Biological ceramic / bacterial cellulose composite artificial bone, preparation method and application
Through the combination of bioceramics, bacterial cellulose composite artificial bone and carbon nanotube layers, the problem of poor mechanical properties of existing artificial bone materials is solved, bone defect repair in load-bearing parts is realized, and the stability and stability of bone repair materials are improved. Biocompatible, promotes bone formation.
Patent Information
- Application Number
- CN202411193724.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-10-29
AI Technical Summary
Existing artificial bone materials have poor mechanical properties in the repair of bone defects in load-bearing parts, which can easily lead to stress shielding effects, loosening of bone repair materials and poor bone absorption, and cannot meet the needs of load-bearing parts.
Bioceramics and bacterial cellulose are used to composite artificial bone, and a carbon nanotube layer is set on the outside. Through the combination of gradient freeze-drying and carbon nanotube coating, the mechanical properties and biocompatibility of the material are improved, and bone formation is promoted.
It improves the mechanical properties and biocompatibility of artificial bone, reduces the stress shielding effect, enhances the stability and integration ability of bone repair materials, promotes bone formation and cell growth, and meets the needs of bone defect repair in load-bearing parts.
Smart Images

Figure CN118846210A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of medical technology, and in particular to a bioceramic / bacterial cellulose composite artificial bone, a preparation method and an application thereof. Background Art
[0002] Clinically, bone defects caused by trauma, infection, bone disease or congenital malformation are increasing, and the repair of bone defects, especially the treatment and functional reconstruction of bone defects in load-bearing parts such as the skull, maxillofacial region, spine, and limb bones, is a difficult problem faced by orthopedics. After the bone defects in these load-bearing parts are repaired, the implanted materials need to withstand the various forces acting on them by the body, which places high demands on the mechanical properties of the materials.
[0003] At present, the materials used for repairing bone defects in load-bearing parts such as the skull, maxillofacial region, spine, and limb bones mainly include three series: medical stainless steel, cobalt-based alloys, and titanium alloys. Titanium alloys have the characteristics of low specific gravity, high specific strength, low elastic modulus, and easy processing and forming. They have now developed into an ideal functional structural material for surgical implants. However, the complex internal environment of the human body can cause corrosion of titanium alloys and release toxic elements, reducing biocompatibility. In addition, the elastic modulus of titanium alloys is too different from that of human bone tissue, which can easily produce a stress shielding effect, which is not conducive to the growth and remodeling of new bones, and may even lead to secondary fractures. Therefore, people are committed to seeking bone repair materials that are more corrosion-resistant, biocompatible, and closer to the mechanical properties of human bones.
[0004] As an inorganic non-metallic biomaterial, bioceramic materials have attracted more and more attention due to their advantages such as no toxic side effects, appropriate biomechanics, good biocompatibility, corrosion resistance, degradability, osteoinduction and osteoconductivity, and have become a hot spot and focus in the field of bone transplantation and repair.
[0005] A Chinese invention patent with the authorization publication number CN111070376B discloses a 3D printed bionic porous bioceramic artificial bone and a preparation method thereof. The method adopts a combined TPMS (Triply Periodic Minimal Surface) and CSG (Constructive Solid Geometry) method to design a porous bioceramic artificial bone model, uses bioceramic powder and a binder to prepare a printable slurry, and combines the 3D filamentless printing process to prepare a porous bioceramic artificial bone. Although the precise design of the porosity, connectivity and uniformity in the artificial bone is achieved, the prepared porous bioceramic artificial bone has poor mechanical properties such as elastic modulus, toughness and fracture strength, and is prone to stress shielding, and cannot be accurately matched with human bones, resulting in loose bone repair materials and poor bone absorption effects, thereby failing to meet the needs of bone defect repair in load-bearing areas. Summary of the invention
[0006] In view of the problems in the prior art of poor mechanical properties of artificial bones, loosening of bone repair materials due to stress shielding, and poor bone absorption effect, the present invention provides a bioceramic / bacterial cellulose composite artificial bone, a preparation method and application.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] The present invention provides a bioceramic / bacterial cellulose composite artificial bone, comprising an artificial bone main body, wherein a carbon nanotube layer is arranged on the outside of the artificial bone main body;
[0009] The raw material components of the artificial bone main body include: 53wt% to 84wt% of bioceramics, 10wt% to 32wt% of bacterial cellulose and 6wt% to 15wt% of a binder.
[0010] Furthermore, the bioceramic is one or more of hydroxyapatite, β-tricalcium phosphate, calcium sulfate, calcium silicate, calcium carbonate and calcined bone powder.
[0011] Furthermore, the binder is one or more of polyvinyl alcohol, polylactic acid, polyethylene glycol, polyglycolic acid, polyglycolic acid copolymer, chitosan, gelatin and collagen.
[0012] Furthermore, the bioceramic / bacterial cellulose composite artificial bone has a porosity of 30% to 80% and a pore size of 400 to 1000 μm.
[0013] Furthermore, the thickness of the carbon nanotube layer is 0.05-0.3 mm.
[0014] The present invention provides a method for preparing a bioceramic / bacterial cellulose composite artificial bone, comprising:
[0015] 53 wt% to 84 wt% of bioceramic, 10 wt% to 32 wt% of bacterial cellulose and 6 wt% to 15 wt% of a binder are uniformly mixed to obtain a slurry;
[0016] The slurry is printed into a preliminary blank, and gradient freeze-dried to obtain an artificial bone body;
[0017] A carbon nanotube layer is prepared on the outside of the artificial bone body to obtain a bioceramic / bacterial cellulose composite artificial bone.
