Protective film and preparation method thereof, curved screen assembly and electronic equipment

By using an anti-fingerprint layer containing double-terminated siloxane-based perfluoropolyether and single-terminated siloxane-based perfluoropolyether on curved screen mobile phones, combined with a hardened layer, the wear resistance and anti-fingerprint properties of the existing protective film are solved. It solves the problem of insufficient resistance, achieves better anti-fouling and anti-fingerprint effects, and extends the service life.

CN118834612APending Publication Date: 2024-10-25GUANGDONG OPPO MOBILE TELECOMMUNICATIONS CORP LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411110553.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

The protective film of existing curved screen mobile phones has poor wear resistance, fingerprint resistance, and oil resistance during use, resulting in oil and fingerprints easily remaining on the surface, affecting the user's visual experience.

Method used

A protective film including a base material layer, a hardened layer and an anti-fingerprint layer is designed. The anti-fingerprint layer is composed of double-ended siloxane-based perfluoropolyether and single-ended siloxane-based perfluoropolyether, with a mass ratio of 2 /3 to 4, by increasing the fluorine content and surface energy, it enhances the bonding with the hardened layer and provides better anti-fouling and anti-fingerprint effects.

Benefits of technology

It achieves longer service life and better anti-fouling and anti-fingerprint effects, reducing oil stains and fingerprint residues, and improving user experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118834612A_ABST
    Figure CN118834612A_ABST
Patent Text Reader

Abstract

The invention provides a protective film and a preparation method thereof, a curved screen assembly and electronic equipment. The protective film provided by the embodiment of the invention comprises a base material layer; the hardened layer is arranged on one side of the base material layer; the anti-fingerprint layer is arranged on one side, deviating from the base material layer, of the hardened layer; the anti-fingerprint layer is prepared from the following raw material components: double-end siloxane group perfluoropolyether and single-end siloxane group perfluoropolyether; the range of the mass ratio of the double-end siloxane group perfluoropolyether to the single-end siloxane group perfluoropolyether in the raw material components of the anti-fingerprint layer is 2 / 3 to 4. The protective film provided by the embodiment of the invention has a relatively good anti-smudginess effect and an anti-fingerprint effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electronics, and in particular to a protective film and a preparation method thereof, a curved screen assembly and an electronic device. Background Art

[0002] With the development of the form of electronic devices such as mobile phones, in order to pursue a large viewing area, a thin body, and a delicate appearance, more and more mobile phones and other electronic devices are designed with 3D curved screen covers, with curved surfaces on the left and right sides, or four curved surfaces with equal depth on four sides, etc. The protective film of curved screen mobile phones and other electronic devices in the related art has poor wear resistance, anti-fingerprint, and anti-oil effects. When people use curved screen mobile phones, oil stains and fingerprints are easily left on the surface, which will seriously affect the user's visual experience for a long time. Summary of the invention

[0003] The embodiment of the present application provides a protective film having good anti-fouling and anti-fingerprint effects.

[0004] In a first aspect, an embodiment of the present application provides a protective film, comprising:

[0005] substrate layer;

[0006] a hardening layer, the hardening layer being disposed on one side of the substrate layer; and

[0007] An anti-fingerprint layer, wherein the anti-fingerprint layer is arranged on a side of the hardened layer away from the substrate layer; the raw material components of the anti-fingerprint layer include a double-ended siloxane-based perfluoropolyether and a single-ended siloxane-based perfluoropolyether; the mass ratio of the double-ended siloxane-based perfluoropolyether and the single-ended siloxane-based perfluoropolyether in the raw material components of the anti-fingerprint layer is in a range of 2 / 3 to 4.

[0008] In a second aspect, the present application also provides a method for preparing a protective film, which comprises:

[0009] providing a substrate layer;

[0010] forming a hardening layer on one side of the base material layer; and

[0011] An anti-fingerprint layer is formed on a side of the hardened layer away from the substrate layer, wherein the anti-fingerprint layer comprises a dual-end siloxane-based perfluoropolyether and a single-end siloxane-based perfluoropolyether; in the anti-fingerprint layer, a mass ratio of the dual-end siloxane-based perfluoropolyether to the single-end siloxane-based perfluoropolyether is in a range of 2 / 3 to 4.

[0012] In a third aspect, the embodiment of the present application further provides a curved screen assembly, which includes:

[0013] A curved screen, the curved screen having a display surface; and

[0014] The protective film described in the embodiment of the present application is arranged on the display surface, between the substrate layer, the hardening layer and the curved screen.

[0015] In a fourth aspect, an embodiment of the present application further provides an electronic device, comprising:

[0016] The curved screen assembly described in the embodiment of the present application; and

[0017] A processor is electrically connected to the curved screen assembly and is used to control the curved screen assembly to display.

[0018] The protective film of the embodiment of the present application includes a substrate layer, a hardening layer and an anti-fingerprint layer. The raw material components of the anti-fingerprint layer include a double-ended siloxane-based perfluoropolyether and a single-ended siloxane-based perfluoropolyether; in the raw material components of the anti-fingerprint layer, the mass ratio of the double-ended siloxane-based perfluoropolyether and the single-ended siloxane-based perfluoropolyether is in the range of 2 / 3 to 4. In this embodiment, by designing the raw material components of the anti-fingerprint layer, the anti-fingerprint layer has a higher fluorine content, a lower surface energy and a higher initial water drop angle, so that it has better anti-fouling effect and anti-fingerprint effect. In addition, the anti-fingerprint layer can form a stable chemical bond with the hardening layer, so that the anti-fingerprint layer has better bonding with the hardening layer, so that the anti-fingerprint layer has a longer service life and is not easy to wear off or fall off after long-term use. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0020] Figure 1 It is a schematic diagram of the planar structure of a protective film according to an embodiment of the present application.

[0021] Figure 2 The protective film of the first embodiment of the present application is Figure 1 Schematic diagram of the structure in the AA direction.

[0022] Figure 3 The protective film of the second embodiment of the present application is Figure 1 Schematic diagram of the structure in the AA direction.

[0023] Figure 4 The protective film of the third embodiment of the present application is Figure 1 Schematic diagram of the structure in the AA direction.

[0024] Figure 5 The protective film of the fourth embodiment of the present application is Figure 1 Schematic diagram of the structure in the AA direction.

[0025] Figure 6 The protective film of the fifth embodiment of the present application is Figure 1 Schematic diagram of the structure in the AA direction.

[0026] Figure 7 The protective film of the sixth embodiment of the present application is Figure 1 Schematic diagram of the structure in the AA direction.

[0027] Figure 8 The protective film of the seventh embodiment of the present application is Figure 1 Schematic diagram of the structure in the AA direction.

[0028] Fig. 9 The protective film of the eighth embodiment of the present application is Figure 1 Schematic diagram of the structure in the AA direction.

[0029] Fig.10 It is a schematic flow chart of a first method for preparing a protective film according to an embodiment of the present application.

[0030] Fig.11 It is a schematic flow chart of a second method for preparing the protective film of an embodiment of the present application.

[0031] Fig.12 It is a schematic flow chart of the third method for preparing the protective film of the embodiment of the present application.

[0032] Fig.13 It is a schematic flow chart of a fourth method for preparing a protective film according to an embodiment of the present application.

[0033] Fig.14 It is a schematic flow chart of the fifth method for preparing the protective film of an embodiment of the present application.

[0034] Fig.15 It is a schematic flow chart of the sixth method for preparing the protective film of an embodiment of the present application.

[0035] Fig.16 It is a schematic structural diagram of a curved screen assembly according to an embodiment of the present application.

[0036] Fig.17 It is a schematic diagram of the exploded structure of the curved screen assembly according to an embodiment of the present application.

[0037] Fig.18 This is a side view of the curved screen assembly of one embodiment of the present application.

[0038] Fig.19 It is a schematic diagram of the structure of an electronic device according to an embodiment of the present application.

[0039] Fig. 20It is a schematic diagram of a partial exploded structure of an electronic device according to an embodiment of the present application.

[0040] Fig.21 It is a side view of an electronic device according to an embodiment of the present application.

[0041] Fig. 22 It is a circuit block diagram of an electronic device according to an embodiment of the present application.

[0042] Description of reference numerals:

[0043] 100-protective film, 10-base material layer, 20-hardening layer, 30-shaping layer, 40-adhesive layer, 50-anti-fingerprint layer, 60-intermediate treatment layer, 70-anti-reflective layer, 71-first coating layer, 72-second coating layer, 73-first coating, 74-second coating layer, 200-curved screen assembly, 210-curved screen, 211-display surface, 300-electronic device, 310-processor, 320-memory, 330-housing, 340-middle frame, 350-camera module. DETAILED DESCRIPTION

[0044] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0045] The terms "first", "second", etc. in the specification and claims of this application and the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally includes steps or units that are not listed, or optionally includes other steps or units inherent to these processes, methods, products or devices.

[0046] The technical solutions in the embodiments of the present application will be described below in conjunction with the accompanying drawings.

[0047] It should be noted that, for the convenience of explanation, in the embodiments of the present application, the same figure marks represent the same components, and for the sake of brevity, detailed descriptions of the same components are omitted in different embodiments.

[0048] With the development of the form of electronic devices such as mobile phones, in order to pursue a large viewing area, a thin body, and a delicate appearance, more and more mobile phones and other electronic devices are designed with 3D curved screen covers, with curved surfaces on the left and right sides, or four curved surfaces with equal depth on four sides, etc. The protective film of curved screen mobile phones and other electronic devices in the related art has poor wear resistance, anti-fingerprint, and anti-oil effects. When people use curved screen mobile phones, oil stains and fingerprints are easily left on the surface, which will seriously affect the user's visual experience for a long time.

[0049] See also Figure 1 and Figure 2 , the embodiment of the present application provides a protective film 100, which includes a substrate layer 10, a hardening layer 20 and an anti-fingerprint layer 50. The hardening layer 20 is arranged on one side of the substrate layer 10; the anti-fingerprint layer 50 is arranged on the side of the hardening layer 20 away from the substrate layer 10; the raw material components of the anti-fingerprint layer 50 include a double-ended siloxane-based perfluoropolyether and a single-ended siloxane-based perfluoropolyether; in the raw material components of the anti-fingerprint layer 50, the mass ratio of the double-ended siloxane-based perfluoropolyether to the single-ended siloxane-based perfluoropolyether is in the range of 2 / 3 to 4.

[0050] The protective film 100 of the embodiment of the present application is applied to electronic devices, as a protective film 100 for a 3D curved screen of an electronic device, and is used to protect the curved screen. Optionally, the electronic device may include but is not limited to portable electronic devices such as mobile phones, tablet computers, laptop computers, desktop computers, smart bracelets, smart watches, e-readers, game consoles, etc. Optionally, the curved screen may be curved on two relatively long sides, or on two relatively short sides, or on all four sides.

[0051] In the embodiments of the present application, when a numerical value range from a to b is involved, unless otherwise specified, it means that the numerical value can be any numerical value between a and b, including the endpoint numerical value a and the endpoint numerical value b.

[0052] It can be understood that the substrate layer 10, the hardening layer 20 and the anti-fingerprint layer 50 are stacked in sequence. When the protective film 100 is applied to a curved screen, the substrate layer 10 is closer to the display surface of the curved screen than the anti-fingerprint layer 50. In other words, the anti-fingerprint layer 50 is closer to the contact surface, that is, the outer surface, than the substrate layer 10.

[0053] Specifically, in the raw material components of the anti-fingerprint layer 50, the mass ratio of the dual-end siloxane-based perfluoropolyether to the single-end siloxane-based perfluoropolyether can be, but is not limited to, 2 / 3, 0.8, 1, 1.3, 1.5, 1.8, 2, 2.3, 2.5, 2.8, 3, 3.2, 3.5, 3.8, 4, etc. Both ends of the double-ended siloxanyl perfluoropolyether are siloxanyl groups. After hydrolysis, the siloxanyl group at one end can react with the adjacent double-ended siloxanyl perfluoropolyether or single-ended siloxanyl perfluoropolyether, and the other end can react with the -OH of the hardened layer 20 to play a bridging role, thereby improving the bonding between the anti-fingerprint layer 50 and the hardened layer 20. In addition, the double-ended siloxanyl perfluoropolyether can also increase the F (fluorine) content in the anti-fingerprint layer 50, thereby improving the anti-fouling and anti-fingerprint performance of the anti-fingerprint layer 50; only one end of the single-ended siloxanyl perfluoropolyether can participate in the reaction. When the siloxanyl group of the siloxanyl perfluoropolyether is hydrolyzed, it preferentially participates in the reaction between the double-ended siloxanyl perfluoropolyether or the single-ended siloxanyl perfluoropolyether, thereby playing a capping role. At the same time, the single-ended siloxanyl perfluoropolyether can also increase the F (fluorine) content in the anti-fingerprint layer 50, thereby improving the anti-fouling and anti-fingerprint performance of the anti-fingerprint layer 50. The mass ratio of the double-ended siloxane perfluoropolyether to the single-ended siloxane perfluoropolyether in the raw material components of the anti-fingerprint layer 50 is too large, that is, the content of the double-ended siloxane perfluoropolyether is too high, the molecular structure stability of the anti-fingerprint coating (AF coating, that is, the coating composed of the raw material components of the anti-fingerprint layer 50) is poor, and the siloxane groups in the double-ended siloxane perfluoropolyether or the single-ended siloxane perfluoropolyether that do not participate in the reaction are easily hydrolyzed; the mass ratio of the double-ended siloxane perfluoropolyether to the single-ended siloxane perfluoropolyether in the raw material components of the anti-fingerprint layer 50 is too low, that is, the content of the single-ended siloxane perfluoropolyether is too high, the ends of the molecular chains in the anti-fingerprint coating are all CF stable bonds, it is difficult to form a bridge with the hardening layer 20, and the adhesion is poor.

[0054] It can be understood that the anti-fingerprint layer 50 is formed by curing the anti-fingerprint coating liquid.

[0055] Optionally, the structural formula of the double-terminal siloxane-based perfluoropolyether is:

[0056] Optionally, the structural formula of the single-ended siloxane-based perfluoropolyether is:

[0057] The protective film 100 of the embodiment of the present application includes a substrate layer 10, a hardening layer 20 and an anti-fingerprint layer 50. The raw material components of the anti-fingerprint layer 50 include a double-ended siloxane-based perfluoropolyether and a single-ended siloxane-based perfluoropolyether; in the raw material components of the anti-fingerprint layer 50, the mass ratio of the double-ended siloxane-based perfluoropolyether and the single-ended siloxane-based perfluoropolyether is in the range of 2 / 3 to 4. In this embodiment, by designing the raw material components of the anti-fingerprint layer 50, the anti-fingerprint layer 50 has a higher fluorine content, a lower surface energy and a higher initial water drop angle, so that it has a better anti-fouling effect and anti-fingerprint effect. In addition, the anti-fingerprint layer 50 can form a stable chemical bond with the hardening layer 20, so that the anti-fingerprint layer 50 has a better bonding with the hardening layer 20, so that the anti-fingerprint layer 50 has a longer service life and is not easy to wear off or fall off after long-term use.

[0058] Optionally, the thickness of the protective film 100 ranges from 100 μm to 120 μm. Specifically, the thickness of the protective film 100 may be, but is not limited to, 100 μm, 102 μm, 104 μm, 106 μm, 108 μm, 110 μm, 112 μm, 114 μm, 116 μm, 118 μm, 120 μm, etc. If the thickness of the protective film 100 is too thin, the strength of the protective film 100 is insufficient, and when applied to a curved screen assembly, the protective force of the curved screen is reduced; if the thickness of the protective film 100 is too thick, the rigidity of the protective film 100 is too high, and when the protective film 100 is attached to the curved screen, it is easy to warp.

