold product as a polypropylene resin.
[0068] Furthermore, the propylene-based polymer (II-1) preferably has an isotactic stereostructure, but may have a syndiotactic structure or a mixture of these structures, or may contain a portion of an atactic structure.
[0069] On the other hand, examples of ethylene polymers (II-2) include: homopolymers of ethylene; random copolymers of ethylene and α-olefins having 3 to 10 carbon atoms (e.g., propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, etc.). In the ethylene polymer (II-2), the amount of structural units other than ethylene is preferably 10 mol% or less relative to the total amount of structural units.
[0070] The ethylene polymer (II-2) may be a product obtained by a known polymerization method, and may be a manufactured or sold product as a high pressure low density polyethylene, a linear low density polyethylene, a high density polyethylene, or the like.
[0071] · Method for preparing dynamic crosslinker
[0072] The above-mentioned dynamic crosslinked body can be prepared by adding known crosslinking agent, crosslinking aid and softening agent as required in the above-mentioned ethylene-α-olefin-non-conjugated polyene copolymer [I] and the polyolefin resin [II] and mixing (dynamic crosslinking) to modulate. In addition, commercially available products can also be used. When carrying out dynamic crosslinking, any one of non-open type device, open type device can be used, preferably non-open type device is used.
[0073] Dynamic crosslinking is preferably carried out in an inert gas atmosphere such as nitrogen or carbon dioxide. The temperature during dynamic crosslinking is generally in the range of the melting point of the polyolefin resin [II] to 300°C, preferably 150 to 270°C, more preferably 170 to 250°C. The kneading time is preferably 1 to 20 minutes, more preferably 1 to 10 minutes. In addition, the shear rate at this time is preferably 10 to 50,000 sec. -1 , more preferably 100 to 20,000 seconds -1 .
[0074] Examples of kneading devices used for dynamic crosslinking include mixing rolls, intensive mixers (eg, Banbury mixers, kneaders), single-screw or twin-screw extruders, etc., preferably a non-open type device, and particularly preferably a twin-screw extruder.
[0075] <Compound (B)>
[0076] The compound (B) used in the present disclosure is a compound used as a thermochromic material and having a flash point of 155°C or higher, preferably 156°C or higher and 300°C or lower, more preferably 157°C or higher and 290°C or lower, and further preferably 158°C or higher and 280°C or lower (however, it is a compound other than the above-mentioned component (A)). When the flash point is within the above range, the compound (B) can be included in the resin composition without thermal decomposition even when melt-kneaded with the component (A) or the like at a high temperature of 150°C or higher, and can exhibit excellent thermochromic properties.
[0077] The phase transition temperature of the compound (B) is preferably 30 to 100° C., more preferably 25 to 75° C. When the phase transition temperature is within the above range, the compound (B) can be included in the resin composition without thermal decomposition even when melt-kneaded with the component (A) or the like at a high temperature of 150° C. or higher, and can exhibit excellent thermochromic properties.
[0078] As the compound (B) as described above, for example, there can be listed: compounds having a cyclic, non-repeated and small chain structure; compounds having a structure containing hydrocarbons; compounds having a structure containing hydrogen bonding units such as carbonyl and hydroxyl groups, etc. More specifically, there can be listed fatty acid esters, aliphatic alcohols, fatty acids, etc. Among them, fatty acid esters are preferred, and fatty acid esters having chain substituents at both ends of the ester are more preferred.
[0079] The fatty acid ester is preferably an ester compound of a monovalent aliphatic carboxylic acid having 10 to 25 carbon atoms and a monovalent aliphatic alcohol having 10 to 25 carbon atoms. The aliphatic alcohol more preferably has 20 to 25 carbon atoms. The fatty acid more preferably has 20 to 25 carbon atoms.
