A kind of medical dressing for quick hemostasis and preparation method thereof

In the preparation process of medical dressings, the combination of seaweed fiber and dandelion villi fiber, combined with image analysis and hydrospinning pressure adjustment technology, the problem of insufficient hemostatic performance of traditional dressings is solved, and the surface density and tensile resistance of the dressings are improved. , enhances the hemostatic effect.

CN118846186BActive Publication Date: 2024-11-22CHANGSHA WEIZE MEDICAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411329435.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-22
Estimated Expiration
2044-09-24

AI Technical Summary

Technical Problem

Traditional medical dressings have shortcomings in hemostasis performance, and insufficient hydrospinning pressure in the hydrospinning process will lead to incomplete curing of the non-woven substrate, affecting surface density, tensile resistance and tear resistance.

Method used

By adding sulfonamide to the aqueous sodium alginate solution, seaweed fibers are obtained and mixed with dandelion velvet fibers and adhesive fibers, fiber cloth images are collected during hydrospuncture treatment, fiber interweaving loose coefficient and hydrospuncture feedback strength are analyzed, and water is adjusted The pressure is pricked to ensure the fibers are interwoven tightly, and the composite sol is then coated for vacuum and hot rolling.

Benefits of technology

The surface density, tensile and tear resistance of the composite fiber non-woven substrate is improved, thereby enhancing the hemostatic performance of medical dressings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118846186B_ABST
    Figure CN118846186B_ABST
Patent Text Reader

Abstract

The present application relates to the field of medical dressings, and specifically to a medical dressing for rapid hemostasis and a preparation method thereof, the method comprising: adding sulfonamide drugs into a sodium alginate aqueous solution to obtain a sodium alginate / sulfonamide aqueous solution, performing vacuum degassing to obtain a spinning solution; the spinning solution is sprayed out in a calcium chloride solution and solidified into seaweed fibers, and seaweed staple fibers are obtained after being cut and dried; seaweed staple fibers, dandelion fluff fibers, and adhesive fibers are mixed, opened, and combed, and then laid and pressed into fiber cloth; the fiber cloth is transported to a spunlace machine for spunlace treatment, and then dried to obtain a composite fiber non-woven fabric substrate, and the spunlace pressure during the spunlace treatment is feedback-adjusted to obtain a composite sol; the composite sol is coated on the composite fiber non-woven fabric substrate, and vacuum treatment and hot rolling treatment are performed to obtain an initial dressing, and after drying and sterilization, a medical dressing is obtained. Thus, the hemostatic effect of the medical dressing is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of medical dressings, and in particular to a medical dressing for rapid hemostasis and a preparation method thereof. Background Art

[0002] As a layer of covering on the surface of skin wounds, medical dressings usually have properties such as elasticity, permeability and water absorption, providing protection and a suitable microenvironment for the wounds. At the same time, they also need to have biological properties such as hemostasis and antibacterial properties to improve the ability of wound healing. Traditional dressings such as natural gauze can quickly absorb exudate on the surface of the wound, and the production process is simple and easy to implement, but the permeability is too high and the risk of cross infection is high; modern dressings can provide a better wound healing environment. For example, hydrogel dressings are comfortable, but have poor viscosity and need to be fixed, and are prone to forming "fish eyes". Therefore, a medical dressing that can quickly stop bleeding is needed.

[0003] At present, in the preparation process of medical dressings, the hydroentanglement process uses the continuous injection of high-pressure water from the hydroentanglement head to generate hydraulic effects, causing the fibers of the non-woven fabric substrate to begin to move and rearrange, and interweave with each other to achieve the solidification of the non-woven fabric substrate. However, if the hydroentanglement pressure during the hydroentanglement process is insufficient, it is easy to cause incomplete solidification of the non-woven fabric substrate and low strength, and also greatly affect the surface density of the non-woven fabric substrate, as well as its tensile and tear resistance, further affecting the hemostatic performance of the medical dressing. Summary of the invention

[0004] In order to solve the above technical problems, the purpose of this application is to provide a medical dressing for rapid hemostasis and a preparation method thereof. The technical solutions adopted are as follows:

[0005] In a first aspect, an embodiment of the present application provides a method for preparing a medical dressing for rapid hemostasis, the method comprising the following steps:

[0006] Adding sulfonamide into the sodium alginate aqueous solution to obtain a sodium alginate / sulfonamide aqueous solution;

[0007] The sodium alginate / sulfonamide aqueous solution is pumped into the spinning kettle for vacuum degassing to obtain the spinning solution;

[0008] The spinning solution is sent into a coagulation bath, the spinning solution is sprayed out in a calcium chloride solution and solidified into seaweed fibers, and the seaweed short fibers are obtained after being cut and dried;

[0009] The seaweed staple fiber, dandelion fluff fiber and viscose fiber are mixed, opened and combed, and then laid out and pressed into a fiber cloth;

[0010] After the fiber cloth is transported to the spunlacing machine for spunlacing treatment, it is dried to obtain a composite fiber nonwoven fabric substrate, and the spunlacing pressure during the spunlacing treatment is feedback-adjusted, specifically:

[0011] (1) Collect images of the composite fiber non-woven fabric substrate at each time in each time period and extract the foreground image at each time; analyze the deformation degree of the fiber mesh pores corresponding to each connected domain in the foreground image and the probability of adjacent fiber mesh pores to determine the fiber interweaving loose coefficient of each connected domain in the foreground image;

[0012] (2) performing threshold segmentation based on the fiber interweaving loose coefficient, taking each connected domain whose fiber interweaving loose coefficient is greater than the segmentation threshold as each fiber sparse area; dividing the foreground image at each moment into each horizontal interval, analyzing the distribution of the fiber sparse area in each horizontal interval, and obtaining the water entanglement feedback intensity of each horizontal interval at each moment;

[0013] (3) adjusting the water jet pressure in the next time period of each time period based on the difference between the water jet feedback intensity and a preset adjustment threshold and in combination with the water jet pressure in each time period;

[0014] The composite sol is obtained by using raw materials of hydroxybutyl chitosan, acetic acid solution, cross-linking agent and anti-inflammatory agent;

[0015] The composite sol is coated on the composite fiber non-woven fabric substrate, and vacuum treatment and hot rolling treatment are performed to obtain the initial dressing, and after drying and sterilization, the medical dressing is obtained.