[0059] Furthermore, the thickness of the protective film 100 ranges from 105 μm to 110 μm. Specifically, the thickness of the protective film 100 may be, but is not limited to, 105 μm, 106 μm, 107 μm, 108 μm, 109 μm, 110 μm, etc. In this way, the protective film 100 can have better protection and better fit with the curved screen, making it less prone to warping.

[0060] Optionally, the thickness of the substrate layer 10 ranges from 18 μm to 40 μm. Specifically, the thickness of the substrate layer 10 may be, but is not limited to, 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm, 25 μm, 28 μm, 30 μm, 33 μm, 35 μm, 38 μm, 40 μm, etc. If the thickness of the substrate layer 10 is too thin, the coating difficulty will be increased when the substrate layer 10 is prepared by coating, and the hardness is not enough, which reduces the wear resistance of the protective film 100. In addition, the stiffness of the substrate layer 10 is not enough, which makes the protective film 100 prone to wrinkles, orange peel and other poor appearance phenomena; if the thickness of the substrate layer 10 is too thick, the rebound force of the protective film 100 during shaping is too large, which makes the protective film 100 not fit the edge of the curved screen well and prone to warping.

[0061] Furthermore, the thickness of the substrate layer 10 is in the range of 18 μm to 25 μm. In this way, the substrate layer 10 has good coating performance during preparation, high strength and hardness, and low rebound force, which can well support the hardening layer 20. When applied to a curved screen, the protective film 100 has good adhesion to the curved screen and is not prone to warping.

[0062] In some embodiments, the substrate layer 10 is isotropic, and the substrate layer 10 includes at least one of thermoplastic elastomers such as thermoplastic polyurethane and silicone rubber.

[0063] It can be understood that the substrate layer 10 is non-polarized.

[0064] In the related art, the substrate is usually made of polyethylene terephthalate (PET) and the like. The substrate is usually prepared by biaxial stretching. During the stretching process, the molecular chains will be oriented, which makes the substrate of the related art anisotropic and has high mechanical strength. When it is applied to the protective film of the curved screen and is formed, the forming layer will shrink in volume toward the substrate layer after photocuring. The modulus of the substrate layer is large, which will produce greater stress and rebound force, so that warping, bubbles, wrinkles, etc. are likely to occur at the edge of the curved screen, making it difficult to fully fit the curved screen.

[0065] The substrate layer 10 of the embodiment of the present application is isotropic, and thermoplastic polyurethane and silicone rubber have a lower elastic modulus than substrates such as PET, are soft and easy to deform, and have extremely low rebound force. Therefore, when applied to a curved screen, the substrate layer 10 can easily deform together with the shaping layer when the protective film 100 is formed, so that it can better fit the structure of the curved screen, and is not prone to rebound or warping after fitting, thereby better protecting the curved screen.

[0066] The substrate layer 10 of the embodiment of the present application is isotropic, and thermoplastic polyurethane and silicone rubber have a lower elastic modulus than substrates such as PET, are easy to deform themselves, and have extremely low rebound force. Therefore, when applied to a curved screen, the substrate layer 10 can easily deform together with the shaping layer when the protective film 100 is formed, so that it can better fit the structure of the curved screen, and is not prone to rebound or warping after fitting, thereby better protecting the curved screen.

[0067] In some embodiments, the elastic modulus of the substrate layer 10 ranges from 1.5 GPa to 4 GPa. Specifically, the elastic modulus of the substrate layer 10 may be, but is not limited to, 1.5 GPa, 1.8 GPa, 2.0 GPa, 2.3 GPa, 2.5 GPa, 2.8 GPa, 3.0 GPa, 3.3 GPa, 3.5 GPa, 3.8 GPa, 4.0 GPa, etc. If the elastic modulus of the substrate layer 10 is too low, the hardness of the substrate layer 10 is insufficient, which reduces the hardness and wear resistance of the protective film 100. In addition, the stiffness of the substrate layer 10 is insufficient, which makes the protective film 100 prone to wrinkles, orange peel and other poor appearance phenomena; if the elastic modulus of the substrate layer 10 is too high, the rebound force of the protective film 100 during shaping is too large, which makes the protective film 100 not fit the edge of the curved screen well and prone to warping.

[0068] Optionally, the tensile strength of the substrate layer 10 ranges from 40MPa to 100MPa. Specifically, the tensile strength of the substrate layer 10 may be, but is not limited to, 40MPa, 50MPa, 60MPa, 70MPa, 80MPa, 90MPa, 100MPa, etc. If the tensile strength of the substrate layer 10 is too low, the hardness of the substrate layer 10 is insufficient, which reduces the hardness and wear resistance of the protective film 100. In addition, the stiffness of the substrate layer 10 is insufficient, which makes the protective film 100 prone to wrinkles, orange peel and other poor appearance phenomena; if the tensile strength of the substrate layer 10 is too high, the rebound force of the protective film 100 during shaping is too large, which makes the protective film 100 not fit the edge of the curved screen well and prone to warping.

[0069] Optionally, the elongation at break of the substrate layer 10 ranges from 1% to 5%. Specifically, the elongation at break of the substrate layer 10 may be, but is not limited to, 1%, 1.5%, 2%, 3%, 4%, 5%, etc. If the elongation at break of the substrate layer 10 is too large, the hardness of the substrate layer 10 is insufficient, which reduces the hardness and wear resistance of the protective film 100. In addition, the stiffness of the substrate layer 10 is insufficient, which makes the protective film 100 prone to wrinkles, orange peel and other poor appearance phenomena; if the elongation at break of the substrate layer 10 is too small, the bending and stretching properties of the substrate layer 10 are insufficient, and the rebound force of the protective film 100 during shaping is too large, which makes the protective film 100 not fit the edge of the curved screen well and prone to warping.

[0070] Optionally, the thickness of the hardened layer 20 ranges from 1 μm to 5 μm. Specifically, the thickness of the hardened layer 20 may be, but is not limited to, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, etc. If the thickness of the hardened layer 20 is too thin, the hardness and wear resistance of the hardened layer 20 are reduced, and the stiffness is reduced, so that the smoothness and feel of the protective film 100 are reduced; if the thickness of the hardened layer 20 is too thick, the hardness of the hardened layer 20 is too large, and the rebound force of the protective film 100 during shaping is too large, so that the protective film 100 is not sufficiently fitted to the edge of the curved screen, and warping is prone to occur.

[0071] In some embodiments, the raw material components (also referred to as hardening liquid) of the hardening layer 20 include, by mass fraction: 20% to 50% of polyurethane acrylate prepolymer, 10% to 30% of hyperbranched acrylic resin, 3% to 10% of short-chain fluoride, 1% to 10% of inorganic particles, 5% to 20% of the first reaction monomer, 0.5% to 2% of the first photoinitiator and the remainder of the first solvent.

[0072] Specifically, the mass fraction of the polyurethane acrylate prepolymer in the raw material components of the hardened layer 20 may be, but not limited to, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc. The mass fraction of the hyperbranched acrylic resin in the raw material components of the hardened layer 20 may be, but not limited to, 10%, 15%, 20%, 25%, 30%, etc. The mass fraction of the short-chain fluoride in the raw material components of the hardened layer 20 may be, but not limited to, 3%, 5%, 7%, 9%, 10%, etc. The mass fraction of the inorganic particles in the raw material components of the hardened layer 20 may be, but not limited to, 1%, 3%, 5%, 7%, 9%, 10%, etc. The mass fraction of the first reaction monomer in the raw material components of the hardened layer 20 may be, but not limited to, 5%, 8%, 10%, 13%, 15%, 18%, 20%, etc. The mass fraction of the first photoinitiator in the raw material components of the hardened layer 20 may be, but is not limited to, 0.5%, 1%, 1.5%, 2%, etc.

[0073] In this embodiment, the hardening layer 20 includes polyurethane acrylate resin and hyperbranched acrylic resin. Polyurethane acrylate is the main molecular structure, providing the main mechanical properties and molecular chain structure. The hyperbranched acrylic resin plays a toughening and strengthening role. Through the combination of polyurethane acrylate resin and hyperbranched acrylic resin, the hardening layer 20 has high hardness and rigidity, high wear resistance and scratch resistance, and good toughness. When applied to a curved screen, it can be bent better and is not easy to crack. In addition, the hyperbranched acrylic resin has the characteristics of good fluidity, low viscosity, not easy to crystallize, good film-forming properties, and good solubility and good weather resistance. The hyperbranched acrylic resin is applied to the polyurethane acrylate resin system to effectively increase the double bond content of the system, thereby effectively improving the rate of light curing (such as ultraviolet light curing, referred to as UV curing) and the mechanical properties of the hardening layer 20; furthermore, at the same solid content, the hyperbranched acrylic resin can significantly reduce the viscosity of the system, which is beneficial to the construction of the hardening layer 20 and saves energy consumption. Furthermore, the hyperbranched acrylic resin has more side chains, which can better form a cross-linked network structure in the hardened layer 20, increase the cross-linking degree of the hardened layer 20, and make the hardened layer 20 have better toughness and wear resistance. In addition, in this embodiment, the hardened layer 20 also includes short-chain fluorides. Short-chain fluorides can improve the anti-fingerprint performance and anti-fouling performance of the hardened layer 20. Furthermore, in this embodiment, the hardened layer 20 also includes inorganic particles, which can increase the wear resistance and hardness of the hardened layer 20 and improve the service life of the protective film 100.

[0074] Optionally, the inorganic particles are nanoparticles, and the inorganic particles may be, but are not limited to, at least one of aluminum oxide, silicon dioxide, boron nitride, silicon nitride, zirconium oxide, and the like.

[0075] Optionally, the short-chain fluorinated compound may be, but is not limited to, at least one of perfluoropolyether (PFPE) and perfluoropolyether derivatives.

[0076] Optionally, the first reactive monomer may be, but is not limited to, at least one of acrylic monomers such as ethoxylated trimethylolpropane triacrylate, pentaerythritol hexaacrylate, isobornyl acrylate, and 1,6-hexanediol diacrylate.

[0077] Optionally, the first photoinitiator can be, but is not limited to, methyl benzoylformate, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (TPO), propyl thioxanthone (ITX), benzophenone (BP), photoinitiator 1700 (25 wt% of photoinitiator 819 and 75 wt% of photoinitiator 1173), bis [2,6-difluoro-3- (1H-pyrrolyl-1) phenyl] titanocene (photoinitiator 784), photoinitiator 1800 (25% photoinitiator 819 and 75% photoinitiator 184), photoinitiator 4265 (50% TPO and 50% photoinitiator 1173), 1-hydroxycyclohexyl phenyl ketone (1-hydroxycyclohexyl phenyl ketone, photoinitiator 184), 2-Hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (photoinitiator 2959), 2-hydroxy-2-methyl-1-phenyl-1-propanone (photoinitiator 1173), 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone (photoinitiator 907), 2-hydroxy-1-[4-[4-(2-hydroxy-2-methylpropionyl)phenoxy]phenyl]-2-methylpropanone (photoinitiator 160), etc.

[0078] Optionally, the first solvent may be, but is not limited to, one or more of ethyl acetate, propyl acetate, butyl acetate, cyclohexanone, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether, isopropanol, butanone, and methyl butanone.

[0079] In some embodiments, the raw material components of the anti-fingerprint layer 50 further include a hydrolysis promoter, and the amount of the hydrolysis promoter added to the raw material components of the anti-fingerprint layer 50 is 2% to 10% of the total mass of the dual-end siloxane perfluoropolyether and the single-end siloxane perfluoropolyether.

[0080] Specifically, the amount of the hydrolysis promoter added in the raw material components of the anti-fingerprint layer 50 can be but is not limited to 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10% and the like of the total mass of the dual-end siloxane perfluoropolyether and the single-end siloxane perfluoropolyether. If the mass fraction of the hydrolysis promoter in the raw material components of the anti-fingerprint layer 50 is too small, the hydrolysis amount of the single-end siloxane perfluoropolyether and the double-end siloxane perfluoropolyether is small, the reaction with the hardening layer 20 is small, the bridging effect between the anti-fingerprint layer 50 and the hardening layer 20 is small, and the bonding force between the anti-fingerprint layer 50 and the hardening layer 20 or the anti-fingerprint layer 50 is reduced; if the mass fraction of the hydrolysis promoter in the raw material components of the anti-fingerprint layer 50 is too large, after the single-end siloxane perfluoropolyether and the double-end siloxane perfluoropolyether are hydrolyzed, the reaction in the anti-fingerprint layer 50 is too intense, which will also reduce the reaction between the single-end siloxane perfluoropolyether and the double-end siloxane perfluoropolyether and the hardening layer 20, and reduce the bonding force between the anti-fingerprint layer 50 and the hardening layer 20.

[0081] Optionally, the hydrolysis accelerator may be, but is not limited to, at least one of diisopropyl ether, lauryl alcohol, sodium lauryl sulfate, lauryl alcohol polyoxyethylene ether, isooctyl alcohol and chain polyethylene glycol.

[0082] In the embodiment of the present application, a hydrolysis promoter is added to the raw material components of the anti-fingerprint layer 50, so as to promote the hydrolysis of the single-end siloxanyl perfluoropolyether and the double-end siloxanyl perfluoropolyether, increase the reaction between the single-end siloxanyl perfluoropolyether and the double-end siloxanyl perfluoropolyether, and increase the reaction between the double-end siloxanyl perfluoropolyether and the hardening layer 20, so as to better improve the bonding force between the anti-fingerprint layer 50 and the hardening layer 20.

[0083] In some embodiments, the raw material components of the anti-fingerprint layer 50 include, by mass fraction, 10% to 30% of dual-end siloxane-based perfluoropolyether, 5% to 20% of single-end siloxane-based perfluoropolyether, and 1% to 3% of a hydrolysis accelerator.

[0084] It can be understood that the anti-fingerprint coating liquid includes, by mass fraction, 10% to 30% of dual-end siloxane-based perfluoropolyether, 5% to 20% of single-end siloxane-based perfluoropolyether and 1% to 3% of a hydrolysis accelerator.

[0085] Specifically, the mass fraction of the bisiloxane perfluoropolyether in the raw material components of the anti-fingerprint layer 50 can be, but is not limited to, 10%, 13%, 15%, 18%, 20%, 23%, 25%, 28%, 30%, etc.

[0086] Specifically, the mass fraction of the single-ended siloxane-based perfluoropolyether in the raw material components of the anti-fingerprint layer 50 may be, but is not limited to, 5%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, etc.

[0087] Specifically, the mass fraction of the hydrolysis promoter in the raw material components of the anti-fingerprint layer 50 may be, but is not limited to, 1%, 1.3%, 1.5%, 1.8%, 2%, 2.3%, 2.5%, 2.8%, 3%, etc.

[0088] The anti-fingerprint layer 50 made of the raw material components of the anti-fingerprint layer 50 described in this embodiment has better anti-fouling effect and anti-fingerprint effect, and has better bonding force with the hardening layer 20 and better wear resistance, thereby having a longer service life.

[0089] Optionally, the anti-fingerprint coating liquid further includes a fluoroether solvent and an auxiliary agent.