[0080] As a specific example of fatty acid ester, for example, isocetyl myristate, octyl dodecyl myristate, isocetyl isostearate, 2-ethylhexanoic acid cetyl, methyl stearate, isocetyl stearate, 2-ethylhexyl palmitate, isotridecyl stearate, butyl stearate, dodecyl stearate, myristyl myristate, cetyl myristate, methyl palmitate, hexadecyl palmitate, stearyl stearate, behenyl behenate, etc. are listed. Among them, stearyl stearate, myristyl myristate, cetyl myristate, behenyl behenate are preferred. If compound (B) is these fatty acid esters, the refractive index is suitable and good thermochromicity can be exerted.
[0081] The compound (B) may be used by appropriately selecting the compound according to the desired thermochromic property, or may be used alone or in combination of two or more.
[0082] <Porous Inorganic Compound (C)>
[0083] The porous inorganic compound (C) used in the present disclosure has an oil absorption of 4.0 g / g or more, preferably 4.5 g / g or more and 10.0 g / g or less, more preferably 5.0 g / g or more and 9.5 g / g or less, and further preferably 5.0 g / g or more and 9.0 g / g or less. When the porous inorganic compound (C) has an oil absorption within the above range, more compound (B) can be retained, and thus the leakage of compound (B) from the resin when a molded body is produced can be suppressed.
[0084] The average particle size of the porous inorganic compound (C) is preferably 1 μm or more and 100 μm or less. The above effect is further improved by the average particle size of the porous inorganic compound (C) being within the above range. It should be noted that the above average particle size is a value measured by an apparatus and analytical method suitable for particle size, for example, a value measured by a laser diffraction / scattering method.
[0085] The porous inorganic compound (C) is not particularly limited as long as it has the above-mentioned oil absorption amount. From the viewpoint of having excellent heat resistance, for example, silicon dioxide, aluminum oxide, and carbon can be cited. One of these can be used alone, or two or more can be used. Among the above, silicon dioxide is preferred, and hydrophobic silicon dioxide is more preferred from the viewpoint of further improving the oil absorption effect, refractive index, and thermochromicity.
[0086] In addition, the porous inorganic compound (C) is preferably a substance that is less volatile and less ignitable than when the compound (B) is kept at a temperature above the melting point (melting peak temperature) of the compound (B) or when the compound (B) is a single component. Examples of such a preferred porous inorganic compound (C) include "AEROS" manufactured by THILIUM and "AIRLICA" manufactured by Tokuyama Corporation.
[0087] <Composition>
[0088] The content of each component in the resin composition of the present disclosure is as follows relative to 100 parts by mass of the thermoplastic resin (A):
[0089] The content of the compound (B) is 10 to 100 parts by mass, preferably 20 to 70 parts by mass, and more preferably 30 to 50 parts by mass.
[0090] The content of the porous inorganic compound (C) is 1.5 to 20 parts by mass, preferably 3 to 16 parts by mass, and more preferably 7 parts by mass or more and less than 14 parts by mass.
[0091] When the content of the porous inorganic compound (C) is 100 parts by mass, the content of the compound (B) is more than 200 parts by mass and less than 700 parts by mass, preferably 250 to 670 parts by mass, and more preferably 300 to 650 parts by mass.
[0092] When the contents of the components satisfy the above conditions, the compound (B) does not leak out (bleed out) from the resin when the molded article is formed, sufficient thermochromic properties can be obtained, and a molded article excellent in brittleness resistance and lightness can be obtained.
[0093] <Optional Ingredients>
[0094] The resin composition of the present invention may contain, in addition to the above-mentioned components (A) to (C), lubricants, nucleating agents, fillers, antioxidants, weather stabilizers, colorants (including thermochromic materials other than compound (B)), foaming agents, pigments, dyes, antistatic agents, flame retardants and other additives as arbitrary components within the scope of not impairing the effects of the present invention.
[0095] <Optical Characteristics>
[0096] For the resin composition of the present disclosure, when the total light transmittance at 1600 to 300 nm at a temperature 5°C lower than the phase transition temperature of the above-mentioned compound (B) is set to T1 (%), the total light transmittance at 1600 to 300 nm at a temperature 5°C higher than the phase transition temperature of the above-mentioned compound (B) is set to T2 (%), and ΔT=T2-T1 (%),
[0097] The average value of ΔT at 1600 to 300 nm is 10% or more, preferably 20 to 60%, and more preferably 25 to 50%. If this requirement is satisfied, desired thermochromic properties can be obtained.
