IBC battery aluminum paste, preparation method thereof and IBC battery
By adding fumed silica to the aluminum paste, the problem of warping and cracking of the IBC battery aluminum paste when it is printed into the positive electrode grid is solved, achieving the effect of reducing warpage and maintaining electrical performance.
Patent Information
- Application Number
- CN202310384824.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-04-11
AI Technical Summary
When the existing IBC battery aluminum paste is printed into positive grid lines, it is easy to cause warping and cracking of the battery, causing economic losses.
An aluminum slurry composed of aluminum powder, boron powder, glass powder, fumed silica, organic binder and organic additives is used. By adding fumed silica to the aluminum slurry, it is evenly distributed around the aluminum powder to prevent the aluminum powder from interacting with each other. Melting reduces the difference in stress release coefficient between the aluminum paste and the silicon wafer and reduces warpage.
It effectively solves the warping problem of IBC batteries when cooling after sintering, reduces cell cracks, and maintains good electrical performance of the battery.
Smart Images

Figure CN118841203A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of crystalline silicon solar cell manufacturing, and in particular to an IBC battery aluminum paste and a preparation method thereof, and an IBC battery. Background Art
[0002] The interdigitated back contact (IBC) battery is a new type of battery in which the contact electrodes of the P / N junction, substrate and emitter region are made in an interdigitated shape on the back of the battery. Its core technology is to prepare high-quality p+ and n+ regions on the back of the battery with interdigitated arrangement.
[0003] At present, IBC batteries need to print aluminum paste in the p+ region and sinter to form positive electrode grid lines. However, aluminum and silicon easily form aluminum-silicon alloy during the sintering process. When the aluminum-silicon alloy is cooled, the warping of the IBC battery will increase, causing hidden cracks in the battery cell, which will lead to economic losses. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide an IBC battery aluminum paste and a preparation method thereof, and an IBC battery, so as to solve the problem that the existing IBC battery aluminum paste is prone to warping when printing into positive electrode grid lines, resulting in hidden cracks in the battery cell.
[0005] In order to solve the above problems, the present invention is achieved through the following technical solutions:
[0006] The present invention provides an IBC battery aluminum paste, wherein the components constituting the aluminum paste include aluminum powder, boron powder, glass powder, fumed silica, an organic binder and an organic additive.
[0007] Furthermore, in the IBC battery aluminum paste, the mass percentage of the aluminum powder is 72-77%; the mass percentage of the boron powder is 0.04-0.1%; the mass percentage of the glass powder is 1-1.5%; the mass percentage of the fumed silica is 0.03-0.06%; the mass percentage of the organic binder is 20.74-25.74%; and the mass percentage of the organic additive is 0.2-0.6%.
[0008] Furthermore, in the IBC battery aluminum paste, the fumed silica includes nano-scale fumed silica.
[0009] Furthermore, in the IBC battery aluminum paste, the organic additive includes one or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl alcohol phosphate, Digo 655, and BYKl10.
[0010] Furthermore, in the IBC battery aluminum paste, the aluminum powder includes micron-spherical aluminum powder and nano-spherical aluminum powder.
[0011] Furthermore, in the IBC battery aluminum paste, the organic binder includes a high molecular polymer resin and an organic solvent;
[0012] The mass fraction of the high molecular weight polymer in the organic binder is 6 to 8%;
[0013] The mass fraction of the organic solvent in the organic binder is 92-94%.
[0014] Furthermore, in the IBC battery aluminum paste, the organic solvent includes at least four of benzyl alcohol, diethyl phthalate, pineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.
[0015] Furthermore, in the IBC battery aluminum paste, the glass powder is composed of 3 to 15 parts by mass of SiO 2 , 1 to 15 parts Bi 2 O 3 , 35-80 parts PbO, 0.5-5 parts TiO 2 , 0.5~5 parts Al 2 O 3 , 0.5-10 parts ZnO, 0.5-3 parts MgO, 0.5-5 parts V 2 O 5 , 0.5~3 parts Li 2 O is obtained by sintering and crushing.