[0090] Optionally, the fluoroether solvent may be, but is not limited to, at least one of perhydrofluoroether, tetrafluoroethyl ether, trifluoroethyl ether, difluoromethyl-2,2,2-trifluoroethyl ether, trifluoromethylethane (HFC-236fa), hexafluoroisopropyl ether (HFIP), hexafluoroacetone (HFA), hexafluoroisopropanol (HFIP-OH), etc. Optionally, the auxiliary agent may be, but is not limited to, at least one of a leveling agent and a defoaming agent, etc.

[0091] In a specific embodiment, the anti-fingerprint coating liquid includes, by mass fraction: 10% to 30% of double-ended siloxane-based perfluoropolyether, 5% to 20% of single-ended siloxane-based perfluoropolyether, 50% to 83% of fluoroether solvent, 1% to 3% of hydrolysis promoter, and 1% to 5% of auxiliary agent.

[0092] Optionally, the thickness of the anti-fingerprint layer 50 is 10nm to 120nm. Specifically, the thickness of the anti-fingerprint layer 50 may be, but is not limited to, 10nm, 12nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, etc. If the thickness of the anti-fingerprint layer 50 is too small, the anti-fingerprint effect of the anti-fingerprint layer 50 is reduced; if the thickness of the anti-fingerprint layer 50 is too thick, the cost of the anti-fingerprint layer 50 is increased.

[0093] In some embodiments, the number average molecular weight of the bi-terminal siloxane-based perfluoropolyether ranges from 3000 to 8000. Specifically, the number average molecular weight of the bi-terminal siloxane-based perfluoropolyether may be, but is not limited to, 3000, 3500, 4000, 4500, 5000, 5500, 6000, 6500, 7000, 7500, 8000, etc. If the number average molecular weight of the bi-terminal siloxane-based perfluoropolyether is too small, the fluorine content in the anti-fingerprint layer 50 is too low, which reduces the anti-fingerprint performance and anti-fouling performance of the anti-fingerprint layer 50; if the number average molecular weight of the bi-terminal siloxane-based perfluoropolyether is too large, the preparation cost of the anti-fingerprint layer 50 is increased, and it is even difficult to achieve.

[0094] Optionally, the number average molecular weight of the single-ended siloxane-based perfluoropolyether is 1000 to 8000. Specifically, the number average molecular weight of the single-ended siloxane-based perfluoropolyether may be, but is not limited to, 1000, 1500, 2000, 2500, 3000, 3500, 4000, 4500, 5000, 5500, 6000, 6500, 7000, 7500, 8000, etc. If the number average molecular weight of the single-ended siloxane-based perfluoropolyether is too small, the fluorine content in the anti-fingerprint layer 50 is too low, which reduces the anti-fingerprint performance and anti-fouling performance of the anti-fingerprint layer 50; if the number average molecular weight of the single-ended siloxane-based perfluoropolyether is too large, the preparation cost of the anti-fingerprint layer 50 is increased, and it is even difficult to achieve.

[0095] In this embodiment, by designing the number average molecular weight of the dual-end siloxane-based perfluoropolyether and the single-end siloxane-based perfluoropolyether, the anti-fingerprint layer 50 has a higher fluorine content, thereby having a lower surface energy and a higher initial water drop angle, and having better anti-fingerprint and anti-fouling effects.

[0096] See also Figure 3 In some embodiments, the protective film 100 further includes an intermediate processing layer 60 , wherein the intermediate processing layer 60 is located between the hardening layer 20 and the anti-fingerprint layer 50 , and the intermediate processing layer 60 includes a silane coupling agent.

[0097] Optionally, the silane coupling agent may be, but is not limited to, at least one of 2-chloroethylmethyldimethoxysilane, γ-aminopropyltriethoxysilane (KH550), 3-(2,3-epoxypropoxy)propyltrimethoxysilane (KH560), γ-methacryloxypropyltrimethoxysilane (KH570), and the like.

[0098] In this embodiment, an intermediate treatment layer 60 having a silane coupling agent is added between the hardening layer 20 and the anti-fingerprint layer 50, and the alkyl group of the silane coupling agent has good compatibility with the hardening layer 20; in addition, the -Si-OH formed after the hydrolysis of the silane coupling agent can react with the -OH of the inorganic nanoparticles in the hardening layer 20 and the -Si-OH generated by the hydrolysis of the double-ended siloxane-based perfluoropolyether and the single-ended siloxane-based perfluoropolyether of the anti-fingerprint layer 50, thereby forming a stable Si-O-Si chemical bond, which plays a bridging role, thereby improving the adhesion between the hardening layer 20 and the anti-fingerprint layer 50. In addition, the wear resistance of the protective film 100 can be better improved, and the service life of the anti-fingerprint layer 50 can be improved.

[0099] In some embodiments, the intermediate treatment layer 60 further includes inorganic nanoparticles. In the intermediate treatment layer 60 , the mass fraction of the silane coupling agent ranges from 97.5% to 99.9%, and the mass fraction of the inorganic nanoparticles ranges from 0.1% to 2.5%.

[0100] Optionally, the inorganic nanoparticles may be, but are not limited to, at least one of aluminum oxide, silicon dioxide, boron nitride, silicon nitride, zirconium oxide, and the like.

[0101] Specifically, in the intermediate treatment layer 60, the mass fraction of the inorganic nanoparticles may be, but is not limited to, 0.1%, 0.3%, 0.5%, 0.8%, 1.0%, 1.3%, 1.5%, 1.8%, 2.0%, 2.3%, 2.5%, etc.

[0102] Specifically, in the intermediate treatment layer 60, the mass fraction of the silane coupling agent can be but is not limited to 97.5%, 97.8%, 98%, 98.3%, 98.5%, 98.8%, 99%, 99.3%, 99.6%, 99.9%, etc.

[0103] In this embodiment, inorganic nanoparticles are added to the intermediate treatment layer 60 to increase the amount of -Si-OH in the intermediate treatment layer 60, thereby increasing the bridging effect between the intermediate treatment layer 60 and the hardening layer 20 and the intermediate treatment layer 60 and the anti-fingerprint layer 50, improving the bonding force between the anti-fingerprint layer 50 and the hardening layer 20, thereby improving the anti-fingerprint effect and service life of the protective film 100. If the content of inorganic nanoparticles in the intermediate treatment layer 60 is too low, the improvement of the bonding force between the intermediate treatment layer 60 and the hardening layer 20 and the intermediate treatment layer 60 and the anti-fingerprint layer 50 is limited; if the content of inorganic nanoparticles in the intermediate treatment layer 60 is too high, the haze of the intermediate treatment layer 60 is increased, the light transmittance of the intermediate treatment layer 60 is reduced, and thus the light transmittance of the protective film 100 is reduced.

[0104] Optionally, the intermediate treatment layer 60 is formed by coating a treatment liquid. Optionally, the treatment liquid includes 40% to 80% of a silane coupling agent, 0.1% to 1% of inorganic nanoparticles, and 19.9% ​​to 59% of a solvent by mass fraction. Optionally, the solvent may be, but is not limited to, one or more of ethyl acetate, propyl acetate, butyl acetate, cyclohexanone, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether, isopropyl alcohol, butanone, and methyl butanone.

[0105] Optionally, the thickness of the intermediate processing layer 60 ranges from 5nm to 80nm. Specifically, the thickness of the intermediate processing layer 60 may be, but is not limited to, 5nm, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, etc. If the thickness of the intermediate processing layer 60 is too thin, the effective component that can provide adhesion is low, the intermediate processing layer 60 forms fewer chemical bonds with the hardening layer 20 and the anti-fingerprint layer 50, and the bridging effect is weak; if the thickness of the intermediate processing layer 60 is too thick, the preparation cost of the protective film 100 is increased; in addition, compared with the hardening layer 20 and the anti-fingerprint layer 50, the wear resistance of the processing layer is poor, and the thickness of the intermediate processing layer 60 is too thick, which will reduce the wear resistance of the protective film 100.

[0106] In some embodiments, a thickness ratio of the intermediate treatment layer 60 to the anti-fingerprint layer 50 ranges from 0.5 to 0.67.

[0107] Specifically, the thickness ratio of the intermediate processing layer 60 to the anti-fingerprint layer 50 may be, but is not limited to, 0.5, 0.52, 0.54, 0.56, 0.58, 0.60, 0.62, 0.64, 0.66, 0.67, etc.

[0108] In this embodiment, if the thickness ratio of the intermediate processing layer 60 to the anti-fingerprint layer 50 is too small, the thickness of the intermediate processing layer 60 is too thin, and it is difficult to control the uniformity of the coating when the processing liquid is applied; in addition, if the intermediate processing layer 60 is too thin, the effective component that can provide adhesion is relatively low, and the chemical bonds formed by the intermediate processing layer 60 with the hardening layer 20 and the anti-fingerprint layer 50 are relatively small, and the bridging effect is relatively weak; if the thickness ratio of the intermediate processing layer 60 to the anti-fingerprint layer 50 is too large, the intermediate processing layer 60 is relatively thick, which increases the preparation cost of the protective film 100; in addition, compared with the hardening layer 20 and the anti-fingerprint layer 50, the wear resistance of the processing layer is poor, and the thickness of the intermediate processing layer 60 is too thick, which will reduce the wear resistance of the protective film 100.

[0109] See also Figure 4 and Figure 5In some embodiments, the protective film 100 is applied to a curved screen, and the protective film 100 further includes a shaping layer 30 and an adhesive layer 40, wherein the shaping layer 30 is disposed on a side of the substrate layer 10 away from the hardening layer 20, and the shaping layer 30 is a heat-light dual-curing shaping layer 30, and before the protective film 100 is applied to the curved screen, the shaping layer 30 is thermally cured, and when the protective film 100 is applied to the curved screen, the shaping layer 30 is light-cured and shaped; and an adhesive layer 40, wherein the adhesive layer 40 is disposed on a side of the shaping layer 30 away from the substrate layer 10, and the adhesive layer 40 is used to bond the protective film 100 to the curved screen.

[0110] Optionally, the thickness of the shaping layer 30 is in the range of 60μm to 120μm. Specifically, the thickness of the shaping layer 30 may be, but is not limited to, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, etc. If the thickness of the shaping layer 30 is too thin, when the protective film 100 is applied to the curved screen and shaped, the shaping force provided by the shaping layer 30 is insufficient, so that the protective film 100 is prone to warping. In addition, if the shaping layer 30 is too thin, the hardness and stiffness of the protective film 100 will be reduced, affecting the wear resistance of the protective film 100. If the thickness of the shaping layer 30 is too thick, it will increase the difficulty of coating the shaping layer 30, and it is easy to make the coating of the shaping layer 30 uneven. In addition, after the shaping layer 30 is cured, the volume shrinks too much, and the internal stress generated by the volume shrinkage is easy to cause the protective film 100 to warp when it is attached to the curved screen.

[0111] Further, the thickness of the shaping layer 30 is in the range of 70 μm to 80 μm. Specifically, the thickness of the shaping layer 30 may be, but is not limited to, 70 μm, 72 μm, 74 μm, 76 μm, 78 μm, 80 μm, etc. In this way, the shaping layer 30 has a higher shaping force and a more suitable hardness, and is not prone to warping when attached to a curved screen.

[0112] Optionally, the setting layer 30 is formed by curing the setting liquid. The raw material components of the setting layer 30 include a first raw material component and a second raw material component, wherein the first raw material component includes 20% to 70% of polyurethane acrylate prepolymer, 0.1% to 1% of a first coupling agent, 15% to 30% of a second reactive monomer, 5% to 30% of a curing agent, 0.5% to 3% of a second photoinitiator and the remainder of a second solvent by mass fraction. The second raw material component includes 40% to 80% of an acrylic monomer, 0.1% to 1% of a second coupling agent, 1% to 5% of a film-forming agent and the remainder of a third solvent by mass fraction. The mass ratio of the first raw material component to the second raw material component ranges from 3 to 8. The setting layer 30 prepared by the setting liquid of this embodiment has better setting force, and when the protective film 100 is applied to a curved screen, it has a better setting effect, and makes the protective film 100 have a better fit with the curved screen, and is more prone to warping or rebounding.

[0113] Optionally, in the first raw material component, the weight average molecular weight of the polyurethane acrylate prepolymer ranges from 4,000 to 12,000.

[0114] Optionally, one of the first coupling agent and the second coupling agent is a silane coupling agent, and the other is a silane coupling agent with a thermal reaction group. One of the first coupling agent and the second coupling agent is a silane coupling agent, and the other is a silane coupling agent with a thermal reaction group. Adding a silane coupling agent to the raw material components of the shaping layer 30 can improve the compatibility of the first raw material component and the second raw material component. The silane coupling agent with a thermal reaction group can form a cross-linked network structure in the shaping layer 30, and increase the cross-linking degree of the shaping layer 30 without affecting the flexibility of the shaping layer 30, so that the shaping layer 30 has better resistance to high and low temperature. In addition, the addition of the first coupling agent and the second coupling agent can also increase the bonding performance of the shaping layer 30 and the film layer directly attached to the substrate layer.

[0115] Optionally, the silane coupling agent may be, but is not limited to, at least one of 2-chloroethylmethyldimethoxysilane, γ-aminopropyltriethoxysilane (KH550), 3-(2,3-epoxypropoxy)propyltrimethoxysilane (KH560), γ-methacryloxypropyltrimethoxysilane (KH570), and the like.

[0116] Optionally, the thermal reaction group may be, but is not limited to, at least one of an isocyanate group, a hydroxyl group, a carboxyl group, etc. The silane coupling agent having a thermal reaction group may be, but is not limited to, a silane coupling agent having a group such as an isocyanate group, a hydroxyl group, a carboxyl group, etc. Specifically, the silane coupling agent having a thermal reaction group may be, but is not limited to, at least one of 3-isocyanate propyl trimethoxy silane, a dihydroxy silane coupling agent, etc.; that is, the second coupling agent may be, but is not limited to, at least one of 3-isocyanate propyl trimethoxy silane, a dihydroxy silane coupling agent, etc.

[0117] Optionally, the second reactive monomer may be, but is not limited to, at least one of hydroxyethyl methacrylate, ethylene glycol dimethacrylate, diphenylmethane diisocyanate, etc. The second reactive monomer is used to participate in the reaction and dilute the glue solution composed of the first raw material component.

[0118] Optionally, the curing agent may be, but is not limited to, at least one of succinic anhydride, maleic anhydride, and the like.

[0119] Optionally, the second photoinitiator may be but is not limited to at least one of methyl benzoylformate, TPO, ITX, BP, photoinitiator 1700, photoinitiator 784, photoinitiator 1800, photoinitiator 4265, photoinitiator 184, photoinitiator 2959, photoinitiator 1173, photoinitiator 907, photoinitiator 160, etc.

[0120] Optionally, the second solvent may be, but is not limited to, one or more of ethyl acetate, propyl acetate, butyl acetate, toluene, cyclohexanone, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether, isopropanol, butanone, and methyl butanone.

[0121] Optionally, the acrylic monomer may be, but is not limited to, at least one of hydroxyethyl methacrylate, methacrylic acid (MMA), ethylene glycol dimethacrylate, and the like.

[0122] Alternatively, the film former may be, but is not limited to, poly(melamine-co-formaldehyde)methanol.

[0123] Optionally, the third solvent may be, but is not limited to, one or more of methylal, ethyl acetate, propyl acetate, butyl acetate, cyclohexanone, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether, isopropanol, butanone, and methyl butanone.