[0016] In one embodiment, the sodium alginate / sulfonamide aqueous solution is obtained by:

[0017] The concentration of sodium alginate in the sodium alginate aqueous solution is 2-5wt%, sulfonamide is added to the sodium alginate aqueous solution until the sulfonamide concentration is 2-10wt%, and stirred for 30-40 minutes to obtain a sodium alginate / sulfonamide aqueous solution;

[0018] The vacuum degassing conditions are -0.09MPa~-0.1MPa, and the duration is 30~50min.

[0019] In one embodiment, the preparation of the dandelion fluff fiber includes:

[0020] The dandelion fluff is put into a sodium bicarbonate solution for ultrasonic activation treatment, and then the ultrasonically activated dandelion fluff is washed with deionized water until the washing solution is neutral, and then the dandelion fluff fiber is obtained after drying.

[0021] In one of the embodiments, the mass ratio of the seaweed staple fiber, dandelion fluff fiber, and viscose fiber is 3:3:4; the hydroentanglement pressure of the hydroentanglement treatment is 2.2~4MPa, and the feed and discharge speed is 12~15m / min; the drying temperature is 80°C, and the drying time is 2~5min.

[0022] In one embodiment, the process of determining the fiber interlacing looseness coefficient is as follows:

[0023] Calculate the fractal dimension of each connected domain contour in the foreground image, obtain the standard fractal dimension of each connected domain contour in the standard foreground image, and use the average of the differences between the fractal dimension of each connected domain contour in the foreground image and the standard fractal dimension of all connected domain contours in the standard foreground image as the degree of fiber web gap deformation of each connected domain in the foreground image;

[0024] Calculate the mean of the number of pixels in all connected domains in the standard foreground image, calculate the ratio of the number of pixels in each connected domain in the foreground image to the mean, calculate the chaos degree of the metric distance from multiple pixels on the contour of each connected domain in the foreground image to the centroid of the connected domain, and use the normalized value of the product of the ratio and the chaos degree as the probability of fiber web gap connection of each connected domain in the foreground image;

[0025] The fiber interlacing looseness coefficient is the product of the deformation degree of the fiber web gaps and the probability of the fiber web gaps being connected.

[0026] In one embodiment, the process of determining the water spurt feedback intensity is as follows:

[0027] For each transverse interval, if the centroid of a fiber sparse region in any transverse interval belongs to the any transverse interval, then the fiber sparse region belongs to the any transverse interval, and the sum of the fiber interlacing loose coefficients of all fiber sparse regions in each transverse interval is calculated as the interlacing unformed degree of each transverse interval;

[0028] Calculate the discrete degree of the ordinate of the centroid of all fiber sparse areas in each transverse interval as the fiber sparse area distribution distance in each transverse interval;

[0029] The water entanglement feedback intensity is positively correlated with the degree of interweaving unformation, and negatively correlated with the distribution distance of the fiber sparse area.

[0030] In one embodiment, the adjusting the water jet pressure in the next time period of each time period comprises:

[0031] The average of the water spurt feedback intensity at all times in each lateral interval in each time period is used as the pressure adjustment coefficient of each lateral interval in each time period. If the pressure adjustment coefficient of lateral interval a in the t-th time period is less than or equal to the preset adjustment threshold, the water spurt pressure of lateral interval a in the t+1-th time period is not adjusted. Otherwise, the water spurt adjustment value of lateral interval a in the t-th time period is The calculation method is:

[0032] ; In the formula, is the pressure adjustment coefficient of the horizontal interval a in the tth time period, To preset the adjustment threshold, is the mean value of the water jet pressure of all water jet heads in the column corresponding to the horizontal interval a in the tth time period;

[0033] The water jet pressure of all water jet heads corresponding to the transverse interval a in the t+1th time period is adjusted to the water jet adjustment value.

[0034] In one embodiment, the preparation of the composite sol comprises:

[0035] Put hydroxybutyl chitosan into 1-2% acetic acid solution, the content of hydroxybutyl chitosan is 4-10wt%, then put in a cross-linking agent, the content of the cross-linking agent is 5-15wt%, add an anti-inflammatory agent, the content of the anti-inflammatory agent is 0.5-1wt%, stir until it is completely dissolved to obtain a composite sol, wherein the stirring speed is 200-300r / min.

[0036] In one embodiment, the vacuum environment of the vacuum treatment is -0.09MPa~-0.1MPa, and the temperature of the hot rolling treatment is 50~70°C.

[0037] In a second aspect, an embodiment of the present application further provides a medical dressing for rapid hemostasis, wherein the medical dressing for rapid hemostasis is made by the above-mentioned method for preparing a medical dressing for rapid hemostasis.