[0018] Further, the method of gradient freeze drying is:
[0019] The blank is placed at a temperature of -45°C to -1°C for pre-freezing;
[0020] After the pre-freezing is completed, the pre-form is placed in a vacuum degree of 5 to 20 Pa and a temperature of -45°C to -30°C for freeze drying;
[0021] After freeze-drying, the preform is placed in a vacuum condition of 5 Pa and 20°C to 35°C for analytical drying to complete gradient freeze-drying.
[0022] Furthermore, the method for preparing the carbon nanotube layer outside the artificial bone body is:
[0023] The artificial bone body is immersed in a carbon nanotube dispersion and dried to obtain a bioceramic / bacterial cellulose composite artificial bone; wherein the concentration of the carbon nanotube dispersion is 7-10 μg / mL.
[0024] Furthermore, the artificial bone body is immersed in the carbon nanotube dispersion for 2 to 4 hours, and the drying temperature is 55° C. to 70° C.
[0025] The application of the bioceramic / bacterial cellulose composite artificial bone as mentioned above in the preparation of bone defect repair materials.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The invention discloses a bioceramic / bacterial cellulose composite artificial bone, comprising an artificial bone main body, wherein a carbon nanotube layer is arranged on the outside of the artificial bone main body; the raw material components of the artificial bone main body include: 53wt% to 84wt% of bioceramic, 10wt% to 32wt% of bacterial cellulose and 6wt% to 15wt% of a binder. The artificial bone main body of the artificial bone is a main body composited with bioceramic and bacterial cellulose, and bacterial cellulose, as an ideal biomedical material, has the characteristic of excellent corrosion resistance, and bacterial cellulose does not chemically react with common inorganic salt compounds, hydrochloric acid, concentrated nitric acid and even "aqua regia" at room temperature. Therefore, in the complex liquid environment in the human body, bacterial cellulose can ensure good stability. Secondly, biological tissues are easy to grow on the surface of bacterial cellulose implants, can be integrated with human soft and hard tissues, enhance the adhesion ability of cells, and promote cell growth. Therefore, the artificial bone body of the present invention has good biocompatibility, does not cause inflammatory reaction, and its elastic modulus, toughness and fracture strength and other mechanical properties match human bones, do not cause stress shielding, and have good mechanical strength; the setting of the carbon nanotube layer, in addition to improving the mechanical properties of artificial bones, has the ability to promote mineralization, and can better promote osteoblast attachment, diffusion and proliferation. An important process in bone repair is calcification, which needs to be accelerated by early calcification speed. Carbon nanotubes can attract calcium ions through their own negative potential, further strengthen the bone absorption process on the basis of bacterial cellulose, increase the concentration of calcium around osteoblasts, thereby promoting calcification and inducing osteogenesis. At the same time, the good strength, elasticity and fatigue resistance of carbon nanotubes make it an excellent reinforcing material in artificial bones, which can effectively improve the strength and toughness of materials, and carbon nanotubes have good biocompatibility, good toughness and high strength. Therefore, in terms of physical properties, the bioceramic / bacterial cellulose composite artificial bone can reduce the negative effects such as loosening of bone repair materials and bone absorption caused by stress shielding, further enhance the mechanical properties, surface roughness and porosity of the artificial bone, and in terms of biological properties, it can increase protein adsorption in the repair process of the artificial bone, increase cell adhesion and proliferation, promote osteogenic differentiation, and improve the applicability of the artificial bone.
[0028] The porosity of the bioceramic / bacterial cellulose composite artificial bone is 30% to 80%; the pore size is 400 to 1000 μm. On the basis of ensuring sufficient strength and rigidity, the higher porosity allows more host bone cells and blood vessels to grow into the artificial bone to form a tight bond, thereby enhancing the stability and durability of the artificial bone. The pores provide the necessary space for cell growth and allow nutrients and metabolic waste to be freely exchanged between the artificial bone and the host bone, which is beneficial to the survival and proliferation of cells. At the same time, the weight of the artificial bone can be reduced, making it closer to the density and weight of natural bone tissue, reducing the burden on the patient's body.
[0029] The thickness of the carbon nanotube layer is 0.05 to 0.3 mm. A carbon nanotube coating of appropriate thickness can significantly improve its overall mechanical properties, making the artificial bone more stable and reliable when subjected to mechanical loads. At the same time, the presence of the coating increases the surface area of the artificial bone, providing more attachment points for bone cells, which is beneficial to the growth and attachment of bone cells on the surface of the artificial bone, allowing bone cells and blood vessels to grow into the coating to form a tight bond, thereby enhancing the integration ability of the artificial bone with the host bone tissue.
[0030] The present invention also provides a method for preparing a bioceramic / bacterial cellulose composite artificial bone, wherein the method comprises the steps of uniformly mixing bioceramics, bacterial cellulose and a binder, printing them into a preliminary blank, and drying them to obtain an artificial bone body; and preparing a carbon nanotube layer on the outside of the artificial bone body to obtain a bioceramic / bacterial cellulose composite artificial bone. By cleverly combining the effects of bacterial cellulose and carbon nanotube coatings, stress shielding can be effectively reduced, bone tissue absorption can be avoided, and bone formation can be further promoted; at the same time, the negative effects of bone repair materials can be avoided and the mechanical properties of bone repair materials can be enhanced. The preparation method is simple and easy to control, and the precise design of the porosity, connectivity and uniformity of artificial bones can be achieved.
[0031] Gradient freeze-drying is used in the preparation process, which makes the drying more thorough and less prone to deformation such as cracking and collapse, thereby further improving the strength of the artificial bone body.