[0124] Optionally, after the shaping layer 30 is thermally cured and before light-curing, the peeling force of the adhesive layer 40 on the surface with a water drop angle of 115° ranges from 40gf / 25mm to 100gf / 25mm; after the shaping layer 30 is thermally-light-durable, the peeling force of the adhesive layer 40 on the surface with a water drop angle of 115° ranges from 10gf / 25mm to 40gf / 25mm.

[0125] It can be understood that after the shaping layer 30 is thermally cured but before light-curing, the peeling force of the adhesive layer 40 for the curved screen with a water drop angle of 115° ranges from 40gf / 25mm to 100gf / 25mm; after the shaping layer 30 is thermally-light-durable, the peeling force of the adhesive layer 40 for the curved screen with a water drop angle of 115° ranges from 10gf / 25mm to 40gf / 25mm.

[0126] It should be noted that after the shaping layer 30 is photocured, the shaping layer 30 shrinks in volume and hardens, generating a shrinking tensile force or internal stress on the adhesive layer 40, thereby making the adhesive layer 40 harder as a whole and reducing its viscosity. Therefore, after the shaping layer 30 is dual-cured by heat and light, the peeling force of the adhesive layer 40 on the curved screen or surface is reduced.

[0127] Optionally, the material of the adhesive layer 40 may be, but is not limited to, at least one of silicone glue, acrylic glue, and the like.

[0128] In this embodiment, if the peeling force of the adhesive layer 40 on the surface with a water drop angle of 115° is too small, then when the protective film 100 is attached to the curved screen, the adhesion between the protective film 100 and the curved screen is insufficient, and it is easy to be lifted or even fail to stick; if the peeling force of the adhesive layer 40 on the surface with a water drop angle of 115° is too large, the adhesion between the adhesive layer 40 and the curved screen is too high, and the air exhaust is poor. In addition, when the protective film 100 is replaced, the adhesion between the protective film 100 and the curved screen is too large, and the curved screen is easily damaged.

[0129] Optionally, the thickness of the adhesive layer 40 ranges from 8 μm to 20 μm. Specifically, the thickness of the adhesive layer 40 may be, but is not limited to, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, etc. If the thickness of the adhesive layer 40 is too thin, the adhesive force provided by the adhesive layer 40 is different, and the protective film 100 is prone to warping and bubbles when applied to a curved screen; if the thickness of the adhesive layer 40 is too thick, since the adhesive layer 40 is relatively soft, the hardness of the protective film 100 is reduced, thereby reducing the anti-nail mark effect of the protective film 100.

[0130] Furthermore, the thickness of the adhesive layer 40 is in the range of 10 μm to 16 μm, so that the adhesive layer 40 has a good adhesive force, and at the same time the protective film 100 is kept at a high hardness, thereby improving the anti-nail mark effect of the protective film 100.

[0131] See also Figure 6 and Figure 7 In some embodiments, the protective film 100 further includes an anti-reflection layer 70 , and the anti-reflection layer 70 is located between the hardening layer 20 and the anti-fingerprint layer 50 .

[0132] Understandably, if Figure 6 As shown, when the protective film 100 does not include the intermediate processing layer 60, the anti-reflection layer 70 is located between the hardening layer 20 and the anti-fingerprint layer 50; Figure 7 As shown, when the protection film 100 includes the intermediate treatment layer 60 , the anti-reflection layer 70 is located between the hardening layer 20 and the intermediate treatment layer 60 .

[0133] See also Figure 8 Optionally, the anti-reflection layer 70 includes a first coating layer 71 and a second coating layer 72, wherein the first coating layer 71 is disposed between the hardening layer 20 and the anti-fingerprint layer 50, and the second coating layer 72 is disposed between the hardening layer 20 and the first coating layer 71, and the refractive index of the first coating layer 71 is less than the refractive index of the second coating layer 72. In this embodiment, the first coating layer 71 and the second coating layer 72 are used as the anti-reflection layer 70, which can better reduce the preparation cost of the anti-reflection layer 70, thereby reducing the preparation cost of the protective film 100.

[0134] It can be understood that the first coating layer 71 is closer to the anti-fingerprint layer 50 , and the second coating layer 72 is closer to the hardening layer 20 .

[0135] In this embodiment, by providing an anti-reflection layer 70 between the hardening layer 20 and the anti-fingerprint layer 50, the reflectivity of the protective film 100 can be better reduced and the light transmittance of the protective film 100 can be improved, so that when the protective film 100 is applied to a curved screen assembly, it can better avoid reflection and have a better appearance effect.

[0136] Optionally, the refractive index n1 of the first coating layer 71 is in the range of 1.3≤n1≤1.4. Specifically, the refractive index n1 of the first coating layer 71 may be, but is not limited to, 1.3, 1.31, 1.32, 1.33, 1.34, 1.35, 1.36, 1.37, 1.38, 1.39, 1.4, etc. If the refractive index n1 of the first coating layer 71 is too low, the material is difficult to realize; if the refractive index n1 of the first coating layer 71 is too high, the refractive index difference between the first coating layer 71 and the second coating layer 72 is too small, which is not conducive to improving the anti-reflection effect of the anti-reflection layer 70.

[0137] Optionally, the refractive index n2 of the second coating layer 72 is in the range of 1.6≤n2≤1.7. Specifically, the refractive index n2 of the second coating layer 72 may be, but is not limited to, 1.6, 1.61, 1.62, 1.63, 1.64, 1.65, 1.66, 1.67, 1.68, 1.69, 1.7, etc. If the refractive index n2 of the second coating layer 72 is too small, the refractive index difference between the first coating layer 71 and the second coating layer 72 is too small, which is not conducive to improving the anti-reflection effect of the anti-reflection layer 70; if the refractive index n2 of the second coating layer 72 is too large, the cost and difficulty of preparing the first coating layer 71 are increased, or even cannot be achieved.

[0138] Optionally, the refractive index n3 of the anti-fingerprint layer 50 is in the range of 1.36≤n3≤1.4. Specifically, the refractive index n3 of the anti-fingerprint layer 50 may be, but is not limited to, 1.36, 1.37, 1.38, 1.39, 1.4, etc. If the refractive index n3 of the anti-fingerprint layer 50 is too low, the material is difficult to realize; if the refractive index n3 of the anti-fingerprint layer 50 is too high, the difference between the refractive index of the first coating 71 and the anti-fingerprint coating is too large, which increases the interface reflection between the first coating 71 and the anti-fingerprint layer 50, which is not conducive to improving the light transmittance of the protective film 100.

[0139] Optionally, the refractive index n4 of the intermediate treatment layer 60 is in the range of 1.3≤n4≤1.4. Specifically, the refractive index n4 of the intermediate treatment layer 60 may be, but is not limited to, 1.3, 1.31, 1.32, 1.33, 1.34, 1.35, 1.36, 1.37, 1.38, 1.39, 1.4, etc. If the refractive index n4 of the intermediate treatment layer 60 is too low, the material is difficult to realize; if the refractive index n43 of the intermediate treatment layer 60 is too high, the difference between the refractive index of the first coating layer 71 and the refractive index of the intermediate treatment layer 60 is too large, which increases the interface reflection between the first coating layer 71 and the intermediate treatment layer 60, which is not conducive to improving the light transmittance of the protective film 100.

[0140] Optionally, the first coating liquid includes, by mass fraction, 20% to 50% of polyurethane acrylic resin oligomer, 5% to 20% of acrylic monomer, 1% to 3% of a third photoinitiator, 1% to 2% of a leveling agent, 1% to 20% of hollow inorganic nanoparticles, 0.5% to 1% of a defoaming agent, and the balance of a fourth solvent.

[0141] Optionally, the hollow inorganic nanoparticles may be, but are not limited to, at least one of silicon dioxide, aluminum oxide, aluminum nitride, and the like.

[0142] Optionally, the refractive index of the hollow nanoparticles is less than the refractive index of the fluorine-substituted polyurethane acrylic resin and the first acrylic resin. In this embodiment, by adding hollow inorganic nanoparticles to the first coating layer 71, the refractive index of the first coating layer 71 can be reduced, so that the first coating layer 71 and the second coating layer 72 have a large refractive index difference, so that the anti-reflection layer 70 has a better anti-reflection effect, and the light transmittance of the protective film 100 is better improved; in addition, the first coating layer 71 can also have higher wear resistance.

[0143] Optionally, the third photoinitiator may be, but is not limited to, at least one of methyl benzoylformate, TPO, ITX, BP, photoinitiator 1700, photoinitiator 784, photoinitiator 1800, photoinitiator 4265, photoinitiator 184, photoinitiator 2959, photoinitiator 1173, photoinitiator 907, photoinitiator 160, etc. Optionally, the fourth solvent may be, but is not limited to, one or more of ethyl acetate, propyl acetate, butyl acetate, cyclohexanone, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether, isopropanol, butanone, and methyl butanone. Optionally, the leveling agent may be, but is not limited to, an organosilicon leveling agent, etc. Optionally, the defoamer may be, but is not limited to, at least one of an organosilicon defoamer and a polyether defoamer.

[0144] Optionally, when applying the first coating liquid, it is diluted with a diluent (such as propylene glycol methyl ether) to a solid content of 3% to 10% before applying.

[0145] Optionally, the second coating liquid includes, by mass fraction, 30% to 70% of polyurethane acrylic resin oligomer, 2% to 12% of multifunctional acrylic monomer, 1% to 5% of a fourth photoinitiator, 1% to 3% of a leveling agent, 1% to 15% of solid inorganic nanoparticles, 0.5 to 1% of a defoaming agent, and the remainder of a fifth solvent.

[0146] Optionally, the solid inorganic nanoparticles may be, but are not limited to, at least one of silicon dioxide, zirconium oxide, aluminum oxide, titanium dioxide, calcium carbonate, aluminum nitride, and the like.

[0147] Optionally, the fourth photoinitiator may be, but is not limited to, at least one of methyl benzoylformate, TPO, ITX, BP, photoinitiator 1700, photoinitiator 784, photoinitiator 1800, photoinitiator 4265, photoinitiator 184, photoinitiator 2959, photoinitiator 1173, photoinitiator 907, photoinitiator 160, etc. Optionally, the fifth solvent may be, but is not limited to, one or more of ethyl acetate, propyl acetate, butyl acetate, cyclohexanone, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether, isopropanol, butanone, and methyl butanone. Optionally, the leveling agent may be, but is not limited to, an organosilicon leveling agent, etc. Optionally, the defoamer may be, but is not limited to, at least one of an organosilicon defoamer and a polyether defoamer.

[0148] Optionally, when the second coating liquid is applied, it is diluted with a diluent (such as propylene glycol methyl ether) to a solid content of 3% to 20% before being applied.

[0149] In some embodiments, the thickness of the first coating layer 71 ranges from 80 nm to 90 nm, and the thickness of the second coating layer 72 ranges from 90 nm to 100 nm.

[0150] Specifically, the thickness of the first coating layer 71 may be, but is not limited to, 80 nm, 81 nm, 82 nm, 83 nm, 84 nm, 85 nm, 86 nm, 87 nm, 88 nm, 89 nm, 90 nm, etc. If the thickness of the first coating layer 71 is too thin, the wear resistance of the protective film 100 is reduced and the construction difficulty is increased; if the thickness of the first coating layer 71 is too thick, the anti-reflection effect of the anti-reflection layer 70 is reduced.

[0151] Specifically, the thickness of the second coating layer 72 may be, but is not limited to, 90 nm, 91 nm, 92 nm, 93 nm, 94 nm, 95 nm, 96 nm, 97 nm, 98 nm, 99 nm, 100 nm, etc. If the thickness of the second coating layer 72 is too thin, the wear resistance of the protective film 100 is reduced and the construction difficulty is increased; if the thickness of the second coating layer 72 is too thick, the anti-reflection effect of the anti-reflection layer 70 is reduced.

[0152] See also Fig. 9 In some embodiments, the anti-reflection layer 70 includes multiple first coating films 73 and multiple second coating films 74, wherein the first coating films 73 and the second coating films 74 are alternately stacked in sequence. The first coating films 73 and the second coating films 74 have different refractive indices.

[0153] The term "multi-layer" means greater than or equal to two layers.

[0154] Optionally, the first coating film 73 is niobium oxide, and the second coating film 74 is silicon oxide.

[0155] Optionally, the thickness of the first coating film 73 is 10 nm to 40 nm, and the thickness of the second coating film 74 is 80 nm to 140 nm.

[0156] Compared with the solution using the first coating 71 and the second coating 72 , the present embodiment uses a coating as the anti-reflection layer 70 which has a better anti-reflection effect, can better improve the light transmittance of the protective film 100 , reduce the reflectivity of the protective film 100 , and can also better improve the wear resistance of the protective film 100 .

[0157] The protective film 100 of the embodiment of the present application can be prepared by the method described in the following embodiments of the present application. In addition, it can also be prepared by other methods. The preparation method of the embodiment of the present application is only one or more preparation methods of the protective film 100 of the present application and should not be understood as a limitation on the protective film 100 provided by the embodiment of the present application.

[0158] See also Fig.10 The present application also provides a method for preparing a protective film 100, which includes:

[0159] S201, providing a substrate layer 10;

[0160] Optionally, a glue solution composed of raw material components of an optical-grade process film and a substrate layer 10 is provided; the glue solution is coated on the surface of the optical-grade process film to form a glue layer; the glue solution is baked at a temperature of 80°C to 150°C for 2min to 5min; and the glue layer is irradiated for 5 seconds (s) to 15s under an electron beam curing or ultraviolet light curing device (such as a mercury lamp or an LED lamp) to obtain the substrate layer 10.

[0161] S202, forming a hardening layer 20 on one side of the base material layer 10; and

[0162] Optionally, a hardening liquid (i.e., a glue liquid composed of raw material components of the hardening layer 20) is coated on the surface of the substrate layer 10 away from the optical-grade process film, and baked at a temperature of 80°C to 150°C to remove the first solvent in the hardening liquid to form a hardening liquid layer; and irradiated under a UV curing device for 5s to 15s for photocuring to cure the hardening liquid layer to form a hardening layer 20, thereby obtaining an optical-grade process film, a substrate layer 10 and a hardening layer 20 stacked in sequence.

[0163] S203, forming an anti-fingerprint layer 50 on a side of the hardened layer 20 away from the substrate layer 10, wherein the anti-fingerprint layer 50 comprises a dual-end siloxane-based perfluoropolyether and a single-end siloxane-based perfluoropolyether; in the anti-fingerprint layer 50, a mass ratio of the dual-end siloxane-based perfluoropolyether to the single-end siloxane-based perfluoropolyether is in a range of 2 / 3 to 4.

[0164] Optionally, an anti-fingerprint coating liquid is applied on the side of the hardening layer 20 facing away from the substrate layer 10 by spraying or coating, and then dried to form the anti-fingerprint layer 50 .

[0165] For detailed description of other aspects such as the substrate layer 10 , the hardening layer 20 and the anti-fingerprint layer 50 , please refer to the description of the corresponding parts of the above embodiments, which will not be repeated here.

[0166] The protective film 100 prepared by the preparation method of the protective film 100 of the embodiment of the present application includes a substrate layer 10, a hardening layer 20 and an anti-fingerprint layer 50. The raw material components of the anti-fingerprint layer 50 include a double-ended siloxane-based perfluoropolyether and a single-ended siloxane-based perfluoropolyether; in the raw material components of the anti-fingerprint layer 50, the mass ratio of the double-ended siloxane-based perfluoropolyether and the single-ended siloxane-based perfluoropolyether is in the range of 2 / 3 to 4. In this embodiment, by designing the raw material components of the anti-fingerprint layer 50, the anti-fingerprint layer 50 has a higher fluorine content, a lower surface energy and a higher initial water drop angle, so as to have a better anti-fouling effect and anti-fingerprint effect. In addition, the anti-fingerprint layer 50 can form a stable chemical bond with the hardening layer 20, so that the anti-fingerprint layer 50 has better bonding with the hardening layer 20, so that the anti-fingerprint layer 50 has a longer service life and is not easy to wear off or fall off after long-term use.