[0038] This application has at least the following beneficial effects:

[0039] The present application collects images of the composite fiber nonwoven fabric substrate at each time moment in each time period through feedback adjustment of the hydroentanglement pressure during the hydroentanglement treatment process in the preparation of medical dressings, and extracts the foreground image at each time moment; analyzes the degree of deformation of the fiber mesh pores corresponding to each connected domain in the foreground image, and the probability of adjacent fiber mesh pores, and determines the fiber interweaving loose coefficient of each connected domain in the foreground image. The fiber interweaving loose coefficient reflects the sparseness of fiber interweaving of the fiber mesh corresponding to the connected domain, and has the beneficial effect of improving the accuracy of identifying fiber sparse areas, avoiding the problem that the structural characteristics of the fiber mesh caused by the hydroentanglement pressure are not obvious, and it is difficult to accurately judge the insufficient hydroentanglement pressure; further, threshold segmentation is performed based on the fiber interweaving loose coefficient, and each connected domain whose fiber interweaving loose coefficient is greater than the segmentation threshold is taken as each fiber sparse area, and the foreground image at each time moment is taken as the foreground image. The entanglement pressure of the entanglement head is accurately adjusted by feedback, and its beneficial effect lies in comprehensively analyzing the distribution characteristics of the fiber sparse area and eliminating the interference of accidental factors in the entanglement process. At the same time, according to the actual interweaving of the composite fiber non-woven fabric substrate, each column of the entanglement head can be accurately feedback controlled, thereby improving the refinement of the entanglement pressure control and ensuring the surface density and tensile and tear resistance of the composite fiber non-woven fabric substrate. Finally, based on the difference between the entanglement feedback intensity and the preset adjustment threshold, combined with the entanglement pressure in each time period, the entanglement pressure in the next time period of each time period is adjusted, thereby improving the quality of the composite fiber non-woven fabric substrate and further improving the hemostatic performance of the medical dressing. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the technical solutions and advantages in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0041] Figure 1 A flowchart of a method for preparing a medical dressing for rapid hemostasis provided in one embodiment of the present application;

[0042] Figure 2 This is a schematic diagram of image acquisition;

[0043] Figure 3 This is a schematic diagram of the light source installation position;

[0044] Figure 4 It is a schematic diagram of hydroentanglement treatment;

[0045] Figure 5 Non-woven fabric image for dressing;

[0046] Figure 6 is a foreground image of a dressing nonwoven fabric image;

[0047] Figure 7 Flow chart of hydroentanglement pressure adjustment for hydroentanglement treatment. DETAILED DESCRIPTION

[0048] In order to further explain the technical means and effects adopted by the present application to achieve the predetermined invention purpose, the following is a detailed description of a medical dressing for rapid hemostasis and its preparation method proposed in the present application, its specific implementation method, structure, features and effects, in conjunction with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "another embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics in one or more embodiments may be combined in any suitable form.

[0049] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs.

[0050] The specific scheme of a medical dressing for rapid hemostasis and a preparation method thereof provided by the present application is described in detail below in conjunction with the accompanying drawings.

[0051] See also Figure 1 , which shows a flowchart of a method for preparing a medical dressing for rapid hemostasis provided by an embodiment of the present application, the method comprising the following steps:

[0052] S1: In Example 1 of the present application, deionized water is first added to a stirred reactor, and sodium alginate is dissolved in the deionized water to obtain a sodium alginate aqueous solution, and stirred for 20 minutes, wherein the concentration of sodium alginate in the sodium alginate aqueous solution is 2wt%; sulfonamide is then added to the sodium alginate aqueous solution until the sulfonamide concentration is 2wt% to improve the antibacterial properties of the seaweed fiber, and stirred again for 30 minutes to obtain a sodium alginate / sulfonamide aqueous solution;

[0053] In Example 2 of the present application, deionized water is first added to a stirred reactor, and sodium alginate is dissolved in the deionized water to obtain a sodium alginate aqueous solution, which is stirred for 30 minutes, wherein the concentration of sodium alginate in the sodium alginate aqueous solution is 3wt%; sulfonamide is then added to the sodium alginate aqueous solution until the sulfonamide concentration is 6wt% to improve the antibacterial properties of the alginate fiber, and the solution is stirred again for 35 minutes to obtain a sodium alginate / sulfonamide aqueous solution;

[0054] In Example 3 of the present application, deionized water is first added to a stirred reactor, and sodium alginate is dissolved in the deionized water to obtain a sodium alginate aqueous solution, which is then stirred for 40 minutes, wherein the concentration of sodium alginate in the sodium alginate aqueous solution is 5wt%; sulfonamide is then added to the sodium alginate aqueous solution until the sulfonamide concentration is 10wt% to improve the antibacterial properties of the seaweed fiber, and the solution is stirred again for 40 minutes to obtain a sodium alginate / sulfonamide aqueous solution.

[0055] S2: The sodium alginate / sulfonamide aqueous solution is pumped into the spinning kettle by a pumping pump, and vacuum degassing is performed to obtain the spinning solution.

[0056] In Example 1 of the present application, the vacuum degassing condition is -0.09 MPa, and the vacuum degassing time is 30 min.

[0057] In Example 2 of the present application, the vacuum degassing condition is -0.1 MPa, and the vacuum degassing time is 40 min.

[0058] In Example 3 of the present application, the vacuum degassing condition is -0.1 MPa, and the vacuum degassing time is 50 min.

[0059] S3: The spinning solution is sent into a coagulation bath, and the spinning solution is sprayed out in a calcium chloride solution and solidified into seaweed fibers.

[0060] In Example 1 of the present application, the concentration of calcium chloride in the calcium chloride solution is 2 wt %.

[0061] In Example 2 of the present application, the concentration of calcium chloride in the calcium chloride solution is 3 wt %.

[0062] In Example 3 of the present application, the concentration of calcium chloride in the calcium chloride solution is 4 wt %.