[0032] For example, the above-mentioned bioceramic / bacterial cellulose composite artificial bone is used in the preparation of a repair material for bone defects. The repair material for bone defects has excellent biocompatibility, mechanical properties, bone integration ability, etc. The artificial bone has broad application prospects in the fields of orthopedic surgery, dental repair, and orthopedic implants. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The present invention is a schematic diagram of a process for preparing a bioceramic / bacterial cellulose composite artificial bone.
[0034] Figure 2 This is a diagram showing the cytotoxicity test results of a bioceramic / bacterial cellulose composite artificial bone of the present invention. DETAILED DESCRIPTION
[0035] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0036] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0037] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0038] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0039] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0040] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0041] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0042] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0043] Example 1
[0044] The present invention provides a bioceramic / bacterial cellulose composite artificial bone, comprising an artificial bone main body, wherein a carbon nanotube layer is arranged on the outside of the artificial bone main body; the bioceramic / bacterial cellulose composite artificial bone has a porosity of 30% to 80% and a pore size of 400 to 1000 μm;
[0045] The raw material components of the artificial bone body include: 53wt% to 84wt% of bioceramics, 10wt% to 32wt% of bacterial cellulose and 6wt% to 15wt% of a binder; wherein the bioceramics are one or more of hydroxyapatite, β-tricalcium phosphate, calcium sulfate, calcium silicate, calcium carbonate and calcined bone powder; the binder is one or more of polyvinyl alcohol, polylactic acid, polyethylene glycol, polyglycolic acid, polyglycolic acid copolymer, chitosan, gelatin and collagen;
[0046] The thickness of the carbon nanotube layer is 0.05-0.3 mm.
[0047] The artificial bone main body of the artificial bone is a main body composited with bioceramics and bacterial cellulose. As an ideal biomedical material, bacterial cellulose has excellent corrosion resistance. At room temperature, bacterial cellulose does not react chemically with common inorganic salt compounds, hydrochloric acid, concentrated nitric acid, or even "aqua regia". Therefore, in the complex liquid environment in the human body, bacterial cellulose can ensure good stability. Secondly, biological tissues are easy to grow on the surface of bacterial cellulose implants, can be integrated with human soft and hard tissues, enhance the adhesion ability of cells, and promote cell growth. Therefore, the artificial bone main body of the present invention has good biocompatibility, does not cause inflammatory reactions, and its elastic modulus, toughness, and mechanical properties such as fracture strength match those of human bones, do not cause stress shielding, and have good mechanical strength; the setting of the carbon nanotube layer, in addition to improving the mechanical properties of the artificial bone, has the ability to promote mineralization, can better promote the attachment, diffusion, and proliferation of osteoblasts; carbon nanotubes can attract calcium ions through their own negative potential, further strengthen the bone absorption process on the basis of bacterial cellulose, increase the concentration of calcium around osteoblasts, thereby promoting calcification and inducing osteogenesis. At the same time, the good strength, elasticity and fatigue resistance of carbon nanotubes make them an excellent reinforcement material in artificial bones, which can effectively improve the strength and toughness of the material, and carbon nanotubes have the advantages of good biocompatibility, good toughness and high strength. Therefore, in terms of physical properties, the artificial bone of the bioceramic / bacterial cellulose composite can reduce the negative effects such as loosening of bone repair materials and bone absorption caused by stress shielding, further enhance the mechanical properties, surface roughness and porosity of artificial bones, and in terms of biological properties, it can increase protein adsorption in the repair process of artificial bones, increase cell adhesion and proliferation, promote osteogenic differentiation, and improve the applicability of artificial bones.
[0048] Example 2
[0049] See also Figure 1 The present invention provides a method for preparing a bioceramic / bacterial cellulose composite artificial bone, comprising:
[0050] S1: The bioceramic, bacterial cellulose and binder are mixed evenly to obtain a slurry, specifically:
[0051] The mixed bioceramic, bacterial cellulose and binder are placed in a ball mill for 24 to 72 hours to fully mix the raw materials and obtain a fine and soft printing slurry; the fully mixed printing slurry is loaded into a barrel and degassed in a centrifuge to obtain a uniform slurry;
[0052] During the ball milling process, the particle size of the powder material in the raw material can reach the micro-nano level. After ball milling, the powder in the slurry is finer and the particles reach the nano level, which can make the distance between the particles smaller in the subsequent printing process, and the combination of the powders in the same area is tighter, which is conducive to the formation of the structure and the regulation of the pore size, and the toughness is also better; wherein, the raw material components are: 53wt% to 84wt% of bioceramics, 10wt% to 32wt% of bacterial cellulose and 6wt% to 15wt% of a binder; the bioceramics are one or more of hydroxyapatite, β-tricalcium phosphate, calcium sulfate, calcium silicate, calcium carbonate and calcined bone powder; the binder is one or more of polyvinyl alcohol, polylactic acid, polyethylene glycol, polyglycolic acid, polyglycolic acid copolymer, chitosan, gelatin and collagen.
[0053] S2: Print the slurry into a preliminary blank, and perform gradient freeze drying to obtain the artificial bone body, specifically:
[0054] Obtain a bone defect entity model, use medical imaging technology to obtain the DICOM data of the patient's bone defect site, and reconstruct the data in three dimensions. Obtain a morphologically matching bone defect entity model through design and save it as an STL format file;
[0055] The STL format model file established for the bone defect is loaded into the bioceramic 3D printing equipment, and the slurry is 3D printed by the material extrusion method to obtain a preliminary blank; wherein, since the 3D printing method using laser or electron beam focused heating will cause uneven heating and inconsistent thermal changes of the material during the processing, it is easy to cause the prepared artificial bone to have the problem of local stress concentration. Therefore, the 3D printing technology of the present invention uses a nozzle to spray out the printing slurry, and the slurry is bonded layer by layer to form, so as to prepare an artificial bone that matches the performance of the human body's own bone structure.
