Insulator for high-insulation antenna and preparation process thereof
The vacuum dipping process combines the vacuum dipping tube sheet and the polytetrafluoroethylene anti-corrosion layer to form an air gap insulator, which solves the problems of sintered porcelain insulators' insulation performance degradation and acid-base corrosion under high water pressure, and achieves efficient insulation performance. and corrosion resistance.
Patent Information
- Application Number
- CN202411025917.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-12
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-25
AI Technical Summary
Existing sintered porcelain insulators cannot maintain insulation performance under high water pressure, and their resistance to acid and alkali corrosion is insufficient.
The vacuum dipping process is used to combine the vacuum dipping tube, vacuum dipping plate and polytetrafluoroethylene anti-corrosion layer to form an insulator without air gaps and holes. The inert properties of polytetrafluoroethylene are used to improve the acid and alkali corrosion resistance.
It achieves the reliability of insulation performance under high temperature, high pressure and acid and alkali environments, prevents moisture penetration, and significantly improves the acid and alkali corrosion resistance of insulators.
Smart Images

Figure CN118841226A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of insulators and processing thereof, in particular to an insulator for a high-insulation antenna and a preparation process thereof. Background Art
[0002] The insulator is an important part of the antenna. It is located at the root of the antenna body. It is the supporting part of the antenna body, and it is also the channel for insulating the inner and outer conductors of the antenna and connecting the antenna. It is a key part of the entire antenna structure and needs to have good strength, insulation performance and acid and alkali corrosion resistance. The existing insulator is a sintered porcelain insulator.
[0003] However, porcelain insulators have the following disadvantages: due to water penetration under high water pressure, the product cannot achieve insulation. Summary of the invention
[0004] The object of the present invention is to provide an insulator for a high-insulation antenna and a preparation process thereof, so as to solve the problems raised in the above background technology.
[0005] To achieve the above objectives, the present invention provides the following technical solutions: an insulator for a high-insulation antenna, comprising a pressure-bearing tube, a pressure-bearing plate and an anti-corrosion layer, wherein the outer surface of the pressure-bearing tube is provided with a pressure-bearing plate, and the outer surface of the pressure-bearing plate is provided with an anti-corrosion layer.
[0006] Preferably, the pressure-bearing tube is a vacuum-impregnated rubber tube.
[0007] Preferably, the pressure-bearing plate is a vacuum impregnated plate.
[0008] Preferably, the anti-corrosion layer is a polytetrafluoroethylene sleeve.
[0009] A preparation process of an insulator for a high-insulation antenna comprises the following steps:
[0010] Step 1: Processing the pressure pipe;
[0011] Step 2: Processing the pressure plate;
[0012] Step 3: Processing the anti-corrosion layer;
[0013] Step 4: Vacuum pressure dipping: specifically including the following steps:
[0014] 1) Assemble the processed pressure-bearing pipe, pressure-bearing plate and anti-corrosion layer and put them into the vacuum box, then put the vacuum box into the oven and start heating. When the temperature rises to 110-130℃, keep it warm for 2hr±10min. During the insulation process, connect the vacuum pipeline and rubber pipeline;
[0015] 2) When the insulation is finished, adjust the mold temperature control setting to 75-85℃ and start evacuation: the system vacuum degree reaches 0.5-5Pa, and the vacuum drying time is 3hr±10min;
[0016] 3) Degassing of the adhesive liquid is an operation process that is carried out 2-3 hours before glue delivery, and is carried out simultaneously with the heat preservation and vacuum drying of the tube blank. The degassing of the adhesive liquid is carried out in the degassing tank, including three processes: adhesive liquid preparation, degassing in the tank, and entering the pressure tank;
[0017] Add the prepared solvent-free resin glue into the degassing tank. The temperature of the degassing tank is set to 50-56℃, which is closer to the lower limit in summer and closer to the upper limit in winter. The vacuum degree in the tank is controlled below 100Pa, and the degassing is carried out for 2hr±0.5hr.