[0016] The present invention also proposes a method for preparing IBC battery aluminum paste, which comprises:
[0017] mixing an organic binder, boron powder, aluminum powder, fumed silica and glass powder to obtain a mixture;
[0018] After the mixture is ground, an organic additive is added to obtain IBC battery aluminum paste.
[0019] The present invention further proposes an IBC battery, wherein a plurality of positive electrode grid lines are attached to the back of the IBC battery, and the grid lines are prepared from the above-mentioned aluminum paste.
[0020] Compared with the prior art, the embodiments of the present invention have the following advantages:
[0021] In the embodiment of the present invention, the aluminum paste for IBC battery provided comprises aluminum powder, boron powder, glass powder, fumed silica, organic binder and organic additive. By adding fumed silica to the aluminum paste, in the process of forming fine grids of the aluminum paste, the fumed silica can be evenly distributed around the aluminum powder, preventing the aluminum powder from melting into each other, reducing the difference in stress release coefficient between the aluminum paste and the silicon wafer, and reducing the warping of the IBC battery during cooling after sintering, thereby solving the problem that the existing IBC battery aluminum paste is easy to cause the IBC battery to warp when printing the positive grid line, causing the battery cell to crack.
[0022] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a flow chart of the method for preparing silver-aluminum paste for IBC batteries provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0024] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0025] The applicant of the present invention has found that in the current positive electrode metallization process of P-type IBC, it is necessary to print aluminum paste in the laser groove that is connected to the P-type doped area, and then form the positive electrode grid line through high temperature sintering. However, aluminum and silicon are very easy to form aluminum-silicon alloy under high temperature conditions exceeding 577 degrees Celsius, and the grid lines of IBC batteries are all printed on the back of the battery. This makes the above-mentioned aluminum-silicon alloy have a different stress release coefficient from the silicon wafer during cooling, which will significantly increase the warpage of the IBC battery, causing hidden cracks in the battery cell, and thus leading to economic losses.
[0026] In particular, with the influence of factors such as the rising price of silicon materials, the thickness of silicon wafers has been reduced from 170 microns to 140 microns, further aggravating the warping of IBC batteries caused by the formation of aluminum-silicon alloy during the metallization process.
[0027] In order to solve the above problems, an embodiment of the present invention provides an IBC battery aluminum paste, wherein the components constituting the aluminum paste include aluminum powder, boron powder, glass powder, fumed silica, an organic binder and an organic additive.
[0028] The IBC battery aluminum paste provided in the embodiment of the present invention can be an aluminum paste for forming the positive electrode grid line of a P-type IBC battery, or it can be an aluminum paste for forming the positive electrode grid line of an N-type IBC battery. Specifically, it is printed on the back of the IBC battery in the laser groove that is connected to the P-type doped area, and then sintered at a high temperature to form the positive electrode grid line.
[0029] Among them, aluminum powder is the main component, and aluminum powder mainly replaces the P+ emitter of the battery; glass powder is an inorganic adhesive, which will melt into liquid under high temperature conditions and condense when cooled to play a bonding role; organic adhesive can ensure the overall bonding effect; organic additives can reduce the overall viscosity of the aluminum paste; and boron powder can diffuse into the silicon for heavy doping during high-temperature sintering, which is beneficial to improve the contact performance of the slurry and reduce the reaction contact surface between aluminum and silicon; and in the process of aluminum paste forming a fine grid, gas-phase silicon dioxide can be evenly distributed around the aluminum powder, preventing aluminum powder from melting each other, reducing the difference in stress release coefficient between aluminum paste and silicon wafer, reducing the warping of IBC batteries during cooling after sintering, and alleviating hidden cracks in the battery cells caused by warping.
[0030] Therefore, the aluminum paste provided in the embodiment of the present invention can effectively solve the problem that the existing IBC battery aluminum paste is prone to warping and causing hidden cracks in the battery cell when printing the positive electrode grid line.
[0031] Optionally, in one embodiment, in the aluminum paste, the mass percentage of aluminum powder is 72-77%, the mass percentage of boron powder is 0.04-0.1%, the mass percentage of glass powder is 1-1.5%, the mass percentage of fumed silica is 0.03-0.06%, the mass percentage of organic binder is 20.74-25.74%, and the mass percentage of organic additive is 0.2-0.6%. In the aluminum paste provided by the embodiment of the present invention, the content of fumed silica is relatively low, so that the electrical performance of the battery cell remains good.