[0063] S4: The seaweed fiber is stretched by a drafting roller assembly, cut by a water jet cutter, and finally dried by a dryer to obtain seaweed short fibers.

[0064] In Example 1 of the present application, the cutting length by the water jet cutting machine is 30 mm.

[0065] In Example 2 of the present application, the cutting length of the cutting by the water jet cutting machine is 40 mm.

[0066] In Example 3 of the present application, the cutting length by the water jet cutting machine is 45 mm.

[0067] S5: putting the dandelion fluff into a sodium bicarbonate solution for ultrasonic activation treatment, wherein the sodium bicarbonate solution has a solubility of 0.5 mol / L, and then washing the ultrasonically activated dandelion fluff with deionized water until the washing solution is neutral, and drying the dandelion fluff with a dryer to obtain dandelion fluff fibers.

[0068] S6: The seaweed staple fibers obtained in step S4, the dandelion fluff fibers obtained in step S5, and the viscose fibers are put into a mixing box in a mass ratio of 3:3:4 for uniform mixing, and then opened in a fine opener. The opened fibers are combed by a carding machine, and finally the combed fibers are sent to a web laying machine for web laying, and are pressed into fiber cloth by a drafting machine.

[0069] S7: In Example 1 of the present application, the fiber cloth is conveyed to a spunlace machine for spunlace treatment to obtain a composite fiber spunlace cloth, wherein the front and back sides are spunlace compounded twice each, the spunlace pressure ranges from 2.2 to 4 MPa, and the feed and discharge speed is 12 m / min. The composite fiber spunlace cloth is squeezed to dry water and dried in a dryer, wherein the drying temperature is 80°C and the drying time is 2 min, to obtain a composite fiber non-woven fabric substrate.

[0070] In Example 2 of the present application, the feeding and discharging speed may also be 14 m / min, and the drying time may also be 4 min.

[0071] In Example 3 of the present application, the feeding and discharging speed may also be 15 m / min, and the drying time may also be 5 min.

[0072] Based on the obtained composite fiber nonwoven fabric substrate, feedback adjustment is performed on the spunlace pressure of the spunlace machine during the spunlace treatment process. The specific adjustment process is as follows:

[0073] (1) Collect images of the composite fiber non-woven fabric substrate at each time in each time period and extract the foreground image at each time; analyze the deformation degree of the fiber mesh pores corresponding to each connected domain in the foreground image and the probability of adjacent fiber mesh pores to determine the fiber interweaving loose coefficient of each connected domain in the foreground image.

[0074] Hydroentanglement is a key step in the preparation of medical excipients. Increasing the hydroentanglement pressure will increase production energy consumption and production costs. The hydroentanglement pressure has a decisive influence on the surface density, porosity and air permeability of the composite fiber non-woven fabric substrate. Medical dressings have extremely high requirements for composite fiber non-woven fabric substrates, so this embodiment accurately adjusts the hydroentanglement pressure during the hydroentanglement process.

[0075] Place the bracket above the composite fiber non-woven fabric substrate conveyor belt, install a high-resolution camera on the bracket, and tilt the high-resolution camera 45 degrees to align it with the center line of the composite fiber non-woven fabric substrate to capture images of the composite fiber non-woven fabric substrate. The image capture diagram is shown in the figure. Figure 2 As shown, 1 is a composite fiber non-woven fabric substrate, 2 is a high-resolution camera, and 3 is a bracket; light sources are installed on both sides of the camera to ensure the lighting for image acquisition, so that the high-resolution camera can more effectively collect image information of the composite fiber non-woven fabric substrate. The schematic diagram of the light source installation position is shown in Figure 3 As shown, 2 is a high-resolution camera, 3 is a bracket, and 4 is light sources on both sides.

[0076] Set each time period and use a high-resolution camera to capture images of the composite fiber non-woven fabric substrate. In the embodiment of the present application, the acquisition time interval is 10s, which can be adjusted by the implementer according to the actual situation. This embodiment does not limit it. The images collected at each moment are grayed, and the grayed images are denoised by bilateral filtering. The denoised images are used as the dressing non-woven fabric image.

[0077] It should be noted that the implementer may select other existing feasible filtering algorithms for denoising, and this embodiment does not limit this.

[0078] The principle of hydroentanglement is that the fiber cloth enters the hydroentanglement treatment area through the support net curtain, and the hydroentanglement head generates hydraulic action through the high-pressure hydroentanglement jet of the water spray plate. Moreover, after the hydroentanglement penetrates the fiber cloth, it passes through the support net curtain and has reflections in different directions, causing the fiber cloth to be penetrated in different directions, causing the fibers arranged in the fiber cloth to begin to move, intersperse and rearrange, and interweave with each other. The schematic diagram of hydroentanglement is shown in the figure. Figure 4 As shown, 5 is a spunlacing head, 6 is a water spraying plate, 7 is a fiber cloth, 8 is a supporting roller, 9 is a supporting net curtain, 10 is a spunlacing jet, and 11 is a reflected water flow.

[0079] In the dressing non-woven fabric image, due to the large grayscale difference between the web fibers and the fiber gaps, this embodiment uses the dressing non-woven fabric image as the input of the Otsu method, takes the pixel points with grayscale values ​​less than the segmentation threshold as the foreground pixel points, and outputs the foreground image of the dressing non-woven fabric image. All connected domains in the foreground image at each moment are extracted through the eight-neighborhood connected domain, and the contour of each connected domain is extracted. Among them, the Otsu method and the connected domain extraction algorithm are both existing well-known technologies, and the implementer can also choose other algorithms according to the actual situation, which is not limited in this embodiment.