[0018] After degassing, transfer the glue solution into a pre-vacuumed pressure tank and degas under vacuum below 100Pa for 0.5hr for standby use;
[0019] 4) After vacuum drying, slowly open the glue feeding clamp on the rubber tube at the glue inlet end of the mold and the glue outlet valve of the pressure tank, and uniformly feed glue at a flow rate of 10s / 1cm; during the glue feeding process, the mold temperature is controlled at 75-85℃, the system vacuum degree is 0.5-5Pa, and the vacuum glue feeding time is controlled within 1.5±0.5hr;
[0020] 5) The pressure tank is pressurized with N2 at a rate of 0.1 MPa / 10 min, and the final pressure is 0.5-1.0 MPa;
[0021] 6) When glue overflows from the overflow port, close the valve at the glue outlet of the tube mold, release the vacuum, and end the glue feeding. At the same time, the pressure tank is pressurized with N2 to maintain 0.5-1.0MPa, the mold temperature is controlled at 75-85℃, and the pressure holding time is 2.5±0.5hr. The total glue feeding time and pressure holding time are required to be no less than 4hr;
[0022] 7) After the pressure is maintained, the mold is heated and solidified: the mold is heated to 125°C in 25±5 minutes, and kept at 125±5°C for 1hr±10min;
[0023] 8) After the 125℃ heat preservation, the temperature is raised in two steps: the mold is heated to 160℃ for 10±5min and then kept at 160℃ for 5hrs;
[0024] 9) After the insulation is completed, the N2 pressure is removed and the temperature begins to drop. Within 30-45 minutes, the mold temperature drops below 90°C and is ready for demolding;
[0025] Step 5: Machining: According to the product size requirements, the composite blank is machined to the product size.
[0026] Preferably, the processing of the pressure-bearing pipe in step 1 is specifically to cut the φ41 / φ51 vacuum-impregnated pipe into a length of 121 mm, and grind the outer surface with 320-grade sandpaper until there is no reflective surface.
[0027] Preferably, the processing of the pressure plate in step 2 is specifically to process the 124 mm vacuum impregnated board into a truncated cone.
[0028] Preferably, the processing of the anti-corrosion layer in step three is specifically to activate the inner surface of the conical tube processed by using a polytetrafluoroethylene rod.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The present invention adopts a vacuum impregnation plate, a vacuum impregnation tube, and a polytetrafluoroethylene tube. After the three materials are pre-assembled and formed, the three materials are compounded together without air gaps through a vacuum impregnation process. The reliability of the insulation performance of the insulator under high temperature, high pressure and acid and alkali corrosion conditions during use is effectively solved. In addition, the present invention is made by a vacuum pressure impregnation molding process, which effectively realizes that the insulator has no air gaps and no holes, and achieves the purpose of preventing water from penetrating into the insulator under high water pressure. The use of polytetrafluoroethylene on the outside of the insulator also effectively isolates the infiltration of moisture. Due to the inert characteristics of polytetrafluoroethylene, the acid and alkali corrosion resistance of the insulator is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the blank structure of the insulator of the present invention;
[0032] Figure 2 This is a schematic diagram of the finished product structure of the insulator of the present invention;
[0033] Figure 3 It is a structural schematic diagram of the pressure-bearing pipe of the present invention;
[0034] Figure 4 It is a structural schematic diagram of the pressure plate of the present invention;
[0035] Figure 5 It is a schematic diagram of the structure of the anti-corrosion layer of the present invention.
[0036] In the figure: 1. Pressure pipe; 2. Pressure plate; 3. Anti-corrosion layer. DETAILED DESCRIPTION
[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0038] See also Figure 1-5The present invention provides an insulator for a high-insulation antenna, comprising a pressure-bearing tube 1, a pressure-bearing plate 2 and an anti-corrosion layer 3. The pressure-bearing tube 1 is provided with a pressure-bearing plate 2 on its outer surface, and the pressure-bearing plate 2 is provided with an anti-corrosion layer 3 on its outer surface. The pressure-bearing tube 1 is a vacuum-impregnated rubber tube, which has a function of resisting lateral pressure; the pressure-bearing plate 2 is a vacuum-impregnated rubber plate, which has a function of resisting longitudinal pressure; the anti-corrosion layer 3 is a polytetrafluoroethylene sleeve, which has a function of resisting acid and alkali corrosion.