[0032] For example, in the aluminum paste, the mass fractions of aluminum powder, boron powder, glass powder, fumed silica, organic binder and organic additive are 72%, 0.1%, 1.5%, 0.06%, 25.74% and 0.6%, respectively.
[0033] For example, in the aluminum paste, the mass fractions of aluminum powder, boron powder, glass powder, fumed silica, organic binder and organic additive are 77%, 0.04%, 1%, 0.03%, 21.73% and 0.2%, respectively.
[0034] For example, in the aluminum paste, the mass fractions of aluminum powder, boron powder, glass powder, fumed silica, organic binder and organic additive are 77%, 0.1%, 1.5%, 0.06%, 20.74% and 0.6%, respectively.
[0035] For example, in the aluminum paste, the mass fractions of aluminum powder, boron powder, glass powder, fumed silica, organic binder and organic additive are 75%, 0.03%, 1.3%, 0.04%, 23.28% and 0.35%, respectively.
[0036] For example, in the aluminum paste, the mass fractions of aluminum powder, boron powder, glass powder, fumed silica, organic binder and organic additive are 77%, 0.08%, 1.5%, 0.06%, 20.86% and 0.5%, respectively.
[0037] Optionally, in one embodiment, the fumed silica comprises nano-scale fumed silica.
[0038] Optionally, in one embodiment, the boron powder includes micron-sized elemental boron. By adding the micron-sized elemental boron, the boron powder can quickly diffuse into the silicon for heavy doping during high-temperature sintering, which is beneficial to improving the contact performance of the slurry.
[0039] Optionally, in one embodiment, the aluminum powder includes micron-sized spherical aluminum powder and nano-sized spherical aluminum powder, wherein there are gaps between the micron-sized aluminum powder and the nano-sized spherical aluminum powder can just fill and penetrate into the gaps between the micron-sized aluminum powder.
[0040] Optionally, in a specific embodiment, the aluminum powder includes 90-95% by mass of micron-sized spherical aluminum powder and 5-10% by mass of nano-sized spherical aluminum powder. Since there are gaps between the micron-sized aluminum powders, the nano-sized spherical aluminum powder can just fill and penetrate into the gaps between the micron-sized aluminum powders.
[0041] Optionally, in a specific embodiment, the aluminum powder includes micron-sized spherical aluminum powder with a purity of 3 9s and a mass fraction of 90-95%, and nano-sized spherical aluminum powder with a purity of 3 9s and a mass fraction of 5-10%.
[0042] Optionally, in one embodiment, the organic auxiliary agent includes one or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl alcohol phosphate, Digo 655, and BYKl10.
[0043] In the IBC battery aluminum paste provided in the embodiment of the present invention, the above-mentioned organic binder includes a polymer resin and an organic solvent; wherein the polymer resin is dissolved in the organic solvent, so that the organic solvent can be used as an organic binder, that is, the paste plays a role of bonding powder after drying.
[0044] Optionally, in one embodiment, the mass fraction of the high molecular weight polymer in the organic binder is 6-8%; the mass fraction of the organic solvent in the organic binder is 92-94%.
[0045] Optionally, in one embodiment, the high molecular weight polymer is one or more of ethyl cellulose-N20, ethyl cellulose N-50, and ethyl cellulose-N100;
[0046] The organic solvent includes at least four of benzyl alcohol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester dodecahydrate.
[0047] Optionally, in one embodiment, the glass powder comprises 3 to 15 parts by mass of SiO 2 , 1 to 15 parts Bi 2 O 3 , 35-80 parts PbO, 0.5-5 parts TiO 2 , 0.5~5 parts Al 2 O 3 , 0.5-10 parts ZnO, 0.5-3 parts MgO, 0.5-5 parts V 2 O 5 , 0.5~3 parts Li 2 O is obtained by sintering and crushing, and the D50 of the glass powder is 1.0-1.8μm. If D50 is less than 1.0μm, the glass activity is too high, and if D50 is greater than 1.8μm, the glass activity is too low.