[0167] See also Fig.11 The present application also provides a method for preparing a protective film 100, which includes:

[0168] S301, providing a substrate layer 10;

[0169] S302, forming a hardening layer 20 on one side of the base material layer 10;

[0170] For a detailed description of S301 to S302, please refer to the description of the corresponding part of the above embodiment, which will not be repeated here.

[0171] S303, performing surface treatment on the hardened layer 20 so that the water drop angle of the hardened layer 20 away from the surface of the substrate layer 10 is in a range of 10° to 40°; and

[0172] Optionally, the surface of the hardened layer 20 facing away from the substrate layer 10 is treated by corona or plasma treatment, so that the water drop angle of the surface of the hardened layer 20 facing away from the substrate layer 10 is in the range of 10° to 40°.

[0173] Specifically, the water drop angle of the surface of the hardened layer 20 away from the substrate layer 10 can be, but is not limited to, 10°, 15°, 20°, 25°, 30°, 35°, 40°, etc.

[0174] In the present embodiment, by performing corona or plasma treatment on the surface of the hardened layer 20, active groups such as -OH, -COOH, etc. can be formed on the surface of the hardened layer 20, which can reduce the water drop angle of the surface of the hardened layer 20, improve the hydrophilicity of the surface of the hardened layer 20, and thus improve the bonding force between the hardened layer 20 and the intermediate treatment layer 60 or the anti-fingerprint layer 50; when the water drop angle of the hardened layer 20 away from the surface of the substrate layer 10 is too small, the current plasma or corona technology is difficult to implement, and if the plasma or corona effect is too strong, it is easy to destroy the main molecular structure of the hardened layer 20; when the water drop angle of the hardened layer 20 away from the surface of the substrate layer 10 is too large, the content of active groups such as -OH, -COOH, etc. formed on the surface of the hardened layer 20 is too low, and the adhesion between the hardened layer 20 and the anti-fingerprint layer 50 or the intermediate treatment layer 60 is low.

[0175] S304, forming an anti-fingerprint layer 50 on a side of the hardened layer 20 away from the substrate layer 10, wherein the anti-fingerprint layer 50 includes a dual-end siloxane-based perfluoropolyether and a single-end siloxane-based perfluoropolyether; in the anti-fingerprint layer 50, a mass ratio of the dual-end siloxane-based perfluoropolyether to the single-end siloxane-based perfluoropolyether is in a range of 2 / 3 to 4.

[0176] For a detailed description of S304, please refer to the description of the corresponding part of the above embodiment, which will not be repeated here.

[0177] See also Fig.12 The present application also provides a method for preparing a protective film 100, which includes:

[0178] S401, providing a substrate layer 10;

[0179] S402, forming a hardening layer 20 on one side of the base material layer 10;

[0180] S403, performing surface treatment on the hardened layer 20 so that the water drop angle of the hardened layer 20 away from the surface of the substrate layer 10 is in a range of 10° to 40°;

[0181] For a detailed description of S401 to S403, please refer to the description of the corresponding parts of the above embodiment, which will not be repeated here.

[0182] S404, forming an intermediate treatment layer 60 on the surface of the hardened layer 20 away from the substrate layer 10;

[0183] Optionally, a treatment liquid is coated on the surface of the hardened layer 20 facing away from the base layer 10 , and dried to form the intermediate treatment layer 60 .

[0184] S405, forming an anti-fingerprint layer 50 on a side of the intermediate treatment layer 60 away from the substrate layer 10, wherein the anti-fingerprint layer 50 comprises a bi-terminal siloxane-based perfluoropolyether and a mono-terminal siloxane-based perfluoropolyether; in the anti-fingerprint layer 50, a mass ratio of the bi-terminal siloxane-based perfluoropolyether to the mono-terminal siloxane-based perfluoropolyether is in a range of 2 / 3 to 4;

[0185] For a detailed description of S405, please refer to the description of the corresponding part of the above embodiment, which will not be repeated here.

[0186] S406, forming a shaping layer 30 on a side of the base material layer 10 away from the hardening layer 20; and

[0187] Optionally, the optical-grade process film is torn off, and a setting liquid is coated on the surface of the substrate layer 10 away from the hardening layer 20 to form a setting liquid glue layer; and the setting liquid glue layer is baked at a high temperature of 80° C. to 150° C. for 2 min to 5 min to thermally cure the setting liquid glue layer to form a setting layer 30.

[0188] S407 , forming an adhesive layer 40 on a side of the shaping layer 30 away from the substrate layer 10 .

[0189] Optionally, an adhesive is coated on the surface of the shaping layer 30 facing away from the substrate, and baked at a temperature of 120° C. to 150° C. for 1 min to 5 min to cure the adhesive to form the adhesive layer 40 .

[0190] See also Fig.13 The present application also provides a method for preparing a protective film 100, which includes:

[0191] S501, providing a substrate layer 10;

[0192] S502, forming a hardening layer 20 on one side of the base material layer 10;

[0193] S503, performing surface treatment on the hardened layer 20 so that the water drop angle of the hardened layer 20 away from the surface of the substrate layer 10 is in a range of 10° to 40°;

[0194] For a detailed description of S501 to S503, please refer to the description of the corresponding parts of the above embodiment, which will not be repeated here.

[0195] S504, forming a second coating layer 72 on the surface of the hardened layer 20 away from the substrate layer 10;

[0196] Optionally, a second coating liquid is coated on the surface of the hardening layer 20 facing away from the substrate layer 10 , and is irradiated with ultraviolet light to cure and form a second coating layer 72 .

[0197] S505, forming a first coating layer 71 on the surface of the second coating layer 72 away from the substrate layer 10, and performing surface treatment on the first coating layer 71 so that a water drop angle of the surface of the first coating layer 71 away from the second coating layer 72 is in a range of 10° to 40°;

[0198] Optionally, the first coating liquid is coated on the surface of the second coating layer 72 facing away from the substrate layer 10 , and irradiated with ultraviolet light to cure to form the first coating layer 71 .

[0199] S506, forming an anti-fingerprint layer 50 on a side of the first coating layer 71 away from the second coating layer 72;

[0200] For a detailed description of S506, please refer to the description of the corresponding part of the above embodiment, which will not be repeated here.

[0201] S507, forming a shaping layer 30 on a side of the base material layer 10 away from the hardening layer 20; and

[0202] S508 , forming an adhesive layer 40 on a side of the shaping layer 30 away from the substrate layer 10 .

[0203] For a detailed description of S506 to S508, please refer to the description of the corresponding parts of the above embodiment, which will not be repeated here.

[0204] See also Fig.14 The present application also provides a method for preparing a protective film 100, which includes:

[0205] S601, providing a substrate layer 10;

[0206] S602, forming a hardening layer 20 on one side of the base material layer 10;

[0207] S603, performing surface treatment on the hardened layer 20 so that the water drop angle of the hardened layer 20 away from the surface of the substrate layer 10 is in a range of 10° to 40°;

[0208] S604, forming a second coating layer 72 on the surface of the hardened layer 20 away from the substrate layer 10;

[0209] S605, forming a first coating layer 71 on the surface of the second coating layer 72 away from the substrate layer 10, and performing surface treatment on the first coating layer 71 so that a water drop angle of the surface of the first coating layer 71 away from the second coating layer 72 is in a range of 10° to 40°;

[0210] Optionally, the surface of the first coating 71 facing away from the second coating 72 is treated by corona or plasma treatment, so that the water drop angle of the surface of the first coating 71 facing away from the second coating 72 is in the range of 10° to 40°.

[0211] Specifically, the water drop angle of the surface of the first coating 71 away from the second coating 72 can be, but is not limited to, 10°, 15°, 20°, 25°, 30°, 35°, 40°, etc.

[0212] In this embodiment, by performing corona or plasma treatment on the surface of the first coating 71, active groups such as -OH, -COOH, etc. can be formed on the surface of the first coating 71, which can reduce the water drop angle of the surface of the first coating 71, improve the hydrophilicity of the surface of the first coating 71, and thus improve the bonding force between the first coating 71 and the intermediate treatment layer 60 or the anti-fingerprint layer 50; when the water drop angle of the first coating 71 away from the surface of the second coating 72 is too small, the current plasma or corona technology is difficult to implement, and if the plasma or corona effect is too strong, it is easy to destroy the main molecular structure of the first coating 71; when the water drop angle of the first coating 71 away from the second coating 72 is too large, the content of active groups such as -OH, -COOH, etc. formed on the surface of the first coating 71 is too low, and the adhesion between the first coating 71 and the anti-fingerprint layer 50 or the intermediate treatment layer 60 is low.

[0213] S606, forming an intermediate treatment layer 60 on the surface of the first coating layer 71 away from the substrate layer 10;

[0214] Optionally, a treatment liquid is coated on the surface of the hardened layer 20 facing away from the base layer 10 , and dried to form the intermediate treatment layer 60 .

[0215] S607, forming an anti-fingerprint layer 50 on a side of the intermediate processing layer 60 away from the substrate layer 10;

[0216] S608, forming a shaping layer 30 on a side of the substrate layer 10 away from the hardening layer 20; and

[0217] S609 , forming an adhesive layer 40 on a side of the shaping layer 30 away from the substrate layer 10 .

[0218] For a detailed description of S601 to S609 , please refer to the description of the corresponding parts of the above embodiment, which will not be repeated here.

[0219] See also Fig.15 The present application also provides a method for preparing a protective film 100, which includes:

[0220] S701, providing a substrate layer 10;

[0221] S702, forming a hardening layer 20 on one side of the base material layer 10;

[0222] S703, performing surface treatment on the hardened layer 20 so that the water drop angle of the hardened layer 20 away from the surface of the substrate layer 10 is in a range of 10° to 40°;

[0223] S704 , a first coating film 73 and a second coating film 74 are alternately coated on the surface of the hardening layer 20 away from the substrate layer 10 in sequence to obtain an anti-reflection layer 70 .

[0224] Optionally, by evaporation, the first coating film 73 and the second coating film 74 are alternately coated in sequence on the surface of the hardening layer 20 away from the substrate layer 10 .

[0225] S705, forming an anti-fingerprint layer 50 on a side of the anti-reflection layer 70 away from the hardening layer 20;

[0226] S706, forming a shaping layer 30 on a side of the substrate layer 10 away from the hardening layer 20; and

[0227] S707 , forming an adhesive layer 40 on a side of the shaping layer 30 away from the base material layer 10 .

[0228] For a detailed description of S701 to S707, please refer to the description of the corresponding parts of the above embodiment, which will not be repeated here.

[0229] See also Figures 16 to 18 The embodiment of the present application also provides a curved screen assembly 200, which includes: a curved screen 210 and the protective film 100 described in the embodiment of the present application. The curved screen 210 has a display surface 211; the protective film 100 is disposed on the display surface 211, between the substrate layer 10, the hardening layer 20 and the curved screen 210.

[0230] For a detailed description of the protective film 100 , please refer to the description of the corresponding part of the above embodiment, which will not be repeated here.

[0231] It can be understood that the substrate layer 10 is closer to the curved screen 210 than the hardening layer 20. The protective film 100 is bonded to the curved screen 210 via the adhesive layer 40.

[0232] It can be understood that in the present embodiment, the protective film 100 is a 3D protective film, and the shaping layer 30 of the protective film 100 is a shaping layer 30 that has been thermally cured and photocured.

[0233] It can be understood that after the protective film 100 is prepared and before being attached to the curved screen 210, the protective film 100 is a flat structure. When the protective film 100 is applied to the curved screen assembly 200 and attached to the curved screen 210, the adhesive layer 40 of the protective film 100 is adhered to the display surface 211 of the curved screen 210, and the protective film 100 is pressed so that the protective film 100 is completely attached to the curved screen 210; then the protective film 100 is illuminated to further photo-cure the shaping layer 30 of the protective film 100, thereby shaping the protective film 100 to form a 3D protective film 100, so that the protective film 100 matches the shape of the curved screen 210 and is tightly attached to the surface of the curved screen 210.

[0234] Optionally, the curved screen 210 may be curved on two relatively long sides, or on two relatively short sides, or on all four sides. The drawings of the present application are only one of the various forms of the curved screen 210, and should not be construed as limiting the curved screen 210 of the embodiment of the present application, nor should they be construed as limiting the protective film 100 of the present application.

[0235] Optionally, the energy range of the light curing of the shaping layer 30 is 6000 mj / cm 2 Up to 12000mj / cm 2 Specifically, the energy of the light curing of the shaping layer 30 may be, but is not limited to, 6000 mj / cm 2 、7000mj / cm 2 、8000mj / cm 2 、9000mj / cm 2 、10000mj / cm 2 、11000mj / cm 2 、12000mj / cm 2 In this embodiment, if the energy of the light curing of the shaping layer 30 is too low, the shaping layer 30 is not completely cured, the generated shaping force is insufficient, the shaping effect is affected, and the hardness of the shaping layer 30 is insufficient, which affects the anti-nail mark effect of the shaping layer 30; if the energy of the light curing of the shaping layer 30 is too high, the degree of curing of the shaping layer 30 is too high, and after curing, the volume shrinks too much, the internal stress is too large, and the force resisting the bonding force direction is too large, so that the protective film 100 is easy to warp.

[0236] Optionally, the curved screen 210 may be, but is not limited to, one or more of a liquid crystal display, a light emitting diode display (LED display), a micro light emitting diode display (Micro LED display), a sub-millimeter light emitting diode display (Mini LED display), an organic light emitting diode display (OLED display), etc.

[0237] See also Figures 19 to 22The embodiment of the present application also provides an electronic device 300, which includes: the curved screen assembly 200 described in the embodiment of the present application and a processor 310, wherein the processor 310 is electrically connected to the curved screen assembly 200 and is used to control the curved screen assembly 200 to display.

[0238] For a detailed description of the curved screen assembly 200, please refer to the description of the corresponding part of the above embodiment, which will not be repeated here.

[0239] The electronic device 300 of the embodiment of the present application may be, but is not limited to, a mobile phone, a tablet computer, a laptop computer, a desktop computer, a smart bracelet, a smart watch, an e-reader, a game console, and other portable electronic devices 300. It can be understood that the electronic device 300 described in this embodiment is only one form of the electronic device 300 applied by the curved screen assembly 200, and should not be understood as a limitation on the electronic device 300 provided in the present application, nor should it be understood as a limitation on the curved screen assembly 200 provided in each embodiment of the present application.

[0240] Optionally, the processor 310 includes one or more general-purpose processors, wherein the general-purpose processor can be any type of device capable of processing electronic instructions, including a central processing unit (CPU), a microprocessor, a microcontroller, a main processor, a controller, and an ASIC, etc. The processor 310 is used to execute various types of digital storage instructions, such as software or firmware programs stored in a memory, which enables the computing device to provide a wide variety of services.

[0241] Optionally, the electronic device 300 of the present application further includes a memory 320. The memory 320 is electrically connected to the processor 310 and is used to store program codes required for the processor 310 to run, program codes required for controlling the curved screen 210, display content of the curved screen 210, and the like.

