Preparation method of acrylate pressure-sensitive adhesive for water-soluble label

By adding water-soluble modified monomers and introducing AMPS monomers, combined with the self-crosslinking mechanism of N-(hydroxymethyl)acrylamide, a water-soluble acrylate pressure-sensitive adhesive was prepared, which solved the problem of acrylate pressure-sensitive adhesives in the existing technology. The problem of sensitive glue being insoluble in water enables removal without the need for organic solvents and reduces the risk of environmental pollution.

CN118834633APending Publication Date: 2024-10-25JIANGXI ZHENGUAN ENVIRONMENTALLY FRIENDLY BIODEGRADABLE NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411036601.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing acrylic pressure-sensitive adhesives are insoluble in water, requiring the use of organic solvents for removal, causing environmental pollution and making it difficult to obtain.

Method used

By increasing the content of water-soluble modified monomers acrylic acid and hydroxyethyl acrylate, and introducing AMPS monomer, combined with the self-crosslinking mechanism of N-(hydroxymethyl)acrylamide, a water-soluble acrylate pressure-sensitive adhesive was prepared. Completely soluble in water.

Benefits of technology

It realizes that the pressure-sensitive adhesive can be completely removed using clean water at normal temperature, avoiding the use of organic solvents and reducing the risk of environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to a preparation method of an acrylate pressure-sensitive adhesive for a water-soluble label, and belongs to the technical field of synthesis of acrylate pressure-sensitive adhesives. In addition, a special water-soluble monomer 2-acrylamido-2-methylpropanesulfonic acid (abbreviated in English: AMPS) is introduced to overcome the problems mentioned above; aMPS is a sulfonic acid group surfactant with strong anionic water solubility, and active double bonds enable the AMPS to have addition polymerization performance, so that the AMPS can be used for producing copolymers with various hydrocarbon monomers; the prepared acrylate pressure-sensitive adhesive for the water-soluble label can be completely removed after being soaked in clear water at normal temperature (15-35 DEG C).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of synthesis of acrylic ester pressure-sensitive adhesives, and relates to the synthesis and production of water-soluble labels using acrylic ester pressure-sensitive adhesives. Background Art

[0002] Acrylic pressure-sensitive adhesives used in common labels in daily life have certain water resistance, chemical resistance and insolubility in water. If they remain on the surface of the adhered object during the removal process after use, they need to be removed with organic solvents such as ethyl acetate and toluene or professional debonding agents. However, organic solvents are not easy to obtain in daily life or it is troublesome to buy professional debonding agents. In some industrial recycling and reuse, it is necessary to automatically remove labels on packaging, and commonly used labels need to be removed by immersion in organic solvents. The large-scale use of organic solvents is not only expensive, but also easily causes environmental pollution if not handled properly.

[0003] Usually, ordinary acrylic pressure-sensitive adhesives are made of viscous monomers with lower glass transition temperatures (usually glass transition temperature Tg value: -20~-70℃) to provide viscosity, cohesive monomers with higher glass transition temperatures to provide cohesion, and modified monomers containing reactive functional groups to provide cross-linking sites, which react to form high molecular polymers and are then cured. Among them, the viscous monomers and cohesive monomers are mainly alkyl acrylates, which are insoluble in water and usually account for more than 80% of the monomer content. Therefore, common acrylic pressure-sensitive adhesives have good weather resistance and water resistance, and will not dissolve after long-term immersion in water. In addition, commonly used solvent-based acrylic pressure-sensitive adhesives are generally cross-linked and cured with curing agents such as metal salts, isocyanates, and epoxy resins. After cross-linking, they have good water resistance and are not easy to dissolve.