[0048] Among them, SiO 2 As a glass network former, it promotes glass stability and increases glass melting point; Bi 2 O 3 As the main network structure; PbO can adjust the corrosiveness of glass and reduce the melting point of glass; TiO 2 For local crystallization; Al 2 O 3 It can adjust the stability of glass and increase viscosity; ZnO can break the network structure and promote glass crystallization, MgO and V 2 O 5 Used to lower the melting point; Li 2 O can adjust glass stability, increase viscosity and promote crystallization.
[0049] The present invention also provides a method for preparing an IBC battery aluminum paste, wherein: Figure 1 As shown, it includes steps 101 to 102:
[0050] Step 101, mixing an organic binder, boron powder, aluminum powder, fumed silica and glass powder to obtain a mixture;
[0051] Step 102: Grind the mixture, add an organic additive, and obtain IBC battery aluminum paste.
[0052] In the above step 101, 20.74 to 25.74 parts of an organic binder, 0.04 to 0.1 parts of boron powder, 72 to 77 parts of aluminum powder, 0.03 to 0.06 parts of fumed silica, and 1 to 1.5 parts of glass powder are weighed, mixed, and dispersed using a disperser to obtain the above mixture.
[0053] Optionally, in one embodiment, the aluminum powder includes micron spherical aluminum powder and nano spherical aluminum powder. In the above step 101, the organic binder, nano spherical aluminum powder and gas-phase silica are first mixed and dispersed using a disperser, and then boron powder, micron spherical aluminum powder and glass powder are added, dispersed again using a disperser, and then ground to obtain the above mixture.
[0054] In the above step 102, the above mixture is ground and then 0.2 to 0.6 parts of an organic additive are added, and after high-speed dispersion, a low-warpage high-efficiency IBC battery aluminum paste is obtained.
[0055] In the embodiment of the present invention, by adding fumed silica to the aluminum paste, during the process of the aluminum paste forming a fine grid, the fumed silica can be evenly distributed around the aluminum powder, preventing the aluminum powder from fusion with the aluminum powder, reducing the difference in stress release coefficient between the aluminum paste and the silicon wafer, and reducing the warping of the IBC battery during cooling after sintering, thereby solving the problem that the existing IBC battery aluminum paste is prone to warping when printing into positive electrode grid lines, causing hidden cracks in the battery cell.
[0056] Optionally, in the preparation method provided in the embodiment of the present invention, the fumed silica includes nano-scale fumed silica.
[0057] Optionally, in the preparation method provided in the embodiment of the present invention, the organic auxiliary agent includes one or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl alcohol phosphate, Digo 655, and BYKl10.
[0058] Optionally, in the preparation method provided in the embodiment of the present invention, the organic binder comprises a high molecular polymer resin and an organic solvent;
[0059] The mass fraction of the high molecular weight polymer in the organic binder is 6 to 8%;
[0060] The mass fraction of the organic solvent in the organic binder is 92-94%.
[0061] Optionally, in the preparation method provided in an embodiment of the present invention, the organic solvent includes at least four of benzyl alcohol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.
[0062] Optionally, in the preparation method provided in the embodiment of the present invention, the glass powder comprises 3 to 15 parts by weight of SiO 2 , 1 to 15 parts Bi 2 O 3 , 35-80 parts PbO, 0.5-5 parts TiO 2 , 0.5~5 parts Al 2 O 3 , 0.5-10 parts ZnO, 0.5-3 parts MgO, 0.5-5 parts V 2 O 5 , 0.5~3 parts Li 2 O is obtained by sintering and crushing.
[0063] The present invention further provides an IBC battery, wherein a plurality of positive electrode grid lines are attached to the back of the IBC battery, and the grid lines are prepared from the above-mentioned aluminum paste.