[0098] <Method for producing resin composition>
[0099] The method for producing a resin composition disclosed herein comprises a step of kneading a thermoplastic resin (A), a compound (B), a porous inorganic compound (C), and optional components as required at a temperature of 150° C. or higher, preferably 152° C. or higher and 300° C. or lower, and more preferably 154° C. or higher and 260° C. or lower. The kneading time is usually 1 to 20 minutes, preferably 1 to 10 minutes.
[0100] As the kneading device, a mixing roll, an intensive mixer (for example, a Banbury mixer, a kneader), a single-screw or twin-screw extruder, etc. can be used, and a non-open type device is preferred.
[0101] [molded body]
[0102] The molded body of the present invention comprises the resin composition of the present invention. As the molding method, various known methods can be adopted. Specifically, extrusion molding, compression molding, injection molding, calendering molding, hollow molding, etc. can be cited. In addition, the molded body such as the sheet obtained by the above-mentioned molding method can also be subjected to secondary processing by thermoforming, or it can be laminated with other materials to form a molded body.
[0103] The use of the molded article disclosed in the present invention is not particularly limited, and is suitable for various known uses, such as automotive parts, civil engineering / construction materials, electrical / electronic parts, daily necessities, sanitary products, films / sheets, foams, etc. In particular, the molded article can be used to arbitrarily block or transmit ultraviolet rays or near infrared rays by utilizing thermochromic properties, and is therefore useful when used as a sensor material.
[0104] Example
[0105] The present disclosure will be described in more detail below based on examples, but the present disclosure is not limited to these examples.
[0106] [Material]
[0107] The components of the resin compositions prepared in the examples and comparative examples are as follows. It should be noted that the thermoplastic resins (A), compounds (B) and porous inorganic compounds (C) that do not belong to the thermoplastic resins (A), compounds (B) and porous inorganic compounds (C) in the present disclosure are distinguished by being marked with symbols (A'), (B') and (C'), respectively.
[0108] <Thermoplastic Resin (A) or (A')>
[0109] A-1: MILASTOMER 6010NST manufactured by Mitsui Chemicals, Inc. (a cross-linked thermoplastic elastomer with olefin rubber (EPT) and olefin resin (PP) as main components, density: 0.88 g / cm 3 、MFR (230℃, 10kg load): 12g / 10min、Durometer A hardness (instantaneous value): 70)
[0110] A-2: Mitsui Chemicals, Inc. "TAFMER PN3560" (polyolefin-based thermoplastic elastomer, density: 0.87 g / cm 3 、MFR (230℃, 10kg load): 28g / 10min、Durometer A hardness (instantaneous value): 72)
[0111] A'-3: "DYNARON 8600P" manufactured by JSR Corporation (styrene-ethylene butylene-styrene block polymer, density: 0.90 g / cm 3 、MFR (230℃, 10kg load): 140g / 10min、Durometer A hardness (instantaneous value): 48)
[0112] ·A'-4: Polyvinyl chloride (density: 1.2g / cm 3 , Durometer A hardness (instantaneous value): 70)
[0113] <Compound (B) or (B') (Thermochromic Material)>
[0114] · B-1: "EXCEPARL SS" manufactured by Kao Corporation (stearyl stearate, flash point: 258°C, phase transition temperature: 54°C)
[0115] · B-2: "EXCEPARL MY-M" manufactured by Kao Corporation (myristyl myristate, flash point: 239°C, phase transition temperature: 40°C)
[0116] · B-3: NOF Corporation "SPERMACETI" (cetyl myristic acid, flash point: 228°C, phase transition temperature: 47°C)
[0117] · B-4: UNISTAR M-2222SL manufactured by NOF Corporation (behenyl behenate, flash point: 270°C, phase transition temperature: 68°C)
[0118] · B'-5: "Octadecane" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (flash point: 154°C, phase transition temperature: 28°C)
[0119] · B'-6: Miki Riken Industry Co., Ltd. melamine capsule "PMCD-28SP" (flash point: 160°C, phase transition temperature: 28°C)
[0120] <Porous Inorganic Material (C) or (C')>
[0121] C-1: Hydrophobic silica ("AEROS" manufactured by THILIUM, oil absorption: 7 g / g)
[0122] · C'-2: Activated carbide ("SUMILAY" manufactured by Taniguchi Shokai Co., Ltd., oil absorption: 3.4 g / g)
[0123] [Examples 1 to 7 and Comparative Examples 1 to 14]
[0124] Thermoplastic resin (A) or (A'), compound (B) or (B') (thermochromic material) and porous inorganic material (C) or (C') in the amounts (parts by mass) shown in Tables 1 to 2 were kneaded for 5 minutes at a temperature of 240°C and a torque speed of 30 rpm using Labo Plastomill ("80C100" manufactured by Toyo Seiki Seisaku-sho, Ltd.). After kneading, the kneaded material was quickly recovered. The obtained kneaded material was finely cut with scissors to a size of about 0.5 cm × 0.5 cm × 0.5 cm.