[0004] Commonly used modified monomers acrylic acid and hydroxyethyl acrylate are water-soluble monomers, but because acrylic acid (Tg value: 106°C) has a high glass transition temperature, if used alone in large quantities, it will lead to a high overall glass transition temperature of the pressure-sensitive adhesive, and the pressure-sensitive adhesive will lose its initial viscosity and pressure sensitivity. Although hydroxyethyl acrylate (Tg value: -15°C) has a low glass transition temperature, it has a high reaction activity. If used alone in large quantities, gelation is very likely to occur during the reaction, making it impossible to process and coat the subsequent stage. Summary of the invention

[0005] Based on the above, a water-soluble acrylic pressure-sensitive adhesive for labels was developed. The synthesis steps are as follows: Step 1: 290-300 parts by weight of isooctyl acrylate monomer, 40-45 parts by weight of acrylic acid, 17-23 parts by weight of hydroxyethyl acrylate, 200-230 parts by weight of ethyl acetate as solvent, and 100-140 parts by weight of anhydrous ethanol are placed in a glass reactor and passed with nitrogen for more than 1 hour.

[0006] Step 2: Add DMF: 100-140 parts by weight, AMPS: 50-70 parts by weight, modified monomer N-(hydroxymethyl) acrylamide (abbreviated as: N-hydroxy): 10-15 parts by weight, and AIBN: 0.19-0.26 parts by weight into a constant pressure dropping funnel and stir until completely dissolved for later use.

[0007] Step 3: Heat the mixed solution in the reactor in step 1 to 64-65°C and stabilize it for about 5 minutes. Use 8-12 parts by weight of ethyl acetate to dissolve 0.4-0.5 parts by weight of azobisisobutyronitrile (AIBN), add it to the reactor, and start dripping when there is obvious heat release and start timing. Control the temperature at 64-65°C and drip for 2 hours. After the dripping is completed, react at 64-65°C for 1 hour, then gradually increase the temperature (0.5°C / minute) to 70-75°C and continue to react for 1 hour.

[0008] Step 4: Dissolve 1-1.4 parts of AIBN in 12-18 parts by weight of ethyl acetate, add into the reaction kettle, and keep warm at above 78°C for 1 hour.

[0009] Step 5: After keeping warm for 1 hour, dissolve 1.0 g of AIBN in 8-12 parts by weight of ethyl acetate, add the mixture into the reactor, and keep warm at above 78° C. for 2.5 hours.

[0010] Step 6: After the heat preservation is completed, cool to below 50°C, add 40-50 parts by weight of ethyl acetate, 58-62 parts by weight of anhydrous ethanol, and 27-29 parts by weight of triethanolamine (to neutralize the acid and form a salt), stir for more than 1 hour, and package the material.

[0011] Step 7: Take 100g of the prepared glue and apply it directly on the 36umPET substrate. Apply it on the 36umPET substrate. The dry glue is 25~30g / m 2 About, dried at 100℃ for 3 minutes, protected with release film, and aged in an oven at 50℃ for more than 24 hours.

[0012] The present invention overcomes the above-mentioned problems by appropriately increasing the content of water-soluble modified monomers acrylic acid and hydroxyethyl acrylate, and introducing a special water-soluble monomer 2-acrylamide-2-methylpropanesulfonic acid (English abbreviation: AMPS); AMPS is a sulfonic acid group surfactant with strong anionic water solubility, and the active double bond makes it have addition polymerization properties, and can produce copolymers with various hydrocarbon monomers.

[0013] The present invention uses modified monomer N-(hydroxymethyl) acrylamide (abbreviated as: N-hydroxy) for self-crosslinking. Because N-hydroxy contains active hydroxymethyl, the hydroxymethyl will condense with each other and self-crosslink under heating or acid catalysis. Because N-hydroxy has high water solubility, partial crosslinking and hydrolysis after soaking in water greatly increase the water solubility of the pressure-sensitive adhesive. The self-crosslinking mechanism is as follows: .

[0014] The water-soluble acrylate pressure-sensitive adhesive for labels prepared by the present invention can be completely removed by soaking in clean water at room temperature (15-35° C.). DETAILED DESCRIPTION

[0015] The present case will be further explained and illustrated below in conjunction with specific implementation methods.