[0039] A preparation process of an insulator for a high-insulation antenna comprises the following steps:
[0040] Step 1: Process the pressure pipe 1: Cut the φ41 / φ51 vacuum impregnated pipe to a length of 121mm, and polish the outer surface with 320 sandpaper until it has no reflective surface, see attached Figure 3 ;
[0041] Step 2: Process the pressure plate 2: Process the 124mm vacuum impregnated plate into a truncated cone, see attached Figure 4 ;
[0042] Step 3: Process the anti-corrosion layer 3: Use polytetrafluoroethylene rod to process into a conical tube, see attached Figure 5 , inner surface activation treatment;
[0043] Step 4: Vacuum pressure dipping: specifically including the following steps:
[0044] 1) Assemble the processed pressure pipe 1, pressure plate 2 and anti-corrosion layer 3 and put them into the vacuum box, then put the vacuum box into the oven and start heating. When the temperature rises to 110-130℃, keep it warm for 2hr±10min. During the insulation process, connect the vacuum pipeline and rubber pipeline;
[0045] 2) When the insulation is finished, adjust the mold temperature control setting to 75-85℃ and start evacuation: the system vacuum degree reaches 0.5-5Pa, and the vacuum drying time is 3hr±10min;
[0046] 3) Degassing of the adhesive liquid is an operation process that is carried out 2-3 hours before glue delivery, and is carried out simultaneously with the heat preservation and vacuum drying of the tube blank. The degassing of the adhesive liquid is carried out in the degassing tank, including three processes: adhesive liquid preparation, degassing in the tank, and entering the pressure tank;
[0047] Add the prepared solvent-free resin glue into the degassing tank. The temperature of the degassing tank is set to 50-56℃, which is closer to the lower limit in summer and closer to the upper limit in winter. The vacuum degree in the tank is controlled below 100Pa, and the degassing is carried out for 2hr±0.5hr.
[0048] After degassing, transfer the glue solution into a pre-evacuated pressure tank (temperature control setting is the same as the degassing tank), degas under vacuum below 100Pa for 0.5hr, and set aside;
[0049] 4) After vacuum drying, slowly open the glue delivery clamp on the rubber tube at the mold inlet end and the glue outlet valve of the pressure tank, and deliver glue at a uniform speed of 10s / 1cm (glass tube with inner diameter Φ9mm); during the glue delivery process, the mold temperature is controlled at 75-85℃ (same as vacuum drying), the system vacuum degree is 0.5-5Pa, and the vacuum glue delivery time is controlled within 1.5±0.5hr;
[0050] 5) The pressure tank is pressurized with N2 at a rate of 0.1 MPa / 10 min, and the final pressure is 0.5-1.0 MPa;
[0051] 6) When glue overflows from the overflow port, close the valve at the glue outlet of the tube mold, release the vacuum, and end the glue feeding. At the same time, the pressure tank is pressurized with N2 to maintain 0.5-1.0MPa, the mold temperature is controlled at 75-85℃ (same as vacuum glue feeding), and the pressure holding time is 2.5±0.5hr. The glue feeding time and pressure holding time are required to be no less than 4hr in total;
[0052] 7) After the pressure is maintained, the mold is heated and solidified: the mold is heated to 125°C in 25±5 minutes, and kept at 125±5°C for 1hr±10min;
[0053] 8) After the 125℃ heat preservation, the temperature is raised in two steps: the mold is heated to 160℃ for 10±5min and then kept at 160℃ for 5hrs;
[0054] 9) After the insulation is completed, the N2 pressure is removed and the temperature begins to drop. Within 30-45 minutes, the mold temperature drops below 90°C and is ready for demolding;
[0055] Step 5: Machining: According to the product size requirements, the composite blank (see attached Figure 1 ) Machining to product size (see attached Figure 2 ).
[0056] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An insulator for a high insulation antenna, characterized in that: It comprises a pressure-bearing pipe (1), a pressure-bearing plate (2) and an anti-corrosion layer (3); the outer surface of the pressure-bearing pipe (1) is provided with a pressure-bearing plate (2), and the outer surface of the pressure-bearing plate (2) is provided with an anti-corrosion layer (3).
2. The insulator for high insulation antenna according to claim 1, characterized in that: The pressure-bearing pipe (1) is a vacuum rubber-impregnated pipe.