[0064] The steps of using the aluminum paste provided in the embodiment of the present invention to make a P-type IBC battery are as follows:
[0065] (1) After forming an ultra-thin silicon oxide layer and a polysilicon layer on the back of a P-type silicon wafer, phosphorus is doped into the back polysilicon layer;
[0066] (2) forming interdigitated n+ doped regions and p+ doped regions by laser grooving; then performing double-sided atomic layer deposition (ALD) to form an aluminum oxide film, and a silicon nitride film on the front and back sides to form a passivation layer;
[0067] (3) Laser grooving the back of the battery to form a laser groove that is conductive to the p+ doped region;
[0068] (4) printing the aluminum paste in the laser groove and printing the silver paste on the passivation layer directly facing the n+ doped area;
[0069] (5) The printed silicon wafer is sintered at a maximum temperature of 788 degrees Celsius to produce a P-type IBC battery.
[0070] The present invention is described in detail below by way of examples.
[0071] Example 1
[0072] (1) Providing silver aluminum paste a1: In parts by mass, the IBC battery aluminum paste a1 is composed of 75 parts of aluminum powder, 0.03 parts of boron powder, 1.3 parts of glass powder, 0.04 parts of fumed silica, 23.28 parts of organic binder and 0.35 parts of organic additive;
[0073] Among them, the above-mentioned organic auxiliary agent is lauryl phosphate; the aluminum powder includes micron spherical aluminum powder with a purity of 3 nines and a mass fraction of 92%, and nano spherical aluminum powder with a purity of 3 nines and a mass fraction of 8%; the organic binder includes ethyl cellulose-N100 with a mass fraction of 7% and an organic solvent with a mass fraction of 93%, and the organic solvent includes butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester.
[0074] (2) After forming a silicon oxide layer and a polysilicon layer on the back of the P-type silicon wafer, phosphorus is doped into the back polysilicon layer;
[0075] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;
[0076] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the aluminum paste a1 is screen-printed with 360 mesh in the laser groove that is connected to the p+ doped region to form a positive electrode grid line, and a silver paste negative electrode grid line is printed on the back silicon nitride layer that is opposite to the n+ doped region;
[0077] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 788° C., to produce an IBC battery.
[0078] After sintering, the electrical properties tested were: open circuit voltage of 0.722V, short circuit current of 13.915A, fill factor of 82.55%, photoelectric conversion efficiency of 25.12%, and warpage of 0.3mm lower than that of conventional aluminum paste.
[0079] Example 2
[0080] (1) Providing silver aluminum paste a2: In parts by mass, the IBC battery aluminum paste a2 is composed of 77 parts of aluminum powder, 0.08 parts of boron powder, 1.5 parts of glass powder, 0.06 parts of fumed silica, 20.86 parts of organic binder and 0.5 parts of organic additive;
[0081] Among them, the above-mentioned organic auxiliary agent is lauryl alcohol phosphate; the aluminum powder includes micron spherical aluminum powder with a purity of 3 nines and a mass fraction of 93%, and nano spherical aluminum powder with a purity of 3 nines and a mass fraction of 7%; the organic binder includes ethyl cellulose-N100 with a mass fraction of 8% and an organic solvent with a mass fraction of 92%, and the organic solvent includes butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.
[0082] (2) After forming a silicon oxide layer and a polysilicon layer on the back of the P-type silicon wafer, phosphorus is doped into the back polysilicon layer;
[0083] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;
[0084] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the aluminum paste a2 is screen-printed with 360 mesh in the laser groove that is connected to the p+ doped region to form a positive electrode grid line, and a silver paste negative electrode grid line is printed on the back silicon nitride layer that is opposite to the n+ doped region;
[0085] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 782° C., to produce an IBC battery.
[0086] After sintering, the electrical properties tested were: open circuit voltage of 0.721V, short circuit current of 13.905A, fill factor of 82.45%, photoelectric conversion efficiency of 25.037%, and warpage of 0.4mm lower than that of conventional aluminum paste.
[0087] Example 3
[0088] (1) Providing silver aluminum paste a3: In parts by mass, the IBC battery aluminum paste a3 is composed of 72 parts of aluminum powder, 0.1 parts of boron powder, 1.5 parts of glass powder, 0.06 parts of fumed silica, 25.74 parts of organic binder and 0.6 parts of organic additive;
[0089] Among them, the above-mentioned organic auxiliary agent is lauryl phosphate; the aluminum powder includes micron spherical aluminum powder with a purity of 3 nines and a mass fraction of 92%, and nano spherical aluminum powder with a purity of 3 nines and a mass fraction of 8%; the organic binder includes ethyl cellulose-N100 with a mass fraction of 7% and an organic solvent with a mass fraction of 93%, and the organic solvent includes butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.