[0080] Dandelion fluff fibers and seaweed fibers are tiny. When the water spunlace pressure is too small, the entanglement between the fibers is not tight enough to completely press the fibers into the fiber web, which easily leads to a large number of fiber sparse areas in the dressing non-woven fabric image. The fibers in the fiber sparse areas are not tightly interwoven. In the dressing non-woven fabric image, the fibers around the fiber web gaps are loose, resulting in large differences in the morphological characteristics of the fiber web gaps. Moreover, since the fiber sparse areas correspond to fewer fibers and a smaller surface density, the grayscale values ​​of the fiber web fibers in the corresponding collected images are relatively low, and the contrast with the fiber web gaps is relatively small. The connected domains of different fiber web gaps may stick together, such as Figure 5 , Figure 6 As shown, Figure 5 For dressing nonwoven fabric images, Figure 6 The foreground image is the dressing nonwoven fabric image.

[0081] For each connected domain in the foreground image corresponding to each moment, the deformation degree of the fiber mesh pores corresponding to each connected domain and the probability of adjacent fiber mesh pores are analyzed to obtain the fiber interweaving loose coefficient of each connected domain in the foreground image at each moment, reflecting the sparse degree of fiber interweaving of the fiber mesh near the connected domain. The specific acquisition process is as follows:

[0082] The contour of each connected domain in the foreground image at each moment is taken as the ROI area, and the fractal dimension of the contour of each connected domain is calculated using the Fractal BoxCount plug-in of ImageJ. At the same time, a standard dressing non-woven fabric image, that is, a dressing non-woven fabric image with accurate spunlace pressure control, is obtained from the historical data and recorded as the standard dressing non-woven fabric image. The specific implementer can select it according to the actual situation, and record the foreground image of the standard dressing non-woven fabric image as the standard foreground image. The same method as in this embodiment is used to obtain the fractal dimension of the contour of each connected domain in the standard foreground image, and calculate the degree of deformation of the fiber mesh gap of each connected domain in the foreground image at each moment. The specific calculation method is:

[0083] ; In the formula, is the deformation degree of the fiber mesh gap of the kth connected domain in the foreground image at the jth moment, is the fractal dimension of the contour of the kth connected domain in the foreground image at the jth moment, is the fractal dimension of the i-th connected domain contour in the standard foreground image, and I is the total number of connected domain contours in the standard foreground image.

[0084] When the geometry of the connected domain contour is more complex, that is, The larger it is, the more irregular the fiber void morphology characteristics corresponding to the connected domain contour are, the more obvious the fiber web void morphology changes corresponding to the connected domain are, and the greater the degree of deformation of the fiber web void in the connected domain is.

[0085] The centroid of each connected domain in the foreground image at each moment is obtained, and M contour pixels are randomly selected on the contour of the connected domain, and the metric distance from each contour pixel to the corresponding connected domain centroid is calculated. For any connected domain, the discrete degree of the metric distance from all contour pixels to the corresponding one is calculated, and then the fiber network gap connection probability of each connected domain in the foreground image at each moment is calculated. The specific calculation method is:

[0086] ; In the formula, is the fiber network gap connection probability of the kth connected domain in the foreground image at the jth moment, is the number of pixels in the kth connected domain in the foreground image at the jth moment, is the mean number of pixels in all connected domains in the standard foreground image, is the discrete degree corresponding to the kth connected domain in the foreground image at the jth moment, and Norm[] is the normalization function.

[0087] It should be noted that in this embodiment, M=30, the calculation method of the metric distance is Euclidean distance, and the calculation method of the degree of dispersion can be variance, standard deviation, coefficient of variation, etc. This embodiment uses standard deviation as the calculation method of the degree of dispersion. The implementer can set it according to the actual situation, and this embodiment does not limit it here.

[0088] The larger the connected domain in the foreground image, the The larger the value, the more fiber mesh gap pixels may be contained in the connected domain. The larger it is, the more random and discrete the distribution of the connected domain contour pixels is, and the connected domain is more likely to contain more fiber mesh gaps, and the fiber mesh gaps are connected to each other, and thus, the corresponding fiber mesh gap connection probability is greater.

[0089] The product of the fiber web gap connection probability of the kth connected domain in the foreground image at the jth moment and the fiber web gap deformation degree is taken as the fiber interweaving looseness coefficient of the kth connected domain in the foreground image at the jth moment.

[0090] The same method is used to obtain the fiber interweaving looseness coefficient of each connected domain in the foreground image at each moment.

[0091] (2) Threshold segmentation is performed based on the fiber interweaving loose coefficient, and each connected domain whose fiber interweaving loose coefficient is greater than the segmentation threshold is regarded as a fiber sparse area; the foreground image at each moment is divided into each lateral interval, and the distribution of the fiber sparse area in each lateral interval is analyzed to obtain the water entanglement feedback intensity of each lateral interval at each moment.

[0092] If the deformation degree of the fiber mesh gap of the connected domain is greater, it indicates that the fiber mesh gap corresponding to the connected domain is more likely to belong to the fiber sparse area, the sparse degree of fiber mesh interweaving near the connected domain is higher, and the fiber interweaving loose coefficient is higher. The greater the probability of the fiber mesh gap corresponding to the connected domain being connected, it means that the gray value of the fiber mesh near the connected domain is lower, and it is more likely that the fiber mesh near the connected domain is small in number and sparsely interweaved, and the fiber interweaving loose coefficient is also higher.