[0056] The preform is placed in a freeze dryer to remove moisture and shape the preform through gradient freeze drying to obtain an artificial bone body. The gradient freeze drying method is as follows:
[0057] The blank is placed at a temperature of -45°C to -1°C for pre-freezing;
[0058] After the pre-freezing is completed, the pre-form is placed in a vacuum degree of 5 to 20 Pa and a temperature of -45°C to -30°C for freeze drying;
[0059] After freeze-drying, the blank is placed in a vacuum condition of 5 Pa and 20°C to 35°C for analytical drying to complete gradient freeze-drying to obtain the artificial bone body.
[0060] S3: preparing a carbon nanotube layer outside the artificial bone body to obtain a bioceramic / bacterial cellulose composite artificial bone, specifically:
[0061] Carbon nanotubes and deionized water are prepared into a carbon nanotube dispersion at a concentration of 7 to 10 μg / ml, and a small amount of carbon nanotube water dispersant (TNWDIS) is added after shaking, and the carbon nanotube dispersion is placed in a water bath for ultrasonication for 5 to 10 minutes, and then placed in cold water for defoaming, and the ultrasonication is repeated 3 to 6 times. Finally, the artificial bone body is immersed in the dispersed carbon nanotube dispersion for 2 to 4 hours, then taken out, placed in an oven, and dried at 55°C to 70°C for 2 to 7 hours to solidify the coating, and a porous bioceramic / bacterial cellulose composite artificial bone with a porosity of 30% to 80% and a pore size of 400μm to 1000μm is obtained;
[0062] The bioceramic / bacterial cellulose composite artificial bone is subjected to irradiation sterilization to obtain a finished product.
[0063] Example 3
[0064] Obtaining a physical model of the bone defect: using medical imaging technology to obtain the Digital Imaging and Communications in Medicine (DICOM) data of the patient's bone defect site, and reconstructing the DICOM data in three dimensions, obtaining a morphologically matching physical model of the bone defect through design, and saving the file in stereolithography (StereoLithography, STL) format;
[0065] Preparation: Weigh 7g of polyvinyl alcohol, add deionized water to it, put it in a 75°C water bath to swell for 30 minutes, then place it on a magnetic stirrer to heat it in a 97°C water bath, and stir it at a rate of 200r / min for 2h to prepare a 10wt% polyvinyl alcohol aqueous solution; finally, add 1.3g of polyvinyl pyrrolidone to the polyvinyl alcohol aqueous solution, stir it evenly, and obtain a binder solution;
[0066] First, 35g of hydroxyapatite, 12g of β-tricalcium phosphate and 8g of calcium sulfate are weighed, then 21g of bacterial cellulose powder and 60g of binder solution are added, and finally the raw materials are mixed to obtain a mixture; wherein the raw material components include 67wt% of bioceramics, 25wt% of bacterial cellulose, and 7wt% of binder.
[0067] The mixture was placed in a ball mill and milled at a speed of 150 r / min for 37 hours to make the powder material particle size in the raw material reach the micro-nano level, and the raw materials were fully mixed to obtain a delicate and soft printing slurry;
[0068] The printing slurry was loaded into the dispensing syringe and centrifuged and degassed at 1800 rad / min, 5 min / time for 2 times to obtain a uniform slurry.
[0069] The STL format file saved for the bone defect is loaded into the bioceramic 3D printing device, the barrel filled with the slurry is connected to the print head, the air pressure is adjusted to 0.4-0.5 MPa, the filling rate is set to 45%, the extrusion width is set to 0.6 mm, the STL format model slice file is run, and 3D printing is performed to obtain a blank;
[0070] The preform is placed in a freeze dryer to remove moisture and shape through gradient freeze drying. The specific method is as follows:
[0071] The pre-freezing process is performed by placing the pre-freezing blank at -1°C for 5 minutes, and then placing it at -45°C for 4 hours to complete the pre-freezing process.
[0072] After the pre-freezing is completed, the blank is placed under a vacuum degree of 20Pa, and then placed under a temperature of -45°C for 10 to 30 minutes, -33°C for 9 to 10 hours, and -30°C for 3 to 4 hours, and finally placed under a vacuum degree of 5Pa and -20°C for 3 to 4 hours to complete the freeze-drying of the blank;
[0073] After the freeze-drying is completed, the blank is placed in a vacuum of 5Pa, 20°C for 3-5 hours and 25°C for 3-4 hours for analytical drying, and then placed at a constant temperature of 35°C for shaping to complete gradient freeze drying to obtain the artificial bone body;
[0074] The carbon nanotubes and deionized water were mixed into a dispersion at a concentration of 10 μg / ml, and a small amount of carbon nanotube water dispersant (TNWDIS) was added after shaking, and the dispersion was shaken. Then the dispersion was placed in a water bath for 8 minutes for ultrasonication, and then placed in cold water for defoaming, and the ultrasonication was repeated 5 times. Finally, the shaped artificial bone body was immersed in the dispersed carbon nanotube dispersion for 3 hours and then taken out.
[0075] The artificial bone body after the coating treatment is placed in a 55° C. forced air oven for 4 hours to obtain a bioceramic / bacterial cellulose composite artificial bone with a porosity of 30% to 80%, a pore size of 400 μm to 1000 μm, and a connectivity rate greater than 98%;
[0076] The bioceramic / bacterial cellulose composite artificial bone prepared above is subjected to irradiation sterilization treatment to obtain a finished product.