[0242] Optionally, the memory 320 may include a volatile memory (Volatile Memory), such as a random access memory (Random Access Memory, RAM); the memory 320 may also include a non-volatile memory (NVM), such as a read-only memory (Read-Only Memory, ROM), a flash memory (Flash Memory, FM), a hard disk drive (Hard Disk Drive, HDD) or a solid-state drive (SSD). The memory 320 may also include a combination of the above-mentioned types of memory.

[0243] In some embodiments, the electronic device 300 of the embodiment of the present application further includes a housing 330, a middle frame 340 and a camera module 350, wherein the housing 330 is disposed opposite to the curved screen assembly 200, the middle frame 340 is disposed between the curved screen assembly 200 and the housing 330, and the side of the middle frame 340 is exposed to the housing 330 and the curved screen assembly 200. The middle frame 340 and the housing 330 enclose a housing space (not shown), and the housing space is used to accommodate the processor 310, the memory 320 and the camera module 350. The camera module 350 is electrically connected to the processor 310 for shooting under the control of the processor 310.

[0244] Optionally, the housing 330 has a light-transmitting portion (not shown), and the camera module 350 can shoot through the light-transmitting portion on the housing 330, that is, the camera module 350 in this embodiment is a rear camera module 350. It can be understood that in other embodiments, the light-transmitting portion can be provided on the curved screen assembly 200, that is, the camera module 350 is a front camera module 350. In the schematic diagram of this embodiment, the light-transmitting portion is illustrated as an opening. In other embodiments, the light-transmitting portion may not be an opening, but a light-transmitting material, such as plastic, glass, etc.

[0245] The protective film 100 of the embodiment of the present application is further described below through specific examples.

[0246] Example 1

[0247] The protective film 100 of this embodiment is prepared by the following steps:

[0248] (1) Preparing the substrate layer 10: coating the polyurethane adhesive on the surface of the optical-grade process film, baking at 100° C. for 3 minutes, and irradiating the film under an electron beam curing device for 10 seconds to obtain the thermoplastic polyurethane substrate layer 10;

[0249] The thickness of the substrate layer 10 is 20 μm; the elastic modulus of the substrate layer 10 is 2 GPa, the tensile strength of the substrate layer 10 is 50 MPa, and the elongation at break of the substrate layer 10 is 2%.

[0250] (2) coating the surface of the substrate layer 10 with a hardening liquid, and baking at a temperature of 120° C. for 3 minutes to dry out the solvent; then irradiating the surface with a UV curing device for 10 seconds to cure the hardening liquid to form a hardened layer 20;

[0251] The thickness of the hardened layer 20 is 3 μm; the hardening liquid includes, by mass fraction, 20% of a polyurethane acrylic resin prepolymer, 10% of a hyperbranched acrylic resin (with an octagonal ring in the middle, i.e., the acrylic resin molecule includes eight branches), 5% of ethoxylated trimethylolpropane triacrylate (a first reaction monomer), 3% of methyl benzoylformate (a first photoinitiator), 5% of a double-bond terminated perfluoropolyether (a short-chain fluoride) with a weight average molecular weight of 3000, 5% of an aluminum oxide (inorganic particles) with an average particle size of 20 nm, and 52% of propylene glycol methyl ether (a first solvent);

[0252] (3) performing corona treatment on the surface of the hardened layer 20 facing away from the substrate layer 10 so that the water drop angle of the surface of the hardened layer 20 facing away from the substrate layer 10 is 10°;

[0253] (4) applying the treatment liquid to the surface of the hardened layer 20 away from the substrate layer 10 and drying it to form the intermediate treatment layer 60;

[0254] The thickness of the intermediate treatment layer 60 is 10 nm, and the treatment solution includes 40% 2-chloroethylmethyldimethoxysilane (silane coupling agent), 1% silicon dioxide (inorganic nanoparticles) and 59% ethyl acetate;

[0255] (5) applying the anti-fingerprint coating liquid to the surface of the intermediate treatment layer 60 facing away from the substrate layer 10, and drying to form the anti-fingerprint layer 50;

[0256] The anti-fingerprint layer 50 has a thickness of 20 nm, and the anti-fingerprint coating liquid includes 5% of a double-ended siloxane perfluoropolyether with a number average molecular weight of 8000, 5% of a single-ended siloxane perfluoropolyether with a number average molecular weight of 1000, 84% of tetrafluoroethyl ether (fluoroether solvent), 1% of lauryl alcohol (hydrolysis promoter), and 5% of an auxiliary agent;

[0257] (6) removing the optical-grade process film, applying a setting liquid on the surface of the substrate layer 10 away from the hardening layer 20, and baking at a temperature of 120° C. for 3 minutes to perform thermal curing to form a setting layer 30; and

[0258] The thickness of the setting layer 30 is 75 μm; the setting liquid comprises a first raw material component and a second raw material component, and the mass ratio of the first raw material component to the second raw material component is 5; the first raw material component comprises 50% of a polyurethane acrylate prepolymer with a weight average molecular weight of 10,000, 15% of diphenylmethane diisocyanate (a second reactive monomer), 5% of succinic anhydride (a curing agent), 3% of a photoinitiator 184, 0.5% of 2-chloroethylmethyldimethoxysilane (a first coupling agent), and 26.5% of ethyl acetate (a second solvent); the second raw material component comprises 50% of hydroxyethyl methacrylate (an acrylic monomer), 0.5% of 3-isocyanatepropyltrimethoxysilane (a second coupling agent), 3% of poly(melamine-co-formaldehyde) methanol (a film-forming agent), and 46.5% of methylal (a third solvent);

[0259] (7) coating a silicone adhesive on the surface of the shaping layer 30 facing away from the substrate layer 10, and baking at a temperature of 150° C. for 2 minutes to form an adhesive layer 40;

[0260] The thickness of the adhesive layer 40 is 10 μm.

[0261] Example 2

[0262] The protective film 100 of this embodiment is prepared by the following steps:

[0263] (1) Preparing the substrate layer 10: coating the polyurethane adhesive on the surface of the optical-grade process film, baking at 100° C. for 3 minutes, and irradiating the film under an electron beam curing device for 10 seconds to obtain the thermoplastic polyurethane substrate layer 10;

[0264] The thickness of the substrate layer 10 is 20 μm; the elastic modulus of the substrate layer 10 is 2 GPa, the tensile strength of the substrate layer 10 is 50 MPa, and the elongation at break of the substrate layer 10 is 2%.

[0265] (2) coating the surface of the substrate layer 10 with a hardening liquid, and baking at a temperature of 120° C. for 3 minutes to dry out the solvent; then irradiating the surface with a UV curing device for 10 seconds to cure the hardening liquid to form a hardened layer 20;

[0266] The thickness of the hardened layer 20 is 3 μm; the hardening liquid includes, by mass fraction, 20% of a polyurethane acrylic resin prepolymer, 10% of a hyperbranched acrylic resin (with an octagonal ring in the middle, i.e., the acrylic resin molecule includes eight branches), 5% of ethoxylated trimethylolpropane triacrylate (a first reaction monomer), 3% of methyl benzoylformate (a first photoinitiator), 5% of a double-bond terminated perfluoropolyether (a short-chain fluoride) with a weight average molecular weight of 3000, 5% of an aluminum oxide (inorganic particles) with an average particle size of 20 nm, and 52% of propylene glycol methyl ether (a first solvent);

[0267] (3) performing corona treatment on the surface of the hardened layer 20 facing away from the substrate layer 10 so that the water drop angle of the surface of the hardened layer 20 facing away from the substrate layer 10 is 10°;

[0268] (4) applying the anti-fingerprint coating liquid to the surface of the hardened layer 20 facing away from the substrate layer 10, and drying to form the anti-fingerprint layer 50;

[0269] The anti-fingerprint layer 50 has a thickness of 20 nm, and the anti-fingerprint coating liquid includes 20% of a bi-terminal siloxane perfluoropolyether with a number average molecular weight of 6000, 30% of a mono-terminal siloxane perfluoropolyether with a number average molecular weight of 3000, 48% of tetrafluoroethyl ether (fluoroether solvent), 1% of lauryl alcohol (hydrolysis promoter), and 1% of an auxiliary agent;

[0270] (5) removing the optical-grade process film, applying a setting liquid on the surface of the substrate layer 10 away from the hardening layer 20, and baking at a temperature of 120° C. for 3 minutes to perform thermal curing to form a setting layer 30; and

[0271] The thickness of the setting layer 30 is 75 μm; the setting liquid comprises a first raw material component and a second raw material component, and the mass ratio of the first raw material component to the second raw material component is 5; the first raw material component comprises 50% of a polyurethane acrylate prepolymer with a weight average molecular weight of 10,000, 15% of diphenylmethane diisocyanate (a second reactive monomer), 5% of succinic anhydride (a curing agent), 3% of a photoinitiator 184, 0.5% of 2-chloroethylmethyldimethoxysilane (a first coupling agent), and 26.5% of ethyl acetate (a second solvent); the second raw material component comprises 50% of hydroxyethyl methacrylate (an acrylic monomer), 0.5% of 3-isocyanatepropyltrimethoxysilane (a second coupling agent), 3% of poly(melamine-co-formaldehyde) methanol (a film-forming agent), and 46.5% of methylal (a third solvent);

[0272] (6) coating a silicone adhesive on the surface of the shaping layer 30 facing away from the substrate layer 10, and baking at a temperature of 150° C. for 2 minutes to form an adhesive layer 40;

[0273] The thickness of the adhesive layer 40 is 10 μm.

[0274] Example 3

[0275] The protective film 100 of this embodiment is prepared by the following steps:

[0276] (1) Preparing the substrate layer 10: coating the polyurethane adhesive on the surface of the optical-grade process film, baking at 100° C. for 3 minutes, and irradiating the film under an electron beam curing device for 10 seconds to obtain the thermoplastic polyurethane substrate layer 10;

[0277] The thickness of the substrate layer 10 is 20 μm; the elastic modulus of the substrate layer 10 is 2 GPa, the tensile strength of the substrate layer 10 is 50 MPa, and the elongation at break of the substrate layer 10 is 2%.

[0278] (2) coating the surface of the substrate layer 10 with a hardening liquid, and baking at a temperature of 120° C. for 3 minutes to dry out the solvent; then irradiating the surface with a UV curing device for 10 seconds to cure the hardening liquid to form a hardened layer 20;

[0279] The thickness of the hardened layer 20 is 3 μm; the hardening liquid includes, by mass fraction, 20% of a polyurethane acrylic resin prepolymer, 10% of a hyperbranched acrylic resin (with an octagonal ring in the middle, i.e., the acrylic resin molecule includes eight branches), 5% of ethoxylated trimethylolpropane triacrylate (a first reaction monomer), 3% of methyl benzoylformate (a first photoinitiator), 5% of a double-bond terminated perfluoropolyether (a short-chain fluoride) with a weight average molecular weight of 3000, 5% of an aluminum oxide (inorganic particles) with an average particle size of 20 nm, and 52% of propylene glycol methyl ether (a first solvent);

[0280] (3) performing corona treatment on the surface of the hardened layer 20 facing away from the substrate layer 10 so that the water drop angle of the surface of the hardened layer 20 facing away from the substrate layer 10 is 10°;

[0281] (4) spraying the treatment liquid onto the surface of the hardened layer 20 away from the substrate layer 10 and drying it to form an intermediate treatment layer 60;

[0282] The thickness of the intermediate treatment layer 60 is 80 nm, and the treatment solution includes 40% 2-chloroethylmethyldimethoxysilane (silane coupling agent), 1% silicon dioxide (inorganic nanoparticles) and 59% ethyl acetate;

[0283] (5) spraying the anti-fingerprint coating liquid onto the surface of the intermediate treatment layer 60 facing away from the substrate layer 10, and drying to form the anti-fingerprint layer 50;

[0284] The thickness of the anti-fingerprint layer 50 is 120 nm, and the anti-fingerprint coating liquid includes 5% of a double-ended siloxane perfluoropolyether with a number average molecular weight of 8000, 5% of a single-ended siloxane perfluoropolyether with a number average molecular weight of 1000, 84% of tetrafluoroethyl ether (fluoroether solvent), 1% of lauryl alcohol (hydrolysis promoter), and 5% of an auxiliary agent;

[0285] (6) removing the optical-grade process film, applying a setting liquid on the surface of the substrate layer 10 away from the hardening layer 20, and baking at a temperature of 120° C. for 3 minutes to perform thermal curing to form a setting layer 30; and

[0286] The thickness of the setting layer 30 is 75 μm; the setting liquid comprises a first raw material component and a second raw material component, and the mass ratio of the first raw material component to the second raw material component is 5; the first raw material component comprises 50% of a polyurethane acrylate prepolymer with a weight average molecular weight of 10,000, 15% of diphenylmethane diisocyanate (a second reactive monomer), 5% of succinic anhydride (a curing agent), 3% of a photoinitiator 184, 0.5% of 2-chloroethylmethyldimethoxysilane (a first coupling agent), and 26.5% of ethyl acetate (a second solvent); the second raw material component comprises 50% of hydroxyethyl methacrylate (an acrylic monomer), 0.5% of 3-isocyanatepropyltrimethoxysilane (a second coupling agent), 3% of poly(melamine-co-formaldehyde) methanol (a film-forming agent), and 46.5% of methylal (a third solvent);

[0287] (7) coating a silicone adhesive on the surface of the shaping layer 30 facing away from the substrate layer 10, and baking at a temperature of 150° C. for 2 minutes to form an adhesive layer 40;

[0288] The thickness of the adhesive layer 40 is 10 μm.

[0289] Example 4

[0290] The protective film 100 of this embodiment is prepared by the following steps:

[0291] (1) Preparing the substrate layer 10: coating the polyurethane adhesive on the surface of the optical-grade process film, baking at 100° C. for 3 minutes, and irradiating the film under an electron beam curing device for 10 seconds to obtain the thermoplastic polyurethane substrate layer 10;

[0292] The thickness of the substrate layer 10 is 20 μm; the elastic modulus of the substrate layer 10 is 2 GPa, the tensile strength of the substrate layer 10 is 50 MPa, and the elongation at break of the substrate layer 10 is 2%.