[0125] Place a Teflon (registered trademark) sheet and a mold on a stainless steel plate (hereinafter also referred to as a "SUS plate") in sequence, and cover the holes of the mold with the cut material obtained above. After covering the cut material, stack the Teflon (registered trademark) sheet and the SUS plate in sequence. It should be noted that the Teflon (registered trademark) sheet is used to prevent the mixed material from adhering to the SUS plate due to hot pressing. The length of the above-mentioned mold is 6.5 cm, the width is 6.5 cm, and three thicknesses (1 mm, 2 mm and 5 mm) are used.
[0126] The obtained laminate was hot-pressed at a temperature of 240°C and a pressure of 10 MPa for 5 minutes using a compression molding machine ("ASF-10" manufactured by Shinto Metal Industries, Ltd.). Then, it was quickly moved to a compression molding machine ("NSF-37" manufactured by Shinto Metal Industries, Ltd.) while being clamped by SUS plates, and cooled at a pressure of 10 MPa for 5 minutes. After cooling, the SUS plates and Teflon (registered trademark) sheets were removed from the mold to obtain hot-pressed sheet samples of the thickness described in Tables 1 to 2. The prepared hot-pressed sheet samples were evaluated as follows.
[0127] <Oozing>
[0128] The hot-pressed sheet sample obtained above was clamped on the top and bottom with a 6.5 cm × 6.5 cm surface parallel to the dust-free paper using dust-free paper, and after further clamping it on the top and bottom using SUS plates, it was hot-pressed for 5 minutes using a compression molding machine ("ASF-10" manufactured by Shinto Metal Industries, Ltd.) at a temperature of 100°C and a pressure of 10 MPa. After hot pressing, the hot-pressed sheet sample was quickly peeled off from the dust-free paper. The state of the dust-free paper was confirmed, and the area where the sheet was placed was evaluated as "0: no leakage" if there was no trace, and as "×: leakage" if there was a trace.
[0129] <Brittleness resistance>
[0130] The hot pressed sheet sample obtained above was cut into a size of 1.0 cm in length and 6.5 cm in width to prepare a test piece for tensile test. The tensile elongation of the test piece was measured using a Tensilon universal testing machine (model: RTG-1225) at a tensile speed of 300 mm / min and a distance between chucks of 50 mm. For the value of tensile elongation when the test piece breaks, elongation (%) = elongation value (mm) / distance between chucks (mm), and evaluation was performed based on the measured elongation according to the following criteria.
[0131] ○: more than 10%
[0132] △: 5-10%
[0133] ×: less than 5%
[0134] <Lightweight>
[0135] The weight of the hot pressed sheet sample obtained above was measured with a precision balance, and the value obtained by dividing it by the volume of the hot pressed sheet obtained was defined as density. Based on the obtained density value, evaluation was performed according to the following criteria.