[0090] (2) After forming a silicon oxide layer and a polysilicon layer on the back of the P-type silicon wafer, phosphorus is doped into the back polysilicon layer;
[0091] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;
[0092] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the aluminum paste a3 is screen-printed with 360 mesh in the laser groove that is connected to the p+ doped region to form a positive electrode grid line, and a silver paste negative electrode grid line is printed on the back silicon nitride layer that is opposite to the n+ doped region;
[0093] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 782° C., to produce an IBC battery.
[0094] After sintering, the electrical properties tested were: open circuit voltage of 0.719, short circuit current of 13.854A, fill factor of 83.45%, photoelectric conversion efficiency of 25.161%, and warpage of 0.48mm lower than that of conventional aluminum paste.
[0095] Example 4
[0096] (1) Providing silver aluminum paste a4: In parts by mass, the IBC battery aluminum paste a4 is composed of 77 parts of aluminum powder, 0.04 parts of boron powder, 1 part of glass powder, 0.03 parts of fumed silica, 21.73 parts of organic binder and 0.2 parts of organic additive;
[0097] Among them, the above-mentioned organic auxiliary agent is lauryl phosphate; the aluminum powder includes micron spherical aluminum powder with a purity of 3 nines and a mass fraction of 92%, and nano spherical aluminum powder with a purity of 3 nines and a mass fraction of 8%; the organic binder includes ethyl cellulose-N100 with a mass fraction of 7% and an organic solvent with a mass fraction of 93%, and the organic solvent includes butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.
[0098] (2) After forming a silicon oxide layer and a polysilicon layer on the back of the P-type silicon wafer, phosphorus is doped into the back polysilicon layer;
[0099] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;
[0100] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the aluminum paste a4 is screen-printed with 360 mesh in the laser groove that is connected to the p+ doped region to form a positive electrode grid line, and a silver paste negative electrode grid line is printed on the back silicon nitride layer that is opposite to the n+ doped region;
[0101] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 782° C., to produce an IBC battery.
[0102] After sintering, the electrical properties tested were: open circuit voltage of 0.720V, short circuit current of 13.845A, fill factor of 83.451%, photoelectric conversion efficiency of 25.197%, and warpage of 0.45mm lower than that of conventional aluminum paste.
[0103] Comparative Example 1
[0104] (1) Providing silver aluminum paste b1: In parts by mass, the IBC battery aluminum paste b1 is composed of 77.06 parts of aluminum powder, 0.08 parts of boron powder, 1.5 parts of glass powder, 20.86 parts of organic binder and 0.5 parts of organic additive;
[0105] Among them, the above-mentioned organic auxiliary agent is lauryl phosphate; the aluminum powder includes micron spherical aluminum powder with a purity of 3 nines and a mass fraction of 92%, and nano spherical aluminum powder with a purity of 3 nines and a mass fraction of 8%; the organic binder includes ethyl cellulose-N100 with a mass fraction of 7% and an organic solvent with a mass fraction of 93%, and the organic solvent includes butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.
[0106] (2) After forming a silicon oxide layer and a polysilicon layer on the back of the P-type silicon wafer, phosphorus is doped into the back polysilicon layer;
[0107] (3) laser grooving the back side of the phosphorus-doped P-type silicon wafer to form interdigitated n+ doped regions and p+ doped regions, and removing the front polysilicon layer;
[0108] (4) After removing the front polysilicon layer and sequentially forming a double-sided aluminum oxide layer, a front silicon nitride layer, and a back silicon nitride layer, the positive electrode grid line is formed by screen printing the above aluminum paste b1 in the laser groove connected to the p+ doped area through 360 mesh, and the silver paste negative electrode grid line is printed on the back silicon nitride opposite to the n+ doped area;
[0109] (5) The silicon wafer is sintered at a high temperature in a sintering furnace, with a peak sintering temperature of 782° C., to produce an IBC battery.