[0077] See also Figure 2 The biological properties of the prepared bioceramic / bacterial cellulose composite artificial bone were tested, and the cytotoxicity of the artificial bone was tested using mouse fibroblasts. It was found that the relative survival rate of the cells was 89.7% at 100% concentration of the extract, and the biocompatibility was good.
[0078] Example 4
[0079] Obtaining a bone defect entity model: Using medical imaging technology to obtain the DICOM data of the patient's bone defect, and reconstructing the DICOM data in three dimensions, obtaining a morphologically matching bone defect entity model through design, and saving it in STL format;
[0080] Weigh 11 g of polylactic acid, add NN dimethylformamide thereto, place on a magnetic stirrer and stir at a rate of 150 r / min for 24 h to prepare a 13 wt % polylactic acid solution to obtain a binder solution;
[0081] First, 35g of hydroxyapatite and 23g of calcium silicate are weighed, then 15g of bacterial cellulose powder and 76g of binder solution are added, and finally the raw materials are mixed to obtain a mixture, wherein the raw material components include 69wt% of bioceramic, 19wt% of bacterial cellulose, and 13wt% of binder;
[0082] The mixture was placed in a ball mill and milled at a speed of 150 r / min for 34 hours to make the powder material particle size in the raw material reach the micro-nano level, and the raw materials were fully mixed to obtain a delicate and soft printing slurry;
[0083] The printing slurry was loaded into the dispensing syringe and centrifuged and degassed at 1800 rad / min, 5 min / time for 2 times to obtain a uniform slurry.
[0084] The STL format file saved for the bone defect is loaded into the bioceramic 3D printing device, the barrel filled with the slurry is connected to the print head, the air pressure is adjusted to 0.4-0.5 MPa, the filling rate is set to 45%, the extrusion width is set to 0.6 mm, the STL format model slice file is run, and 3D printing is performed to obtain a blank;
[0085] The preform is placed in a freeze dryer to remove moisture and shape the preform through gradient freeze drying to obtain an artificial bone body;
[0086] Prepare a dispersion of carbon nanotubes and deionized water at a concentration of 8 μg / ml, add a small amount of carbon nanotube water dispersant after shaking, and shake well. Then place the dispersion in a water bath for 8 minutes of ultrasound, then place it in cold water for defoaming, and repeat ultrasound 5 times. Finally, immerse the shaped artificial bone body in the dispersed carbon nanotube dispersion for 4 hours and then take it out.
[0087] The artificial bone body after the coating treatment is placed in a 60° C. forced air oven for 3 hours to obtain a bioceramic / bacterial cellulose composite artificial bone with a porosity of 30% to 80%, a pore size of 400 μm to 1000 μm, and a connectivity rate greater than 98%;
[0088] The bioceramic / bacterial cellulose composite artificial bone prepared above is subjected to irradiation sterilization treatment to obtain a finished product.
[0089] Example 5
[0090] Obtaining a bone defect entity model: Using medical imaging technology to obtain the DICOM data of the patient's bone defect, and reconstructing the DICOM data in three dimensions, obtaining a morphologically matching bone defect entity model through design, and saving it in STL format;
[0091] Weigh 4 g of gelatin, add 76 g of deionized water, place on a magnetic stirrer and stir at a rate of 150 r / min for 6 h to prepare a gel suspension to obtain a binder solution;
[0092] First, 13 g of calcium carbonate and 26 g of calcined bone powder are weighed, and then 18 g of bacterial cellulose powder and 50 g of a binder solution are added, and finally the raw materials are mixed to obtain a mixture, wherein the raw material components include 65.5 wt % of bioceramic, 30 wt % of bacterial cellulose, and 4 wt % of a binder;
[0093] The mixture was placed in a ball mill and milled at a speed of 150 r / min for 25 h to make the powder material particle size in the raw material reach the micro-nano level, and the raw materials were fully mixed to obtain a delicate and soft printing slurry;
[0094] The printing slurry was loaded into the dispensing syringe and centrifuged and degassed twice at 1800 rad / min, 5 min / time to obtain a uniform slurry.
[0095] The STL format file saved for the bone defect is loaded into the bioceramic 3D printing device, the barrel filled with the slurry is connected to the print head, the air pressure is adjusted to 0.4-0.5 MPa, the filling rate is set to 45%, the extrusion width is set to 0.6 mm, the STL format model slice file is run, and 3D printing is performed to obtain a blank;
[0096] The preform is placed in a freeze dryer to remove moisture and shape the preform through gradient freeze drying to obtain an artificial bone body;
[0097] Prepare a dispersion of carbon nanotubes and deionized water at a concentration of 8 μg / ml, add a small amount of carbon nanotube water dispersant after shaking, and shake well. Then place the dispersion in a water bath for 8 minutes of ultrasound, then place it in cold water for defoaming, and repeat ultrasound 4 times. Finally, immerse the shaped artificial bone body in the dispersed carbon nanotube dispersion for 4 hours and then take it out.
[0098] The artificial bone body after the coating treatment is placed in a 70° C. forced air oven for 4 hours to obtain a bioceramic / bacterial cellulose composite artificial bone with a porosity of 30% to 80%, a pore size of 400 μm to 1000 μm, and a connectivity greater than 98%;
[0099] The bioceramic / bacterial cellulose composite artificial bone prepared above is subjected to irradiation sterilization treatment to obtain a finished product.