[0293] (2) coating the surface of the substrate layer 10 with a hardening liquid, and baking at a temperature of 120° C. for 3 minutes to dry out the solvent; then irradiating the surface with a UV curing device for 10 seconds to cure the hardening liquid to form a hardened layer 20;

[0294] The thickness of the hardened layer 20 is 3 μm; the hardening liquid includes, by mass fraction, 20% of a polyurethane acrylic resin prepolymer, 10% of a hyperbranched acrylic resin (with an octagonal ring in the middle, i.e., the acrylic resin molecule includes eight branches), 5% of ethoxylated trimethylolpropane triacrylate (a first reaction monomer), 3% of methyl benzoylformate (a first photoinitiator), 5% of a double-bond terminated perfluoropolyether (a short-chain fluoride) with a weight average molecular weight of 3000, 5% of an aluminum oxide (inorganic particles) with an average particle size of 20 nm, and 52% of propylene glycol methyl ether (a first solvent);

[0295] (3) performing corona treatment on the surface of the hardened layer 20 facing away from the substrate layer 10 so that the water drop angle of the surface of the hardened layer 20 facing away from the substrate layer 10 is 10°;

[0296] (4) spraying the anti-fingerprint coating liquid onto the surface of the hardened layer 20 facing away from the substrate layer 10, and drying to form the anti-fingerprint layer 50;

[0297] The thickness of the anti-fingerprint layer 50 is 120 nm, and the anti-fingerprint coating liquid includes 5% of a double-ended siloxane perfluoropolyether with a number average molecular weight of 8000, 5% of a single-ended siloxane perfluoropolyether with a number average molecular weight of 1000, 84% of tetrafluoroethyl ether (fluoroether solvent), 1% of lauryl alcohol (hydrolysis promoter), and 5% of an auxiliary agent;

[0298] (5) removing the optical-grade process film, applying a setting liquid on the surface of the substrate layer 10 away from the hardening layer 20, and baking at a temperature of 120° C. for 3 minutes to perform thermal curing to form a setting layer 30; and

[0299] The thickness of the setting layer 30 is 75 μm; the setting liquid comprises a first raw material component and a second raw material component, and the mass ratio of the first raw material component to the second raw material component is 5; the first raw material component comprises 50% of a polyurethane acrylate prepolymer with a weight average molecular weight of 10,000, 15% of diphenylmethane diisocyanate (a second reactive monomer), 5% of succinic anhydride (a curing agent), 3% of a photoinitiator 184, 0.5% of 2-chloroethylmethyldimethoxysilane (a first coupling agent), and 26.5% of ethyl acetate (a second solvent); the second raw material component comprises 50% of hydroxyethyl methacrylate (an acrylic monomer), 0.5% of 3-isocyanatepropyltrimethoxysilane (a second coupling agent), 3% of poly(melamine-co-formaldehyde) methanol (a film-forming agent), and 46.5% of methylal (a third solvent);

[0300] (6) coating a silicone adhesive on the surface of the shaping layer 30 facing away from the substrate layer 10, and baking at a temperature of 150° C. for 2 minutes to form an adhesive layer 40;

[0301] The thickness of the adhesive layer 40 is 10 μm.

[0302] Example 5

[0303] The difference between this embodiment and embodiment 2 is that the anti-fingerprint coating liquid of this embodiment includes 25% of a double-ended siloxane perfluoropolyether with a number average molecular weight of 6000, 25% of a single-ended siloxane perfluoropolyether with a number average molecular weight of 3000, 48% of tetrafluoroethyl ether (fluoroether solvent), 1% of lauryl alcohol (hydrolysis promoter), and 1% of an auxiliary agent.

[0304] Example 6

[0305] The difference between this embodiment and embodiment 2 is that the anti-fingerprint coating liquid of this embodiment includes 33.3% of a double-ended siloxane perfluoropolyether with a number average molecular weight of 6000, 16.7% of a single-ended siloxane perfluoropolyether with a number average molecular weight of 3000, 48% of tetrafluoroethyl ether (fluoroether solvent), 1% of lauryl alcohol (hydrolysis promoter), and 1% of an auxiliary agent.

[0306] Example 7

[0307] The difference between this embodiment and embodiment 2 is that the anti-fingerprint coating liquid of this embodiment includes 37.5% of a double-ended siloxane perfluoropolyether with a number average molecular weight of 6000, 12.5% ​​of a single-ended siloxane perfluoropolyether with a number average molecular weight of 3000, 48% of tetrafluoroethyl ether (fluoroether solvent), 1% of lauryl alcohol (hydrolysis promoter), and 1% of an auxiliary agent.

[0308] Example 8

[0309] The difference between this embodiment and embodiment 2 is that the anti-fingerprint coating liquid of this embodiment includes 40% of a double-ended siloxane perfluoropolyether with a number average molecular weight of 6000, 10% of a single-ended siloxane perfluoropolyether with a number average molecular weight of 3000, 48% of tetrafluoroethyl ether (fluoroether solvent), 1% of lauryl alcohol (hydrolysis promoter), and 1% of an auxiliary agent.

[0310] Comparative Example 1

[0311] The difference between this comparative example and Example 2 is that the anti-fingerprint coating liquid of this example includes 50% of bi-terminal siloxane perfluoropolyether with a number average molecular weight of 6000, 48% of tetrafluoroethyl ether (fluoroether solvent), 1% of lauryl alcohol (hydrolysis promoter), and 1% of auxiliary agent.

[0312] Comparative Example 2

[0313] The difference between this comparative example and Example 2 is that the anti-fingerprint coating liquid of this example includes 50% of single-end siloxane perfluoropolyether with a number average molecular weight of 3000, 48% of tetrafluoroethyl ether (fluoroether solvent), 1% of lauryl alcohol (hydrolysis promoter), and 1% of auxiliary agent.

[0314] The protective film 100 prepared in each embodiment is attached to the display surface 211 of the curved screen 210 or the curved screen 210 of the electronic device 300, and the adhesive layer 40 is located between the curved screen 210 and the hardening layer 20; ultraviolet light is irradiated to make the shaping layer 30 photocured, and the protective film 100 is shaped into a 3D structure, wherein the energy of the photocuring of the shaping layer 30 is 10000 mj / cm 2 According to the test, after the shaping layer 30 is thermally cured and light-cured, the peeling force of the adhesive layer 40 on the curved screen 210 with a water drop angle of 115° is 30 gf / 25 mm.

[0315] The test method of the peeling force of the adhesive layer 40 on the curved screen 210 with a water drop angle of 115° is as follows: 1) the sample to be tested (protective film 200) is made into specifications: 25 mm in width and the length is the length of the sample body to be tested, and is pasted on the test steel plate & test anti-fingerprint screen (abbreviated as AF screen, the AF screen used for testing requires a water drop angle ≥ 115°), ensuring that one end is aligned and parallel to the steel plate / AF screen; 2) A 2Kg weight is used to roll the sample to be tested back and forth three times at a speed of about 120mm / s under its own weight, and placed at room temperature for 20 minutes; 3) The free end of the sample to be tested is folded back 180°, and the adhesive surface is peeled off by about 20mm. The sample to be tested is clamped on the lower clamp, and the free end is extended (if the length of the sample to be tested is not enough, TESA 7475 tape can be used as the extension end) and is adhered to the metal straightening plate and clamped on the upper clamp. The peeling surface should be kept consistent with the force line of the testing machine; 4) Select a 5KG range sensor and set the experimental parameters: peeling speed 300mm / min; 5) Click to execute the test to obtain the peeling curve.

[0316] The curved screen 210 with the protective film 100 is subjected to various performance tests:

[0317] (1) Abrasion resistance test: Use 0000# steel wool with a weight of 1 kg to rub the exterior surface of the protective film 100 (i.e., the surface of the hardened layer 20) back and forth. After rubbing back and forth for a preset number of times, measure the water drop angle on the surface of the protective film 100.

[0318] (2) Pencil hardness test: GB / T 6739-2006 was used to measure the hardness of a 500g pencil.

[0319] (3) High temperature 50°C test: The protective film 100 is bonded to a curved screen mobile phone with an anti-fingerprint layer using the above-mentioned screen bonding method; after bonding, the curved screen mobile phone with the protective film 100 is placed in a constant temperature and humidity environment at 50°C, taken out after 24 hours, and inspected after returning to normal temperature for 1 hour.

[0320] (4) Low temperature test at -15°C: The protective film 100 is bonded to a curved screen mobile phone with an anti-fingerprint layer using the above-mentioned screen bonding method. After bonding, the curved screen mobile phone with the protective film 100 is placed in a constant temperature and humidity environment at -15°C for 24 hours and then taken out and inspected after returning to normal temperature for 1 hour.

[0321] (5) Dynamic friction coefficient test: Use a dynamic friction coefficient meter to test, fix the sample on the test bench, load: 200±20g (weight, 2cm*2cm cover glass, 2cm*2cm double-sided tape, 2cm*2cm test paper hakuai 2022); test instrument: MXD-02 (or equivalent); fix the test sample, move the load 50mm (test speed: 100mm / min).

[0322] (6) Transmittance and haze measurement: The transmittance is measured using a transmittance tester, where the transmittance is the transmittance at 550 nm.

[0323] (7) Lab value: measured by a colorimeter.

[0324] The test results of Examples 1 to 8, Comparative Examples 1 and 2 are shown in Table 1 below:

[0325] Table 1 Performance parameters of the protective film 100 of Examples 1 to 8, Comparative Examples 1 and 2 attached to the curved screen 210

[0326]

[0327]

[0328] From the test results of Examples 1 to 4 in Table 1, it can be seen that when the protective film 100 of the embodiment of the present application is applied to the curved screen assembly 200 or the electronic device 300, it can be well attached to the curved screen 210, has a good fit to the curved screen 210, is not prone to rebound and warping, and has good high and low temperature performance. In addition, the surface of the anti-fingerprint layer 50 side of the protective film 100 of the present application has a lower dynamic friction coefficient and a higher water drop angle. The dynamic friction coefficient of the protective film 100 is less than or equal to 0.03. The surface of the protective film 100 is relatively smooth, and the smoothness is close to that of glass. After 10,000 times of friction, the water drop angle is still above 102°, and it has a good anti-fouling effect and anti-fingerprint effect.

[0329] It can be seen from the test results of Example 1 and Example 3 that when the thickness of the intermediate processing layer 60 and the anti-fingerprint layer 50 increases, the water drop angle of the protective film 100 can be better improved, so that the protective film 100 has a higher water drop angle after 10,000 times of friction, thereby having better anti-fouling effect and anti-fingerprint effect.

[0330] From the test results of Example 3 and Example 4, it can be seen that compared with Example 4, the intermediate processing layer 60 is set between the hardening layer 20 and the anti-fingerprint layer 50 in Example 3, and the protective film 100 obtained in Example 3 has a higher water drop angle after 10,000 times of friction, thereby having a better anti-fouling effect and anti-fingerprint effect. This shows that the intermediate processing layer 60 can better increase the connection between the anti-fingerprint layer 50 and the hardening layer 20, so that the anti-fingerprint layer 50 has better wear resistance, and better improves the service life of the anti-fingerprint layer 50.

[0331] It can be seen from the test results of Example 2 and Example 5 to Example 8 that when the mass ratio of the double-ended siloxanyl perfluoropolyether and the single-ended siloxanyl perfluoropolyether in the raw material components of the anti-fingerprint layer 50 is in the range of 2 / 3 to 4, the surface of the anti-fingerprint layer 50 of the protective film 100 has a smaller dynamic friction coefficient (the dynamic friction coefficient is less than 0.03), and the protective film 100 has good wear resistance. The water drop angle after rubbing with steel wool for 10,000 times is greater than or equal to 101°, and with the increase of the mass ratio of the double-ended siloxanyl perfluoropolyether to the single-ended siloxanyl perfluoropolyether, the wear resistance of the protective film 100 gradually increases, and the water drop angle after rubbing with steel wool for 10,000 times gradually increases.

[0332] From the test results of Example 1, Comparative Example 1 and Comparative Example 2, it can be seen that compared with the combined use of dual-end siloxane-based perfluoropolyether and single-end siloxane-based perfluoropolyether in Example 1, the use of dual-end siloxane-based perfluoropolyether alone (Comparative Example 1) or the use of single-end siloxane-based perfluoropolyether alone (Comparative Example 2) increases the dynamic friction coefficient of the protective film 100 (the dynamic friction coefficient is greater than 0.3), and the wear resistance of the protective film 100 also decreases. The water drop angle after 10,000 times of steel wool friction is less than 100°.

[0333] Example 9

[0334] The protective film 100 of this embodiment is prepared by the following steps:

[0335] (1) Preparing the substrate layer 10: coating the polyurethane adhesive on the surface of the optical-grade process film, baking at 100° C. for 3 minutes, and irradiating the film under an electron beam curing device for 10 seconds to obtain the thermoplastic polyurethane substrate layer 10;

[0336] The thickness of the substrate layer 10 is 20 μm; the elastic modulus of the substrate layer 10 is 2 GPa, the tensile strength of the substrate layer 10 is 50 MPa, and the elongation at break of the substrate layer 10 is 2%.

[0337] (2) coating the surface of the substrate layer 10 with a hardening liquid, and baking at a temperature of 120° C. for 3 minutes to dry out the solvent; then irradiating the surface with a UV curing device for 10 seconds to cure the hardening liquid to form a hardened layer 20;

[0338] The thickness of the hardened layer 20 is 3 μm; the hardening liquid includes, by mass fraction, 20% of a polyurethane acrylic resin prepolymer, 10% of a hyperbranched acrylic resin (with an octagonal ring in the middle, i.e., the acrylic resin molecule includes eight branches), 5% of ethoxylated trimethylolpropane triacrylate (a first reaction monomer), 3% of methyl benzoylformate (a first photoinitiator), 5% of a double-bond terminated perfluoropolyether (a short-chain fluoride) with a weight average molecular weight of 3000, 5% of an aluminum oxide (inorganic particles) with an average particle size of 20 nm, and 52% of propylene glycol methyl ether (a first solvent);

[0339] (3) performing corona treatment on the surface of the hardened layer 20 facing away from the substrate layer 10 so that the water drop angle of the surface of the hardened layer 20 facing away from the substrate layer 10 is 10°;

[0340] (4) applying a second coating liquid on the surface of the hardened layer 20 away from the substrate layer 10, and curing the surface by ultraviolet light to form a second coating layer 72;

[0341] The thickness of the second coating layer 72 is 90 nm, and the second coating solution includes 50% polyurethane acrylic resin oligomer, 8% multifunctional acrylic monomer, 3% fourth photoinitiator (TPO), 1% leveling agent, 10% solid inorganic nanoparticles, 0.5 to 1% defoaming agent and the balance ethyl acetate;

[0342] (5) applying a first coating liquid on the surface of the second coating layer 72 away from the hardened layer 20, curing by ultraviolet light to form a first coating layer 71, and performing a corona treatment on the surface of the first coating layer 71 so that the water drop angle on the surface of the first coating layer 71 is 10°;

[0343] The thickness of the first coating layer 71 is 90 nm, and the first coating solution includes 35% polyurethane acrylic resin oligomer, 12% acrylic monomer, 3% third photoinitiator (TPO), 1% leveling agent, 10% hollow inorganic nanoparticles, 1% defoaming agent, and the balance ethyl acetate;

[0344] (6) applying the anti-fingerprint coating liquid to the surface of the first coating layer 71 facing away from the substrate layer 10, and drying to form the anti-fingerprint layer 50;

[0345] The anti-fingerprint layer 50 has a thickness of 20 nm, and the anti-fingerprint coating liquid includes 5% of a double-ended siloxane perfluoropolyether with a number average molecular weight of 8000, 5% of a single-ended siloxane perfluoropolyether with a number average molecular weight of 1000, 84% of tetrafluoroethyl ether (fluoroether solvent), 1% of lauryl alcohol (hydrolysis promoter), and 5% of an auxiliary agent;

[0346] (7) removing the optical-grade process film, applying a setting liquid on the surface of the substrate layer 10 away from the hardening layer 20, and baking at a temperature of 120° C. for 3 minutes to perform thermal curing to form a setting layer 30; and

[0347] The thickness of the setting layer 30 is 75 μm; the setting liquid comprises a first raw material component and a second raw material component, and the mass ratio of the first raw material component to the second raw material component is 5; the first raw material component comprises 50% of a polyurethane acrylate prepolymer with a weight average molecular weight of 10,000, 15% of diphenylmethane diisocyanate (a second reactive monomer), 5% of succinic anhydride (a curing agent), 3% of a photoinitiator 184, 0.5% of 2-chloroethylmethyldimethoxysilane (a first coupling agent), and 26.5% of ethyl acetate (a second solvent); the second raw material component comprises 50% of hydroxyethyl methacrylate (an acrylic monomer), 0.5% of 3-isocyanatepropyltrimethoxysilane (a second coupling agent), 3% of poly(melamine-co-formaldehyde) methanol (a film-forming agent), and 46.5% of methylal (a third solvent);

[0348] (8) coating a silicone adhesive on the surface of the shaping layer 30 facing away from the substrate layer 10, and baking at a temperature of 150° C. for 2 minutes to form an adhesive layer 40;

[0349] The thickness of the adhesive layer 40 is 10 μm.