[0093] At this point, the fiber interweaving loose coefficient of each connected domain in the foreground image at each moment can be obtained, reflecting the sparseness of the fiber interweaving of the fiber mesh near the connected domain. In this embodiment, the fiber interweaving loose coefficients of all connected domains in the foreground image at each moment are used as the input of the Otsu method to obtain the segmentation threshold, and the connected domain with a fiber interweaving loose coefficient greater than the segmentation threshold is recorded as a fiber sparse area. The Otsu method is an existing well-known technology, and the implementer can choose other existing methods for obtaining the segmentation threshold, which is not limited in this embodiment.

[0094] In the preparation process of medical dressings, in order to improve production capacity, the fiber cloth is wide. During the hydroentanglement process, multiple hydroentanglement heads need to be placed in one row, and multiple rows of hydroentanglement heads are placed. The hydroentanglement pressure of each hydroentanglement head is different. Therefore, this embodiment divides the image of the dressing non-woven fabric into h horizontal intervals along the conveying direction of the conveyor belt, where h is the number of hydroentanglement heads in each row. It should be understood that due to the presence of multiple rows of hydroentanglement heads, one horizontal interval corresponds to a row of hydroentanglement heads. For the images of the dressing non-woven fabric collected at all times, the horizontal intervals are divided in the same way. In this embodiment, h=5, and the implementer can set it according to the actual situation. This embodiment does not limit it here.

[0095] The web fibers in the same transverse section of the composite fiber spunlace fabric are repeatedly sprayed by the water jet from the same spunlace head. If there are multiple connected domains with high fiber interweaving loose coefficients in the transverse section, the spunlace pressure of the spunlace head corresponding to the transverse section is more likely to be inappropriate. In order to make the composite fiber non-woven fabric substrate have appropriate surface density and better tensile and tear resistance, it is more necessary to feedback and adjust the spunlace pressure.

[0096] For each corresponding lateral interval in the foreground image at each moment, if the centroid of the fiber sparse area in any lateral interval belongs to any lateral interval, then the fiber sparse area belongs to any lateral interval. Therefore, the fiber sparse area in each lateral interval can be divided.

[0097] The cumulative sum of the fiber interlacing looseness coefficients of all fiber sparse areas in each lateral interval corresponding to the foreground image at each moment is taken as the interlacing unformed degree of each lateral interval corresponding to the foreground image at each moment.

[0098] When the looseness of all web fibers in the transverse interval is generally high, that is, the greater the cumulative sum of the fiber interlacing looseness coefficients of all fiber sparse areas, the lower the entanglement effect of the fibers in the transverse area caused by the water jet of the water jet head, and the higher the corresponding interlacing unformed degree.

[0099] At the same time, due to unexpected factors during the hydroentanglement process, such as fluctuations in water quality, poor water quality can cause the hydroentanglement head to be blocked, affecting the fiber entanglement effect and causing fiber sparse areas. Therefore, in order to avoid errors in the determination of fiber sparse areas, the discrete degree of the ordinate of the centroid of all fiber sparse areas in each transverse interval is calculated as the fiber sparse area distribution distance in each transverse interval.

[0100] The closer the fiber sparse areas are in the transverse interval, that is, the smaller the discreteness of the vertical coordinate is, the less likely the fiber sparse areas in the transverse interval are accidental factors in the industrial preparation process, and the worse the entanglement effect of the water jet head on the fibers, that is, the lower the distribution distance of the fiber sparse areas.

[0101] Furthermore, the water spurt feedback intensity in each lateral interval at each moment is calculated. The specific calculation method is:

[0102] ; is the water thorn feedback intensity corresponding to the horizontal interval q in the foreground image at the jth moment, is the degree of interlacing unformation corresponding to the horizontal interval q in the foreground image at the jth moment, is the fiber sparse area distribution distance corresponding to the lateral interval q in the foreground image at the jth moment, In order to preset a value greater than 0 and avoid the denominator being 0, the value is taken as 0.01 in this embodiment. The implementer can set it according to the actual situation, and this embodiment does not limit it here.

[0103] The higher the degree of unformed interweaving in the transverse interval, the lower the water jet pressure of the water jet head is, which is insufficient to fully form the fibers in the fiber web. At the same time, the lower the distribution distance of the sparse fiber area in the transverse interval, the more frequently the water jet pressure of the water jet head is insufficient, and the more it is necessary to increase the water jet pressure of the water jet head to promote fiber entanglement and fiber web interweaving, and to make feedback adjustments in time, that is, the greater the water jet feedback intensity in the transverse interval.

[0104] (3) Based on the difference between the water jet feedback intensity and a preset adjustment threshold, and in combination with the water jet pressure in each time period, the water jet pressure in the next time period of each time period is adjusted.

[0105] The water jet pressure in the water jet treatment process is adjusted once every preset time period. In this embodiment, the length of a time period is 5 minutes. The implementer can adjust it according to the actual situation, and this embodiment does not limit it here.

[0106] Since the composite fiber spunlace fabric is transported by a conveyor belt, it will pass through multiple rows of spunlace heads for spunlace treatment during the transportation process. That is, the corresponding area of ​​the collected dressing non-woven fabric image in the composite fiber spunlace fabric will be spunlace treated multiple times. Taking the corresponding horizontal interval a in the foreground image as an example, the average of the spunlace feedback intensity at all moments in the horizontal interval a in each time period is used as the pressure adjustment coefficient of the horizontal interval a in each time period.

[0107] For any time period, when the pressure adjustment coefficient of horizontal interval a is less than or equal to the preset adjustment threshold , indicating that the water jet pressure in the transverse interval a is sufficient and the fiber web interweaving effect is excellent, and there is no need to adjust the water jet pressure of the water jet head corresponding to the transverse interval a in the next time period of any time period, wherein the adjustment threshold This embodiment takes 0.7, and the implementer can set it according to the actual situation. This embodiment does not limit it here.