[0016]

[0017] The pressure-sensitive adhesive prepared above was tested as follows, and the test results are as follows:

Claims

1. A method for preparing an acrylic pressure-sensitive adhesive for a water-soluble label, characterized in that the preparation method comprises the following steps: Step 1: 290-300 parts by weight of isooctyl acrylate, 40-45 parts by weight of acrylic acid, 17-23 parts by weight of hydroxyethyl acrylate, 200-230 parts by weight of ethyl acetate, and 100-140 parts by weight of anhydrous ethanol are placed in a glass reactor and passed with nitrogen for more than 1 hour; Step 2: Add DMF: 100-140 parts by weight, AMPS: 50-70 parts by weight, modified monomer N-(hydroxymethyl) acrylamide: 10-15 parts by weight, and AIBN: 0.19-0.26 parts by weight into a constant pressure dropping funnel and stir until completely dissolved for later use; Step 3: Heat the mixed solution in the reaction kettle in step 1 to 64-65°C, dissolve 0.4-0.5 parts by weight of azobisisobutyronitrile in 8-12 parts by weight of ethyl acetate after stabilization, add the mixture to the reaction kettle, and start dripping when there is obvious heat release and timing, control the temperature to drip at 64-65°C, react at 64-65°C after the dripping is completed, and gradually increase the temperature to 70-75°C at 0.5°C / min to continue the reaction; Step 4: Dissolve 1-1.4 parts by weight of AIBN in 12-18 parts by weight of ethyl acetate, add to the reaction kettle, and keep warm at above 78°C; Step 5: Keep warm, then dissolve AIBN with 8-12 parts by weight of ethyl acetate: 1.0g, add to the reactor, keep warm at above 78℃; Step 6: After the heat preservation is completed, cool the mixture, add 40-50 parts by weight of ethyl acetate, 58-62 parts by weight of anhydrous ethanol, and 27-29 parts by weight of triethanolamine, stir evenly, and package the material; Step 7: Apply the prepared glue directly on the PET substrate, with a dry glue weight of 25-30 g / m 2 About, dried at 100℃ for 3 minutes, attached with release film for protection, and oven cured.

2. The method for preparing the acrylic pressure-sensitive adhesive for water-soluble labels according to claim 1, characterized in that: The preparation method comprises the following steps: Step 1: Put 295g of isooctyl acrylate, 42g of acrylic acid, 20g of hydroxyethyl acrylate, 210g of ethyl acetate and 120g of anhydrous ethanol into a glass reactor and pass nitrogen for more than 1 hour; Step 2: Add 120 g of DMF, 60 g of AMPS, 12 g of modified monomer N-(hydroxymethyl)acrylamide, and 0.23 g of AIBN into a constant pressure dropping funnel and stir until completely dissolved for later use; Step 3: Heat the mixed solution in the reactor to 64-65°C and stabilize for about 5 minutes, use 10g of ethyl acetate to dissolve 0.45g of azobisisobutyronitrile, add it to the reactor, and start dripping when there is obvious heat release and timing, control the temperature at 64-65°C and drip for 2 hours, after the dripping is completed, react at 64-65°C for 1 hour, gradually increase the temperature to 70-75°C at 0.5°C / min and continue to react for 1 hour; Step 4: Dissolve 1.2 g of AIBN in 15 g of ethyl acetate and add to the reactor, and keep the temperature above 78°C for 1 hour; Step 5: After keeping warm for 1 hour, dissolve 1.0 g of AIBN in 10 g of ethyl acetate, add to the reactor, and keep warm at above 78°C for 2.5 hours; Step 6: After the heat preservation is completed, cool to below 50°C, add 45g of ethyl acetate, 60g of anhydrous ethanol, and 28.5g of triethanolamine, stir for more than 1 hour, and package the material; Step 7: Take 100g of the prepared glue and apply it directly on the 36umPET substrate. Apply it on the 36umPET substrate. The dry glue is 25~30g / m 2 About, dried at 100℃ for 3 minutes, protected with release film, and aged in an oven at 50℃ for more than 24 hours.

3. An acrylic pressure-sensitive adhesive for a water-soluble label, characterized in that: The water-soluble acrylic pressure-sensitive adhesive for labels is prepared by the preparation method described in claim 1 or 2.