[0350] Example 10

[0351] The protective film of this embodiment is prepared by the following steps:

[0352] (1) Preparing the substrate layer 10: coating the polyurethane adhesive on the surface of the optical-grade process film, baking at 100° C. for 3 minutes, and irradiating the film under an electron beam curing device for 10 seconds to obtain the thermoplastic polyurethane substrate layer 10;

[0353] The thickness of the substrate layer 10 is 20 μm; the elastic modulus of the substrate layer 10 is 2 GPa, the tensile strength of the substrate layer 10 is 50 MPa, and the elongation at break of the substrate layer 10 is 2%.

[0354] (2) coating the surface of the substrate layer 10 with a hardening liquid, and baking at a temperature of 120° C. for 3 minutes to dry out the solvent; then irradiating the surface with a UV curing device for 10 seconds to cure the hardening liquid to form a hardened layer 20;

[0355] The thickness of the hardened layer 20 is 3 μm; the hardening liquid includes, by mass fraction, 20% of a polyurethane acrylic resin prepolymer, 10% of a hyperbranched acrylic resin (with an octagonal ring in the middle, i.e., the acrylic resin molecule includes eight branches), 5% of ethoxylated trimethylolpropane triacrylate (a first reaction monomer), 3% of methyl benzoylformate (a first photoinitiator), 5% of a double-bond terminated perfluoropolyether (a short-chain fluoride) with a weight average molecular weight of 3000, 5% of an aluminum oxide (inorganic particles) with an average particle size of 20 nm, and 52% of propylene glycol methyl ether (a first solvent);

[0356] (3) performing corona treatment on the surface of the hardened layer 20 facing away from the substrate layer 10 so that the water drop angle of the surface of the hardened layer 20 facing away from the substrate layer 10 is 10°;

[0357] (4) applying a second coating liquid on the surface of the hardened layer 20 away from the substrate layer 10, and curing the surface by ultraviolet light to form a second coating layer 72;

[0358] The thickness of the second coating layer 72 is 90 nm, and the second coating solution includes 50% polyurethane acrylic resin oligomer, 8% multifunctional acrylic monomer, 3% fourth photoinitiator (TPO), 1% leveling agent, 10% solid inorganic nanoparticles, 0.5 to 1% defoaming agent and the balance ethyl acetate;

[0359] (5) applying a first coating liquid on the surface of the second coating layer 72 away from the hardened layer 20, curing by ultraviolet light to form a first coating layer 71, and performing a corona treatment on the surface of the first coating layer 71 so that the water drop angle on the surface of the first coating layer 71 is 10°;

[0360] The thickness of the first coating layer 71 is 90 nm, and the first coating solution includes 35% polyurethane acrylic resin oligomer, 12% acrylic monomer, 3% third photoinitiator (TPO), 1% leveling agent, 10% hollow inorganic nanoparticles, 1% defoaming agent, and the balance ethyl acetate;

[0361] (6) applying the treatment liquid to the surface of the first coating layer 71 away from the substrate layer 10, and drying to form the intermediate treatment layer 60;

[0362] The thickness of the intermediate treatment layer 60 is 10 nm, and the treatment solution includes 40% 2-chloroethylmethyldimethoxysilane (silane coupling agent), 1% silicon dioxide (inorganic nanoparticles) and 59% ethyl acetate;

[0363] (7) applying the anti-fingerprint coating liquid to the surface of the intermediate treatment layer 60 facing away from the substrate layer 10, and drying to form the anti-fingerprint layer 50;

[0364] The anti-fingerprint layer 50 has a thickness of 20 nm, and the anti-fingerprint coating liquid includes 5% of a double-ended siloxane perfluoropolyether with a number average molecular weight of 8000, 5% of a single-ended siloxane perfluoropolyether with a number average molecular weight of 1000, 84% of tetrafluoroethyl ether (fluoroether solvent), 1% of lauryl alcohol (hydrolysis promoter), and 5% of an auxiliary agent;

[0365] (8) removing the optical-grade process film, applying a setting liquid on the surface of the substrate layer 10 away from the hardening layer 20, and baking at a temperature of 120° C. for 3 minutes to perform thermal curing to form a setting layer 30; and

[0366] The thickness of the setting layer 30 is 75 μm; the setting liquid comprises a first raw material component and a second raw material component, and the mass ratio of the first raw material component to the second raw material component is 5; the first raw material component comprises 50% of a polyurethane acrylate prepolymer with a weight average molecular weight of 10,000, 15% of diphenylmethane diisocyanate (a second reactive monomer), 5% of succinic anhydride (a curing agent), 3% of a photoinitiator 184, 0.5% of 2-chloroethylmethyldimethoxysilane (a first coupling agent), and 26.5% of ethyl acetate (a second solvent); the second raw material component comprises 50% of hydroxyethyl methacrylate (an acrylic monomer), 0.5% of 3-isocyanatepropyltrimethoxysilane (a second coupling agent), 3% of poly(melamine-co-formaldehyde) methanol (a film-forming agent), and 46.5% of methylal (a third solvent);

[0367] (9) coating a silicone adhesive on the surface of the shaping layer 30 facing away from the substrate layer 10, and baking at a temperature of 150° C. for 2 minutes to form an adhesive layer 40;

[0368] The thickness of the adhesive layer 40 is 10 μm.

[0369] Embodiment 11

[0370] The protective film 100 of this embodiment is prepared by the following steps:

[0371] (1) Preparing the substrate layer 10: coating the polyurethane adhesive on the surface of the optical-grade process film, baking at 100° C. for 3 minutes, and irradiating the film under an electron beam curing device for 10 seconds to obtain the thermoplastic polyurethane substrate layer 10;

[0372] The thickness of the substrate layer 10 is 20 μm; the elastic modulus of the substrate layer 10 is 2 GPa, the tensile strength of the substrate layer 10 is 50 MPa, and the elongation at break of the substrate layer 10 is 2%.

[0373] (2) coating the surface of the substrate layer 10 with a hardening liquid, and baking at a temperature of 120° C. for 3 minutes to dry out the solvent; then irradiating the surface with a UV curing device for 10 seconds to cure the hardening liquid to form a hardened layer 20;

[0374] The thickness of the hardened layer 20 is 3 μm; the hardening liquid includes, by mass fraction, 20% of a polyurethane acrylic resin prepolymer, 10% of a hyperbranched acrylic resin (with an octagonal ring in the middle, i.e., the acrylic resin molecule includes eight branches), 5% of ethoxylated trimethylolpropane triacrylate (a first reaction monomer), 3% of methyl benzoylformate (a first photoinitiator), 5% of a double-bond terminated perfluoropolyether (a short-chain fluoride) with a weight average molecular weight of 3000, 5% of an aluminum oxide (inorganic particles) with an average particle size of 20 nm, and 52% of propylene glycol methyl ether (a first solvent);

[0375] (3) performing corona treatment on the surface of the hardened layer 20 facing away from the substrate layer 10 so that the water drop angle of the surface of the hardened layer 20 facing away from the substrate layer 10 is 10°;

[0376] (4) alternately evaporating niobium oxide layers and silicon oxide layers on the surface of the hardening layer 20 facing away from the substrate layer 10, wherein the niobium oxide layer is two layers and the silicon oxide layer is two layers, that is, the anti-reflection layer 70 includes a niobium oxide layer, a silicon oxide layer, a niobium oxide layer and a silicon oxide layer stacked in sequence;

[0377] (5) applying the anti-fingerprint coating liquid on the surface of the silicon oxide layer facing away from the substrate layer 10, and drying to form the anti-fingerprint layer 50;

[0378] The anti-fingerprint layer 50 has a thickness of 20 nm, and the anti-fingerprint coating liquid includes 5% of a double-ended siloxane perfluoropolyether with a number average molecular weight of 8000, 5% of a single-ended siloxane perfluoropolyether with a number average molecular weight of 1000, 84% of tetrafluoroethyl ether (fluoroether solvent), 1% of lauryl alcohol (hydrolysis promoter), and 5% of an auxiliary agent;

[0379] (6) removing the optical-grade process film, applying a setting liquid on the surface of the substrate layer 10 away from the hardening layer 20, and baking at a temperature of 120° C. for 3 minutes to perform thermal curing to form a setting layer 30; and

[0380] The thickness of the setting layer 30 is 75 μm; the setting liquid comprises a first raw material component and a second raw material component, and the mass ratio of the first raw material component to the second raw material component is 5; the first raw material component comprises 50% of a polyurethane acrylate prepolymer with a weight average molecular weight of 10,000, 15% of diphenylmethane diisocyanate (a second reactive monomer), 5% of succinic anhydride (a curing agent), 3% of a photoinitiator 184, 0.5% of 2-chloroethylmethyldimethoxysilane (a first coupling agent), and 26.5% of ethyl acetate (a second solvent); the second raw material component comprises 50% of hydroxyethyl methacrylate (an acrylic monomer), 0.5% of 3-isocyanatepropyltrimethoxysilane (a second coupling agent), 3% of poly(melamine-co-formaldehyde) methanol (a film-forming agent), and 46.5% of methylal (a third solvent);

[0381] (7) coating a silicone adhesive on the surface of the shaping layer 30 facing away from the substrate layer 10, and baking at a temperature of 150° C. for 2 minutes to form an adhesive layer 40;

[0382] The thickness of the adhesive layer 40 is 10 μm.

[0383] The protective films 100 of Examples 9 to 11 were subjected to screen-attachment tests, and the test results are shown in Table 2 below:

[0384] Table 2 Performance parameters of the protective film 100 of Example 1, Example 9 to Example 11 attached to the curved screen 210

[0385]

[0386] It can be seen from the test results in Table 2 that after the protective film 100 of the embodiment of the present application is added with the anti-reflection layer 70, the light transmittance of the protective film 100 can be better improved and the haze of the protective film 100 can be reduced. In addition, when compared with the first coating 71 and the second coating 72, when the anti-reflection layer 70 adopts the first coating 73 and the second coating 74, the protective film 100 has a higher transmittance and a lower haze.

[0387] Mentioning "embodiment" and "implementation method" in this application means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrases in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this application can be combined with other embodiments. In addition, it should also be understood that the features, structures or characteristics described in the various embodiments of the present application can be arbitrarily combined to form another embodiment that does not deviate from the spirit and scope of the technical solution of the present application, if there is no contradiction between them.

[0388] Finally, it should be noted that the above implementation modes are only used to illustrate the technical solution of the present application and are not intended to limit it. Although the present application has been described in detail with reference to the above preferred implementation modes, a person of ordinary skill in the art should understand that the technical solution of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present application.

Claims

1. A protective film, characterized in that: include: substrate layer; A hardening layer, wherein the hardening layer is disposed on one side of the substrate layer; as well as An anti-fingerprint layer, wherein the anti-fingerprint layer is arranged on a side of the hardened layer away from the substrate layer; the raw material components of the anti-fingerprint layer include a double-ended siloxane-based perfluoropolyether and a single-ended siloxane-based perfluoropolyether; the mass ratio of the double-ended siloxane-based perfluoropolyether and the single-ended siloxane-based perfluoropolyether in the raw material components of the anti-fingerprint layer is in a range of 2 / 3 to 4.

2. The protective film according to claim 1, characterized in that: The raw material components of the anti-fingerprint layer also include a hydrolysis promoter, and the amount of the hydrolysis promoter added to the raw material components of the anti-fingerprint layer is 2% to 10% of the total mass of the dual-end siloxane-based perfluoropolyether and the single-end siloxane-based perfluoropolyether.

3. The protective film according to claim 1, characterized in that: The raw material components of the anti-fingerprint layer include, by mass fraction, 10% to 30% of double-ended siloxane-based perfluoropolyether, 5% to 20% of single-ended siloxane-based perfluoropolyether and 1% to 3% of a hydrolysis promoter.

4. The protective film according to claim 1, characterized in that: The number average molecular weight of the dual-end siloxane-based perfluoropolyether is in the range of 3000 to 8000; the number average molecular weight of the single-end siloxane-based perfluoropolyether is in the range of 1000 to 8000.

5. The protective film according to claim 1, characterized in that: The protective film further includes an intermediate processing layer, the intermediate processing layer is located between the hardening layer and the anti-fingerprint layer, and the intermediate processing layer includes a silane coupling agent.

6. The protective film according to claim 5, characterized in that: The intermediate treatment layer further comprises inorganic nanoparticles. In the intermediate treatment layer, the mass fraction of the silane coupling agent ranges from 97.5% to 99.9%, and the mass fraction of the inorganic nanoparticles ranges from 0.1% to 2.5%.

7. The protective film according to claim 5, characterized in that: The thickness ratio of the intermediate treatment layer to the anti-fingerprint layer ranges from 0.5 to 0.

67.

8. The protective film according to any one of claims 1 to 7, characterized in that: The protective film is applied to a curved screen, and the protective film further comprises: A shaping layer, which is disposed on a side of the substrate layer away from the hardening layer, and is a heat-light dual-curing shaping layer. Before the protective film is applied to the curved screen, the shaping layer is thermally cured, and when the protective film is applied to the curved screen, the shaping layer is light-cured and shaped; and An adhesive layer is disposed on a side of the shaping layer away from the substrate layer, and is used to adhere the protective film to the curved screen.

9. A method for preparing a protective film, characterized in that: include: providing a substrate layer; forming a hardening layer on one side of the base material layer; as well as An anti-fingerprint layer is formed on a side of the hardened layer away from the substrate layer, wherein the anti-fingerprint layer comprises a dual-end siloxane-based perfluoropolyether and a single-end siloxane-based perfluoropolyether; in the anti-fingerprint layer, a mass ratio of the dual-end siloxane-based perfluoropolyether to the single-end siloxane-based perfluoropolyether is in a range of 2 / 3 to 4.

10. The method for preparing a protective film according to claim 9, characterized in that: Before forming the anti-fingerprint layer on the side of the hardened layer away from the substrate layer, the method further comprises: The hardened layer is surface-treated so that a water drop angle of a surface of the hardened layer facing away from the substrate layer is in a range of 10° to 40°.

11. The method for preparing a protective film according to claim 9, characterized in that: Before forming the anti-fingerprint layer on the side of the hardened layer away from the substrate layer, the method further comprises: forming an intermediate treatment layer on a surface of the hardened layer away from the substrate layer; After the anti-fingerprint layer is formed on the side of the hardened layer away from the substrate layer, the method further comprises: forming a shaping layer on a side of the substrate layer facing away from the hardening layer; and An adhesive layer is formed on the side of the shaping layer facing away from the substrate layer.

12. A curved screen assembly, characterized in that: include: A curved screen, wherein the curved screen has a display surface; as well as The protective film according to any one of claims 1 to 8 is arranged on the display surface, between the substrate layer, the hardened layer and the curved screen.

13. An electronic device, characterized in that: include: The curved screen assembly according to claim 12; as well as A processor is electrically connected to the curved screen assembly and is used to control the curved screen assembly to display.

Citation Information

Cited By

  • Ultrahigh-water-drop-angle 9H curved-surface protective film capable of being bent and shaped and production process

    CN120382702A