[0108] On the contrary, when the pressure adjustment coefficient of the horizontal interval a is greater than the adjustment threshold , indicating that the water jet pressure in the transverse section a is insufficient, and the water jet pressure of the water jet head corresponding to the transverse section a needs to be adjusted. The water jet adjustment value of the transverse section a in any time period is calculated as follows:

[0109] ; In the formula, is the water spurt adjustment value of the horizontal interval a in the tth time period, is the pressure adjustment coefficient of the horizontal interval a in the tth time period, To preset the adjustment threshold, It is the average of the water jet pressures of all water jet heads in the column corresponding to the transverse interval a in the tth time period.

[0110] when The larger it is, the more sparse the fibers in the lateral interval a are and the worse the entanglement effect of the water jet head on the fibers is. A higher water jet pressure should be used to spray the fiber web to reinforce the fiber web, that is, the larger the water jet adjustment value is.

[0111] The water jet pressure of all water jet heads corresponding to the transverse interval a in the t+1th time period is adjusted to The same method is used to adjust the water jet pressure of the water jet head corresponding to each horizontal zone, so as to complete the feedback adjustment of the water jet pressure during the water jet treatment process. Figure 7 shown.

[0112] S8: In Example 1 of the present application, hydroxybutyl chitosan is put into a 1% acetic acid solution, the content of hydroxybutyl chitosan is 4wt%, and then a cross-linking agent is added, the content of the cross-linking agent is 5wt%, wherein the cross-linking agent is CaCl2, and an anti-inflammatory agent is added, the content of the anti-inflammatory agent is 0.5wt%, wherein the anti-inflammatory agent is ciprofloxacin, and the mixture is stirred until dissolved, wherein the stirring speed is 200r / min, to obtain a composite sol.

[0113] In Example 2 of the present application, hydroxybutyl chitosan is put into a 2% acetic acid solution, the content of hydroxybutyl chitosan is 7wt%, and then a cross-linking agent is added, the content of the cross-linking agent is 10wt%, wherein the cross-linking agent is MgCl2, and an anti-inflammatory agent is added, the content of the anti-inflammatory agent is 0.7wt%, wherein the anti-inflammatory agent is rifamycin, and stirring is performed until the solution is completely dissolved, wherein the stirring speed is 250r / min, to obtain a composite sol.

[0114] In Example 3 of the present application, hydroxybutyl chitosan is put into a 2% acetic acid solution, the content of hydroxybutyl chitosan is 10wt%, and then a cross-linking agent is added, the content of the cross-linking agent is 15wt%, wherein the cross-linking agents are CaCl2 and MgCl2, and an anti-inflammatory agent is added, the content of the anti-inflammatory agent is 1wt%, wherein the anti-inflammatory agent is metronidazole, and the mixture is stirred until dissolved, wherein the stirring speed is 300r / min, to obtain a composite sol.

[0115] Among them, chitosan has good biocompatibility and biodegradability. Medical dressings with chitosan added can be antibacterial and hemostatic, do not cause allergies, and accelerate wound healing. Hydroxybutyl can also increase the water solubility of chitosan.

[0116] S9: coating the composite sol on the composite fiber nonwoven fabric substrate, performing a vacuum treatment, and then performing a hot rolling treatment, wherein an initial dressing is obtained.

[0117] In Example 1 of the present application, the vacuum environment is -0.09 MPa, and the temperature of the hot rolling treatment is set to 50°C.

[0118] In Example 2 of the present application, the vacuum environment is -0.1 MPa, and the temperature of the hot rolling treatment is set to 60°C.

[0119] In Example 3 of the present application, the vacuum environment is -0.1 MPa, and the temperature of the hot rolling treatment is set to 70°C.

[0120] S10: The initial dressing is dried in a dryer and finally sterilized to obtain a medical dressing with rapid hemostasis.

[0121] Based on the same inventive concept as the above method, an embodiment of the present application further provides a medical dressing for rapid hemostasis, wherein the medical dressing for rapid hemostasis is made by the above method for preparing a medical dressing for rapid hemostasis.

[0122] It should be noted that the above sequence of the embodiments of the present application is for description only and does not represent the advantages and disadvantages of the embodiments. The above is a description of a specific embodiment of this specification. In addition, the processes depicted in the accompanying drawings do not necessarily require the specific order or continuous order shown to achieve the desired results. In some embodiments, multitasking and parallel processing are also possible or may be advantageous.