[0100] Example 6
[0101] Obtaining a bone defect entity model: Using medical imaging technology to obtain the DICOM data of the patient's bone defect, and reconstructing the DICOM data in three dimensions, obtaining a morphologically matching bone defect entity model through design, and saving it in STL format;
[0102] Weigh 2 g collagen and 5 g chitosan, add 70 g of 0.05 mol / L acetic acid solution, place on a magnetic stirrer and stir at a rate of 150 r / min for 18 h to prepare a gel suspension to obtain a binder solution;
[0103] First, 35g of hydroxyapatite and 23g of calcium silicate are weighed, then 15g of bacterial cellulose powder and 76g of binder solution are added, and finally the raw materials are mixed to obtain a mixture, wherein the raw material components include 72.6wt% of bioceramic, 18.7wt% of bacterial cellulose, and 8.6wt% of binder;
[0104] The mixture was placed in a ball mill and milled at a speed of 150 r / min for 25 h to make the powder material particle size in the raw material reach the micro-nano level, and the raw materials were fully mixed to obtain a delicate and soft printing slurry;
[0105] The printing slurry was loaded into the dispensing syringe and centrifuged and degassed twice at 1800 rad / min, 5 min / time to obtain a uniform slurry.
[0106] The STL format file saved for the bone defect is loaded into the bioceramic 3D printing device, the barrel filled with the slurry is connected to the print head, the air pressure is adjusted to 0.4-0.5 MPa, the filling rate is set to 45%, the extrusion width is set to 0.6 mm, the STL format model slice file is run, and 3D printing is performed to obtain a blank;
[0107] The preform is placed in a freeze dryer to remove moisture and shape the preform through gradient freeze drying to obtain an artificial bone body;
[0108] Prepare a dispersion of carbon nanotubes and deionized water at a concentration of 8 μg / ml, add a small amount of carbon nanotube water dispersant after shaking, and shake well. Then place the dispersion in a water bath for 8 minutes of ultrasound, then place it in cold water for defoaming, and repeat ultrasound 5 times. Finally, immerse the shaped artificial bone body in the dispersed carbon nanotube dispersion for 4 hours and then take it out.
[0109] The artificial bone body after the coating treatment is placed in a 60° C. forced air oven for 3 hours to obtain a bioceramic / bacterial cellulose composite artificial bone with a porosity of 30% to 80%, a pore size of 400 μm to 1000 μm, and a connectivity rate greater than 98%;
[0110] The bioceramic / bacterial cellulose composite artificial bone prepared above is subjected to irradiation sterilization treatment to obtain a finished product.
[0111] Example 7
[0112] Obtaining a bone defect entity model: Using medical imaging technology to obtain the DICOM data of the patient's bone defect, and reconstructing the DICOM data in three dimensions, obtaining a morphologically matching bone defect entity model through design, and saving it in STL format;
[0113] Weigh 2 g collagen and 5 g chitosan, add 70 g of 0.05 mol / L acetic acid solution, place on a magnetic stirrer and stir at a rate of 150 r / min for 18 h to prepare a gel suspension to obtain a binder solution;
[0114] First, 13 g of β-tricalcium phosphate and 15 g of bioglass are weighed, and then 16 g of bacterial cellulose powder and 72 g of a binder solution are added, and finally the raw materials are mixed to obtain a mixture, wherein the raw material components include 55 wt % of bioceramic, 31.7 wt % of bacterial cellulose, and 12.9 wt % of the binder;
[0115] The mixture was placed in a ball mill and milled at a speed of 150 r / min for 34 hours to make the powder material particle size in the raw material reach the micro-nano level, and the raw materials were fully mixed to obtain a delicate and soft printing slurry;
[0116] The printing slurry was loaded into the dispensing syringe and centrifuged and degassed at 1800 rad / min, 5 min / time for 2 times to obtain a uniform slurry.
[0117] The STL format file saved for the bone defect is loaded into the bioceramic 3D printing device, the barrel filled with the slurry is connected to the print head, the air pressure is adjusted to 0.4-0.5 MPa, the filling rate is set to 45%, the extrusion width is set to 0.6 mm, the STL format model slice file is run, and 3D printing is performed to obtain a blank;
[0118] The preform is placed in a freeze dryer to remove moisture and shape the preform through gradient freeze drying to obtain an artificial bone body;
[0119] Prepare a dispersion of carbon nanotubes and deionized water at a concentration of 9 μg / ml, add a small amount of carbon nanotube water dispersant after shaking, and shake well. Then place the dispersion in a water bath for 7 minutes of ultrasound, then place it in cold water for defoaming, and repeat ultrasound 6 times. Finally, immerse the shaped artificial bone body in the dispersed carbon nanotube dispersion for 3 hours and then take it out.
[0120] The artificial bone body after the coating treatment is placed in a 60° C. forced air oven for 3 hours to obtain a bioceramic / bacterial cellulose composite artificial bone with a porosity of 30% to 80%, a pore size of 400 μm to 1000 μm, and a connectivity rate greater than 98%;
[0121] The bioceramic / bacterial cellulose composite artificial bone prepared above is subjected to irradiation sterilization treatment to obtain a finished product.
[0122] Example 8
[0123] Obtaining a bone defect entity model: Using medical imaging technology to obtain the DICOM data of the patient's bone defect, and reconstructing the DICOM data in three dimensions, obtaining a morphologically matching bone defect entity model through design, and saving it in STL format;
[0124] Weigh 8 g of polyethylene glycol, add deionized water thereto, stir at 75° C. until completely dissolved, and prepare a polyethylene glycol solution with a mass fraction of 11 wt %, thereby obtaining a binder solution;
[0125] First, 27g of hydroxyapatite and 16g of calcium carbonate are weighed, then 18g of bacterial cellulose powder and 60g of binder solution are added, and finally the raw materials are mixed to obtain a mixture, wherein the raw material components include 62wt% of bioceramic, 26.6wt% of bacterial cellulose, and 9.8wt% of binder;
[0126] The mixture was placed in a ball mill and milled at a speed of 150 r / min for 50 h to make the powder material particle size in the raw material reach the micro-nano level, and the raw materials were fully mixed to obtain a delicate and soft printing slurry;
[0127] The printing slurry was loaded into the dispensing syringe and centrifuged and degassed twice at 1800 rad / min, 5 min / time to obtain a uniform slurry.