3. The insulator for a high insulation antenna according to claim 1, characterized in that: The pressure-bearing plate (2) is a vacuum-impregnated plate.
4. The insulator for a high insulation antenna according to claim 1, characterized in that: The anti-corrosion layer (3) is a polytetrafluoroethylene sleeve.
5. A process for preparing an insulator for a high insulation antenna according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1: Processing a pressure pipe (1); Step 2: Processing the pressure plate (2); Step 3: Processing the anti-corrosion layer (3); Step 4: Vacuum pressure dipping: specifically including the following steps: 1) Assemble the processed pressure-bearing pipe (1), pressure-bearing plate (2) and anti-corrosion layer (3) and put them into a vacuum box, then put the vacuum box into an oven and start heating. When the temperature rises to 110-130°C, keep it warm for 2hr±10min. During the insulation process, connect the vacuum pipeline and the rubber delivery pipeline; 2) When the insulation is finished, adjust the mold temperature control setting to 75-85℃ and start evacuation: the system vacuum degree reaches 0.5-5Pa, and the vacuum drying time is 3hr±10min; 3) Degassing of the adhesive liquid is an operation process that is carried out 2-3 hours before glue delivery, and is carried out simultaneously with the heat preservation and vacuum drying of the tube blank. The degassing of the adhesive liquid is carried out in the degassing tank, including three processes: adhesive liquid preparation, degassing in the tank, and entering the pressure tank; Add the prepared solvent-free resin glue into the degassing tank. The temperature of the degassing tank is set to 50-56℃, which is closer to the lower limit in summer and closer to the upper limit in winter. The vacuum degree in the tank is controlled below 100Pa, and the degassing is carried out for 2hr±0.5hr. After degassing, transfer the glue solution into a pre-vacuumed pressure tank and degas under vacuum below 100Pa for 0.5hr for standby use; 4) After vacuum drying, slowly open the glue feeding clamp on the rubber tube at the glue inlet end of the mold and the glue outlet valve of the pressure tank, and uniformly feed glue at a flow rate of 10s / 1cm; during the glue feeding process, the mold temperature is controlled at 75-85℃, the system vacuum degree is 0.5-5Pa, and the vacuum glue feeding time is controlled within 1.5±0.5hr; 5) The pressure tank is pressurized with N2 at a rate of 0.1 MPa / 10 min, and the final pressure is 0.5-1.0 MPa; 6) When glue overflows from the overflow port, close the valve at the glue outlet of the tube mold, release the vacuum, and end the glue feeding. At the same time, the pressure tank is pressurized with N2 to maintain 0.5-1.0MPa, the mold temperature is controlled at 75-85℃, and the pressure holding time is 2.5±0.5hr. The total glue feeding time and pressure holding time are required to be no less than 4hr; 7) After the pressure is maintained, the mold is heated and solidified: the mold is heated to 125°C in 25±5 minutes, and kept at 125±5°C for 1hr±10min; 8) After the 125℃ heat preservation, the temperature is raised in two steps: the mold is heated to 160℃ for 10±5min and then kept at 160℃ for 5hrs; 9) After the insulation is completed, the N2 pressure is removed and the temperature begins to drop. Within 30-45 minutes, the mold temperature drops below 90°C and is ready for demolding; Step 5: Machining: According to the product size requirements, the composite blank is machined to the product size.
6. The process for preparing an insulator for a high-insulation antenna according to claim 5, characterized in that: The processing of the pressure-bearing pipe (1) in the step 1 specifically includes cutting the φ41 / φ51 vacuum-impregnated pipe into a length of 121 mm, and grinding the outer surface with 320-grade sandpaper until there is no reflective surface.
7. The process for preparing an insulator for a high-insulation antenna according to claim 5, characterized in that: The processing of the pressure plate (2) in step 2 specifically involves processing the 124 mm vacuum impregnated plate into a truncated cone.
8. The process for preparing an insulator for a high-insulation antenna according to claim 5, characterized in that: The processing of the anti-corrosion layer (3) in the step 3 is specifically to use a polytetrafluoroethylene rod to process the inner surface of the conical tube for activation treatment.