[0123] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0124] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a medical dressing for rapid hemostasis, characterized in that: The method comprises the following steps: Adding sulfonamide into the sodium alginate aqueous solution to obtain a sodium alginate / sulfonamide aqueous solution; The sodium alginate / sulfonamide aqueous solution is pumped into the spinning kettle for vacuum degassing to obtain the spinning solution; The spinning solution is sent into a coagulation bath, the spinning solution is sprayed out in a calcium chloride solution and solidified into seaweed fibers, and the seaweed short fibers are obtained after being cut and dried; The seaweed staple fiber, dandelion fluff fiber and viscose fiber are mixed, opened and combed, and then laid out and pressed into a fiber cloth; After the fiber cloth is transported to the spunlacing machine for spunlacing treatment, it is dried to obtain a composite fiber nonwoven fabric substrate, and the spunlacing pressure during the spunlacing treatment is feedback-adjusted, specifically: (1) Collect images of the composite fiber non-woven fabric substrate at each time in each time period and extract the foreground image at each time; analyze the deformation degree of the fiber web gaps corresponding to each connected domain in the foreground image and the probability of the fiber web gaps being connected, and determine the fiber interweaving looseness coefficient of each connected domain in the foreground image; (2) performing threshold segmentation based on the fiber interweaving loose coefficient, taking each connected domain whose fiber interweaving loose coefficient is greater than the segmentation threshold as each fiber sparse area; dividing the foreground image at each moment into each horizontal interval, analyzing the distribution of the fiber sparse area in each horizontal interval, and obtaining the water entanglement feedback intensity of each horizontal interval at each moment; (3) adjusting the water jet pressure in the next time period of each time period based on the difference between the water jet feedback intensity and a preset adjustment threshold and in combination with the water jet pressure in each time period; The composite sol is obtained by using raw materials of hydroxybutyl chitosan, acetic acid solution, cross-linking agent and anti-inflammatory agent; The composite sol is coated on the composite fiber non-woven fabric substrate, and vacuum treated and hot rolled to obtain an initial dressing, and after drying and sterilization, a medical dressing is obtained; The process of determining the fiber interlacing looseness coefficient is as follows: Calculate the fractal dimension of each connected domain contour in the foreground image, obtain the standard fractal dimension of each connected domain contour in the standard foreground image, and use the average of the differences between the fractal dimension of each connected domain contour in the foreground image and the standard fractal dimension of all connected domain contours in the standard foreground image as the degree of fiber web gap deformation of each connected domain in the foreground image; Calculate the mean of the number of pixels in all connected domains in the standard foreground image, calculate the ratio of the number of pixels in each connected domain in the foreground image to the mean, calculate the chaos degree of the metric distance from multiple pixels on the contour of each connected domain in the foreground image to the centroid of the connected domain, and use the normalized value of the product of the ratio and the chaos degree as the probability of fiber web gap connection of each connected domain in the foreground image; The fiber interlacing looseness coefficient is the product of the deformation degree of the fiber web gaps and the probability of the fiber web gaps being connected.

2. The method for preparing a rapid hemostatic medical dressing according to claim 1, characterized in that: The process of obtaining the sodium alginate / sulfonamide aqueous solution is as follows: The concentration of sodium alginate in the sodium alginate aqueous solution is 2-5wt%, sulfonamide is added to the sodium alginate aqueous solution until the sulfonamide concentration is 2-10wt%, and stirred for 30-40 minutes to obtain a sodium alginate / sulfonamide aqueous solution; The vacuum degassing conditions are -0.09MPa~-0.1MPa, and the duration is 30~50min.

3. The method for preparing a rapid hemostatic medical dressing according to claim 1, characterized in that: The preparation of the dandelion fluff fiber comprises: The dandelion fluff is put into a sodium bicarbonate solution for ultrasonic activation treatment, and then the ultrasonically activated dandelion fluff is washed with deionized water until the washing solution is neutral, and then the dandelion fluff fiber is obtained after drying.

4. The method for preparing a rapid hemostatic medical dressing according to claim 1, characterized in that: The mass ratio of the seaweed staple fiber, dandelion fluff fiber and viscose fiber is 3:3:4; the spunlace pressure of the spunlace treatment is 2.2-4 MPa, and the feed and discharge speed is 12-15 m / min; the drying temperature is 80° C., and the drying time is 2-5 min.

5. The method for preparing a rapid hemostatic medical dressing according to claim 1, characterized in that: The process of determining the water spurt feedback intensity is as follows: For each transverse interval, if the centroid of a fiber sparse region in any transverse interval belongs to the any transverse interval, then the fiber sparse region belongs to the any transverse interval, and the sum of the fiber interlacing loose coefficients of all fiber sparse regions in each transverse interval is calculated as the interlacing unformed degree of each transverse interval; Calculate the discrete degree of the ordinate of the centroid of all fiber sparse areas in each transverse interval as the fiber sparse area distribution distance in each transverse interval; The water entanglement feedback intensity is positively correlated with the degree of interweaving unformation, and negatively correlated with the distribution distance of the fiber sparse area.

6. The method for preparing a rapid hemostatic medical dressing according to claim 1, characterized in that: The step of adjusting the water jet pressure in the next time period of each time period comprises: The average of the water spurt feedback intensity at all times in each lateral interval in each time period is used as the pressure adjustment coefficient of each lateral interval in each time period. If the pressure adjustment coefficient of lateral interval a in the t-th time period is less than or equal to the preset adjustment threshold, the water spurt pressure of lateral interval a in the t+1-th time period is not adjusted. Otherwise, the water spurt adjustment value of lateral interval a in the t-th time period is The calculation method is: ; In the formula, is the pressure adjustment coefficient of the horizontal interval a in the tth time period, To preset the adjustment threshold, is the mean value of the water jet pressure of all water jet heads in the column corresponding to the horizontal interval a in the tth time period; The water jet pressure of all water jet heads corresponding to the transverse interval a in the t+1th time period is adjusted to the water jet adjustment value.

7. The method for preparing a rapid hemostatic medical dressing according to claim 1, characterized in that: The preparation of the composite sol comprises: Put hydroxybutyl chitosan into 1-2% acetic acid solution, the content of hydroxybutyl chitosan is 4-10wt%, then put in a cross-linking agent, the content of the cross-linking agent is 5-15wt%, add an anti-inflammatory agent, the content of the anti-inflammatory agent is 0.5-1wt%, stir until it is completely dissolved to obtain a composite sol, wherein the stirring speed is 200-300r / min.

8. The method for preparing a rapid hemostatic medical dressing according to claim 1, characterized in that: The vacuum environment of the vacuum treatment is -0.09MPa~-0.1MPa, and the temperature of the hot rolling treatment is 50~70℃.

9. A medical dressing for rapid hemostasis, characterized in that: The medical dressing for rapid hemostasis is made by the method described in any one of claims 1 to 8.