[0128] The STL format file saved for the bone defect is loaded into the bioceramic 3D printing device, the barrel filled with the slurry is connected to the print head, the air pressure is adjusted to 0.4-0.5 MPa, the filling rate is set to 45%, the extrusion width is set to 0.6 mm, the STL format model slice file is run, and 3D printing is performed to obtain a blank;
[0129] The preform is placed in a freeze dryer to remove moisture and shape the preform through gradient freeze drying to obtain an artificial bone body;
[0130] Prepare a dispersion of carbon nanotubes and deionized water at a concentration of 10 μg / ml, add a small amount of carbon nanotube water dispersant after shaking, and shake well. Then place the dispersion in a water bath for 8 minutes of ultrasound, then place it in cold water for defoaming, and repeat ultrasound 5 times. Finally, immerse the shaped artificial bone body in the dispersed carbon nanotube dispersion for 4 hours and then take it out.
[0131] The artificial bone body after the coating treatment is placed in a 60° C. forced air oven for 3 hours to obtain a bioceramic / bacterial cellulose composite artificial bone with a porosity of 30% to 80%, a pore size of 400 μm to 1000 μm, and a connectivity rate greater than 98%;
[0132] The bioceramic / bacterial cellulose composite artificial bone prepared above is subjected to irradiation sterilization treatment to obtain a finished product.
[0133] Example 9
[0134] Obtaining a bone defect entity model: Using medical imaging technology to obtain the DICOM data of the patient's bone defect, and reconstructing the DICOM data in three dimensions, obtaining a morphologically matching bone defect entity model through design, and saving it in STL format;
[0135] Weigh 7.8 g of collagen, add 67 g of 0.05 mol / L acetic acid solution, place on a magnetic stirrer and stir at a rate of 150 r / min for 18 h to prepare a gel suspension to obtain a binder solution;
[0136] First, 20g of β-tricalcium phosphate and 27g of bioglass are weighed, then 8g of bacterial cellulose powder and 42g of binder solution are added, and finally the raw materials are mixed to obtain a mixture, wherein the raw material components include 79wt% of bioceramic, 13.5wt% of bacterial cellulose, and 7.5wt% of binder;
[0137] The mixture was placed in a ball mill and milled at a speed of 150 r / min for 72 hours to make the powder material particle size in the raw material reach the micro-nano level, and the raw materials were fully mixed to obtain a delicate and soft printing slurry;
[0138] The printing slurry was loaded into the dispensing syringe and centrifuged and degassed at 1800 rad / min, 5 min / time for 2 times to obtain a uniform slurry.
[0139] The STL format file saved for the bone defect is loaded into the bioceramic 3D printing device, the barrel filled with the slurry is connected to the print head, the air pressure is adjusted to 0.4-0.5 MPa, the filling rate is set to 45%, the extrusion width is set to 0.6 mm, the STL format model slice file is run, and 3D printing is performed to obtain a blank;
[0140] The preform is placed in a freeze dryer to remove moisture and shape the preform through gradient freeze drying to obtain an artificial bone body;
[0141] Prepare a dispersion of carbon nanotubes and deionized water at a concentration of 9 μg / ml, add a small amount of carbon nanotube water dispersant after shaking, and shake well. Then place the dispersion in a water bath for 7 minutes of ultrasound, then place it in cold water for defoaming, and repeat ultrasound 6 times. Finally, immerse the shaped artificial bone body in the dispersed carbon nanotube dispersion for 3 hours and then take it out.
[0142] The artificial bone body after the coating treatment is placed in a 60° C. forced air oven for 3 hours to obtain a bioceramic / bacterial cellulose composite artificial bone with a porosity of 60%, a pore size of 400 μm to 1000 μm, and a connectivity rate greater than 98%;
[0143] The bioceramic / bacterial cellulose composite artificial bone prepared above is subjected to irradiation sterilization treatment to obtain a finished product.
[0144] Example 10
[0145] Obtaining a bone defect entity model: Using medical imaging technology to obtain the DICOM data of the patient's bone defect, and reconstructing the DICOM data in three dimensions, obtaining a morphologically matching bone defect entity model through design, and saving it in STL format;
[0146] Weigh 3.8 g of polyethylene glycol, add deionized water thereto, stir at 75° C. until completely dissolved, and prepare a polyethylene glycol solution with a mass fraction of 11 wt %, thereby obtaining a binder solution;
[0147] First, 27g of hydroxyapatite and 27g of calcium carbonate are weighed, then 9g of bacterial cellulose powder and 50g of a binder solution are added, and finally the raw materials are mixed to obtain a mixture, wherein the raw material components include 78.8wt% of bioceramic, 13.1wt% of bacterial cellulose, and 8wt% of the binder;
[0148] The mixture was placed in a ball mill and milled at a speed of 150 r / min for 50 h to make the powder material particle size in the raw material reach the micro-nano level, and the raw materials were fully mixed to obtain a delicate and soft printing slurry;
[0149] The printing slurry was loaded into the dispensing syringe and centrifuged and degassed twice at 1800 rad / min, 5 min / time to obtain a uniform slurry.