[0110] After sintering, the electrical properties tested were: open circuit voltage of 0.7195V, short circuit current of 13.855A, fill factor of 83.31%, photoelectric conversion efficiency of 25.154%, and warpage of 0.65mm.
[0111] By comparing Examples 1 to 4 with Comparative Example 1, it can be seen that by forming the P+ emitter using aluminum paste doped with gas phase silicon dioxide, the warpage can be reduced by more than 0.45 mm while maintaining the battery efficiency.
[0112] To summarize, in this embodiment, by adding fumed silica to the aluminum paste, during the process of the aluminum paste forming a fine grid, the fumed silica can be evenly distributed around the aluminum powder, preventing the aluminum powder from melting into each other and the aluminum powder from combining with each other under cooling conditions, thereby reducing the warping of the IBC battery after sintering, thereby solving the problem that the existing IBC battery aluminum paste is prone to warping when printing the positive electrode grid line, causing hidden cracks in the battery cell.
[0113] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concept. Therefore, the claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.
[0114] The above is a detailed introduction to an IBC battery aluminum paste and a preparation method thereof, and an IBC battery provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea; at the same time, for a person skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.
Claims
1. An IBC battery aluminum paste, characterized in that: The components constituting the aluminum paste include aluminum powder, boron powder, glass powder, fumed silica, organic binder and organic additive.
2. The IBC battery aluminum paste according to claim 1, characterized in that: In the aluminum paste, the mass percentage of the aluminum powder is 72-77%; the mass percentage of the boron powder is 0.04-0.1%; the mass percentage of the glass powder is 1-1.5%; the mass percentage of the fumed silica is 0.03-0.06%; the mass percentage of the organic binder is 20.74-25.74%; and the mass percentage of the organic additive is 0.2-0.6%.
3. The IBC battery aluminum paste according to claim 1, characterized in that: The fumed silica includes nano-scale fumed silica.
4. The IBC battery aluminum paste according to claim 1, characterized in that: The organic auxiliary agent includes one or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl alcohol phosphate, Digo 655, and BYK110.
5. The IBC battery aluminum paste according to claim 1, characterized in that: The aluminum powder includes micron spherical aluminum powder and nano spherical aluminum powder.
6. The IBC battery aluminum paste according to claim 1, characterized in that: The organic binder includes a high molecular polymer resin and an organic solvent; The mass fraction of the high molecular weight polymer in the organic binder is 6 to 8%; The mass fraction of the organic solvent in the organic binder is 92-94%.
7. The IBC battery aluminum paste according to claim 1, characterized in that: The organic solvent includes at least four of benzyl alcohol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester dodecahydrate.
8. The IBC battery aluminum paste according to claim 1, characterized in that: In parts by mass, the glass powder is obtained by sintering and crushing 3 to 15 parts of SiO2, 1 to 15 parts of Bi2O3, 35 to 80 parts of PbO, 0.5 to 5 parts of TiO2, 0.5 to 5 parts of Al2O3, 0.5 to 10 parts of ZnO, 0.5 to 3 parts of MgO, 0.5 to 5 parts of V2O5, and 0.5 to 3 parts of Li2O.
9. A method for preparing IBC battery aluminum paste, characterized in that: include: mixing an organic binder, boron powder, aluminum powder, fumed silica and glass powder to obtain a mixture; After the mixture is ground, an organic additive is added to obtain IBC battery aluminum paste.
10. An IBC battery, characterized in that: A plurality of positive grid lines are attached to the back of the IBC battery, and the grid lines are prepared from the aluminum paste described in any one of claims 1 to 8.
Citation Information
Patent Citations
Aluminium powder for aluminium slurry of crystalline silicon solar battery, preparation method thereof, and solar battery containing aluminium powder
CN104157330A
Solar back field aluminum slurry applied to double-sided PERC battery process and preparation method thereof
CN109698039A
Aluminum paste material for crystalline silicon photovoltaic cell and preparation method
CN110033876A
High-performance solar front conductive silver paste and preparation method thereof
CN112825276A