[0136] ○: less than 0.9g / cm 3
[0137] △: 0.9g / cm 3 Above and less than 1g / cm 3
[0138] ×: 1g / cm 3 above
[0139] <Transmittance>
[0140] The transmission spectrum of the heat-pressed sheet sample obtained above was measured using an ultraviolet-visible-near-infrared spectrophotometer "UH4150" (manufactured by Hitachi High-Technologies Corporation).
[0141] When the transmittance at 1600 to 300 nm at a temperature 5°C lower than the phase transition temperature of compound (B) or (B') is set as T1(%), and the transmittance at 1600 to 300 nm at a temperature 5°C higher than the phase transition temperature of compound (B) or (B') is set as T2(%), ΔT=T2-T1(%) is set and evaluation is performed according to the following criteria.
[0142] ○: The average ΔT value at 1600 to 300 nm is 20% or more
[0143] △: The average value of ΔT at 1600 to 300 nm is 10% or more and less than 20% ×: The average value of ΔT at 1600 to 300 nm is less than 10%
[0144] <Overall Evaluation>
[0145] In the above evaluation, a comprehensive evaluation with at least one × was recorded as × (not suitable).
[0146] [Table 1]
[0147]
[0148] [Table 2]
[0149]
[0150] In Comparative Examples 13 and 14, smoke was generated from the compound (B) when preparing the hot-pressed sheet samples, and the hot-pressed sheet samples could not be prepared and evaluated, so the comprehensive evaluation was also recorded as "×".
Claims
1. A temperature-sensitive material, comprising: 100 parts by mass of a thermoplastic resin (A) satisfying the following requirements (a-1) to (a-3), 10 to 100 parts by weight of a compound (B) having a flash point of 155° C. or higher and different from the component (A), and 1.5 to 20 parts by weight of a porous inorganic compound (C) having an oil absorption of 4.0 g / g or higher, When the content of the porous inorganic compound (C) is 100 parts by mass, the content of the compound (B) is more than 200 parts by mass and less than 700 parts by mass, When the total light transmittance at 1600 to 300 nm at a temperature 5°C lower than the phase transition temperature of the compound (B) is T1(%), the total light transmittance at 1600 to 300 nm at a temperature 5°C higher than the phase transition temperature of the compound (B) is T2(%), and ΔT=T2-T1(%), The average ΔT value at 1600-300nm is more than 10%, (a-1) Density measured according to the method described in ASTM D 1505 is 0.80 to 1.0 g / cm 3 scope; (a-2) a melt flow rate (MFR) measured at 230°C and 10 kg load according to the method described in ISO 1133 in the range of 0.1 to 100 g / 10 min; (a-3) The instantaneous value of the durometer A hardness measured according to the method described in ISO 7619 is in the range of 50 to 100. 2 . The temperature-sensitive material according to claim 1 , wherein the compound (B) is a fatty acid ester. 3 . The temperature sensitive material according to claim 2 , wherein the fatty acid ester is an ester compound of a monovalent aliphatic carboxylic acid having 10 to 25 carbon atoms and a monovalent aliphatic alcohol having 10 to 25 carbon atoms.
4. The temperature sensitive material according to claim 2 or 3, wherein the fatty acid ester is at least one compound selected from the group consisting of stearyl stearate, myristyl myristate, cetyl myristate and behenyl behenate. 5 . The temperature sensitive material according to claim 1 , wherein the content of the compound (B) is 20 to 70 parts by mass based on 100 parts by mass of the thermoplastic resin (A). 6 . The temperature sensitive material according to claim 1 , wherein the porous inorganic compound (C) has an oil absorption of 4.5 g / g or more and 10.0 g / g or less. 7 . The temperature sensitive material according to claim 1 , wherein the porous inorganic compound (C) is hydrophobic silica. 8 . The temperature sensitive material according to claim 1 , wherein the content of the porous inorganic compound (C) is 3 to 16 parts by mass based on 100 parts by mass of the thermoplastic resin (A). 9 . A formed body comprising the temperature sensitive material according to claim 1 .
10. A method for producing a temperature sensitive material according to any one of claims 1 to 8, comprising the step of kneading a thermoplastic resin (A), a compound (B) and a porous inorganic compound (C) at a temperature of 150°C or higher.