[0150] The STL format file saved for the bone defect is loaded into the bioceramic 3D printing device, the barrel filled with the slurry is connected to the print head, the air pressure is adjusted to 0.4-0.5 MPa, the filling rate is set to 45%, the extrusion width is set to 0.6 mm, the STL format model slice file is run, and 3D printing is performed to obtain a blank;
[0151] The preform is placed in a freeze dryer to remove moisture and shape the preform through gradient freeze drying to obtain an artificial bone body;
[0152] Prepare a dispersion of carbon nanotubes and deionized water at a concentration of 10 μg / ml, add a small amount of carbon nanotube water dispersant after shaking, and shake well. Then place the dispersion in a water bath for 10 minutes of ultrasound, then place it in cold water for defoaming, and repeat ultrasound 3 times. Finally, immerse the shaped artificial bone body in the dispersed carbon nanotube dispersion for 4 hours and then take it out.
[0153] The artificial bone body after the coating treatment is placed in a 70° C. forced air oven for treatment for 5 hours to obtain a bioceramic / bacterial cellulose composite artificial bone with a porosity of 30% to 80%, a pore size of 400 μm to 1000 μm, and a connectivity greater than 98%;
[0154] The bioceramic / bacterial cellulose composite artificial bone prepared above is subjected to irradiation sterilization treatment to obtain a finished product.
[0155] Embodiment 11
[0156] The present invention also provides a use of the bioceramic / bacterial cellulose composite artificial bone as described in Examples 1 to 10 in preparing a bone defect repair material.
[0157] The bone defect repair material has excellent biocompatibility, mechanical properties, bone integration ability, etc., and the artificial bone has broad application prospects in the fields of orthopedic surgery, dental restoration, and orthopedic implants.
[0158] In summary, the present invention provides a bioceramic / bacterial cellulose composite artificial bone, a preparation method and an application thereof. By combining the effects of bacterial cellulose and a carbon nanotube layer, stress shielding can be effectively reduced, bone tissue absorption can be avoided, and the negative effects of bone repair materials can be avoided. At the same time, bone formation can be further promoted, and the mechanical properties of bone repair materials can be enhanced. Combined with 3D technology, the porosity, connectivity and uniformity of artificial bones can be precisely designed. Implants can be personalized according to patient needs, and the complex structural shape of the implant can be precisely controlled to achieve dual adaptation of the implant's appearance and mechanical properties to the body's own bones.
[0159] The above description is only a preferred embodiment of the present invention and is not intended to impose any limitation on the technical solution of the present invention. Those skilled in the art should understand that, without departing from the spirit and principles of the present invention, the technical solution can also be subjected to several simple modifications and substitutions, and these modifications and substitutions are also within the scope of protection covered by the claims.
Claims
1. A bioceramic / bacterial cellulose composite artificial bone, characterized in that: It comprises an artificial bone body, and a carbon nanotube layer is arranged on the outside of the artificial bone body; The raw material components of the artificial bone main body include: 53wt% to 84wt% of bioceramics, 10wt% to 32wt% of bacterial cellulose and 6wt% to 15wt% of a binder.
2. The bioceramic / bacterial cellulose composite artificial bone according to claim 1, characterized in that: The bioceramic is one or more of hydroxyapatite, β-tricalcium phosphate, calcium sulfate, calcium silicate, calcium carbonate and calcined bone powder.
3. The bioceramic / bacterial cellulose composite artificial bone according to claim 1, characterized in that: The binder is one or more of polyvinyl alcohol, polylactic acid, polyethylene glycol, polyglycolic acid, polyglycolic acid copolymer, chitosan, gelatin and collagen.
4. The bioceramic / bacterial cellulose composite artificial bone according to claim 1, characterized in that: Its porosity is 30% to 80% and its pore diameter is 400 to 1000 μm.
5. The bioceramic / bacterial cellulose composite artificial bone according to any one of claims 1 to 4, characterized in that: The thickness of the carbon nanotube layer is 0.05-0.3 mm.
6. A method for preparing a bioceramic / bacterial cellulose composite artificial bone, characterized in that: include: 53 wt% to 84 wt% of bioceramic, 10 wt% to 32 wt% of bacterial cellulose and 6 wt% to 15 wt% of a binder are uniformly mixed to obtain a slurry; The slurry is printed into a preliminary blank, and gradient freeze-dried to obtain an artificial bone body; A carbon nanotube layer is prepared on the outside of the artificial bone body to obtain a bioceramic / bacterial cellulose composite artificial bone.
7. The method for preparing the bioceramic / bacterial cellulose composite artificial bone according to claim 6, characterized in that: The method of gradient freeze drying is: The blank is placed at a temperature of -45°C to -1°C for pre-freezing; After the pre-freezing is completed, the pre-form is placed in a vacuum degree of 5 to 20 Pa and a temperature of -45°C to -30°C for freeze drying; After freeze-drying, the preform is placed in a vacuum condition of 5 Pa and 20°C to 35°C for analytical drying to complete gradient freeze-drying.
8. The method for preparing the bioceramic / bacterial cellulose composite artificial bone according to claim 6, characterized in that: The method for preparing the carbon nanotube layer outside the artificial bone body is: The artificial bone body is immersed in a carbon nanotube dispersion and dried to obtain a bioceramic / bacterial cellulose composite artificial bone; wherein the concentration of the carbon nanotube dispersion is 7-10 μg / mL.
9. The method for preparing the bioceramic / bacterial cellulose composite artificial bone according to claim 7, characterized in that: The artificial bone body is immersed in the carbon nanotube dispersion for 2 to 4 hours, and the drying temperature is 55° C. to 70° C.
10. Use of the bioceramic / bacterial cellulose composite artificial bone according to any one of claims 1 to 5 in preparing bone defect repair materials.
Citation Information
Patent Citations
A 3D-printed biomimetic porous bioceramic artificial bone and its preparation method
CN111070376B