Ultrathin flake silver powder and preparation method and application thereof

By adding polymers, reducing agents and surface treatment agents to the silver nitrate solution, adjusting the pH and adding inorganic salts, the problem of the cumbersome preparation process of flake silver powder in the existing technology is solved, and ultra-thin flakes with controllable morphology are prepared. Shape silver powder improves conductivity and printing performance and simplifies the process.

CN118848005APending Publication Date: 2024-10-29NANTONG T SUN NEW ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410897417.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In the existing technology, the preparation process of flake silver powder is cumbersome and it is difficult to accurately control the ball milling process, resulting in random morphology and coarse powder, which affects the conductivity and printing performance of the conductive paste.

Method used

Ultra-thin flaky silver powder with controllable morphology is prepared by adding polymers, reducing agents and surface treatment agents to the silver nitrate solution. By adjusting the pH and adding inorganic salts, the reaction conditions are controlled.

Benefits of technology

The preparation of ultra-thin flaky silver powder is achieved, with stable morphology, suitable for the conductivity and printing performance of conductive paste, simplifying the process, and suitable for industrial large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118848005A_ABST
    Figure CN118848005A_ABST
Patent Text Reader

Abstract

The invention provides ultrathin flaky silver powder and a preparation method and application thereof, and belongs to the technical field of conductive silver powder. The preparation method comprises the following steps: adding a high polymer, a reducing agent and a surface treating agent into a silver nitrate solution, and stirring for the first time to obtain a nano-silver seed crystal; adjusting the pH value of the silver nitrate solution to 3-4 to obtain a first reaction solution; inorganic salt is added into the reducing agent solution, a mixed solution is obtained through second stirring treatment, the nano-silver seed crystal is added into the mixed solution, and a second reaction solution is obtained; injecting the first reaction solution and the second reaction solution into a reaction container for reaction to obtain a product solution; and the product solution is subjected to precipitation, filtering separation, washing and drying treatment, and the ultrathin flake silver powder is obtained. A non-organic phase is used as a reaction system, the flaky silver powder with the controllable morphology is prepared through induction of inorganic salt and a surface treating agent, and meanwhile the morphology and the particle size of the silver powder can be controlled by adjusting the formula and parameters such as the concentration, the reaction time and the pH of all components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of conductive silver powder, and in particular relates to an ultra-thin flaky silver powder and a preparation method and application thereof. Background Art

[0002] With the rapid development of my country's electronic information, photovoltaic and other application markets, the demand for silver powder in my country has grown rapidly in recent years. The huge market demand has led to the continuous expansion of the silver powder and silver paste market in my country. Conductive silver powder is an environmentally friendly and efficient conductive material that meets the requirements of energy conservation and emission reduction. The country has proposed and implemented a series of policies to encourage enterprises to increase investment in the production of conductive silver powder and promote the research and development of conductive silver powder and the development of the industry.

[0003] The conductive phase used in the conductive paste is a key factor in the conversion efficiency of solar cells. The conductive phase required in the commonly used high-performance conductive paste is mainly silver powder. Silver powder has various shapes, and the silver powder used in conductive silver paste generally has two categories - flake silver powder and spherical silver powder. There are large differences in various performance indicators between the two, which directly affect the thixotropy, viscosity, conductivity, adhesion rate and other aspects of the finished silver paste.

[0004] At present, it is generally believed that compared with spherical silver powder, flaky silver powder has a larger specific surface area and better conductivity. Since the specific surface area of ​​flaky silver powder is relatively large, stable, and the oxidation degree and oxidation tendency are low, when forming a conductive layer, it will not only form surface-to-surface contact, but also repeated superposition of the upper and lower layers, so that the silver sheets are in close contact with each other to form a good conductive whole. Therefore, flaky silver powder is widely used in electronic components such as carbon film potentiometer terminals, membrane switches, filters, etc.

[0005] The preparation methods of flaky silver powder include chemical direct reduction method, evaporation coating stripping method, mechanical ball milling method, etc. At present, industrial production mainly adopts chemical method to prepare ultrafine silver powder, and then uses mechanical ball milling to prepare flaky silver powder. This method is cumbersome and difficult to accurately control the ball milling process. The morphology of flaky silver powder is random, and the flaky silver powder is still too coarse, resulting in insufficient filling amount of flaky silver powder in the conductive paste, and poor conductivity and printing performance of the conductive paste. Summary of the invention

[0006] The present disclosure aims to solve at least one of the technical problems existing in the prior art and provide an ultra-thin flaky silver powder and a preparation method and application thereof.

[0007] In one aspect of the present disclosure, a method for preparing ultra-thin flaky silver powder is provided.

[0008] The preparation method comprises:

[0009] Adding a polymer, a reducing agent and a surface treatment agent into a silver nitrate solution, and performing a first stirring treatment to obtain nano silver seed crystals;

[0010] Adjusting the pH of the silver nitrate solution to 3-4 to obtain a first reaction solution;

[0011] Adding an inorganic salt to the reducing agent solution, stirring for a second time to obtain a mixed solution, and adding the nano silver seed crystals to the mixed solution to obtain a second reaction solution;

[0012] injecting the first reaction solution and the second reaction solution into a reaction container to react and obtain a product solution;

[0013] The product solution is precipitated, filtered, separated, washed and dried to obtain ultra-thin flaky silver powder.

[0014] Optionally, the polymer is polyvinyl pyrrolidone.

[0015] Optionally, the surface treatment agent is H2O2.

[0016] Optionally, the reducing agent includes at least one of ascorbic acid, sodium ascorbate, glucose, formaldehyde, and sodium borohydride; and / or,

[0017] The inorganic salt is a sulfate, preferably at least one of iron sulfate, sodium sulfate, copper sulfate and potassium sulfate, more preferably potassium sulfate.

[0018] Optionally, the nano-silver seeds are added to the mixed solution in the form of a nano-silver seed solution, and the concentration of the nano-silver seed solution is 0.5-2 wt %.

[0019] Optionally, the polymer, the reducing agent, the surface treatment agent and the inorganic salt are all added in the form of a solution; wherein,

[0020] The concentration of the silver nitrate solution is 0.01-0.2M;

[0021] The concentration of the reducing agent solution is 0.1-0.5M;

[0022] The concentration of the inorganic salt solution is 0.2-1.2 mM;

[0023] The concentration of the surface treatment agent solution is 0.05-0.3 mM;

[0024] The concentration of the polymer solution is 0.01-0.1M.

[0025] Optionally, the volume ratio of the silver nitrate solution to the polymer solution, the reducing agent solution and the surface treatment agent solution is (45-55):(4-6):(1-3):1.

[0026] Optionally, the first stirring treatment lasts for 0.5-1.5 hours; and / or,

[0027] The second stirring treatment lasts for 10-20 minutes; and / or,

[0028] The reaction temperature is 20-30°C and the reaction time is 8-12 minutes.

[0029] In another aspect of the present disclosure, an ultra-thin flaky silver powder is provided, wherein the ultra-thin flaky silver powder is prepared by the preparation method described above; wherein:

[0030] The thickness of the ultra-thin flaky silver powder is 110-280 nm.

[0031] In another aspect of the present disclosure, an ultra-thin flaky silver powder as described above is provided for application in any one of photovoltaic, non-photovoltaic ITO, membrane switch, and touch screen.

[0032] The present disclosure proposes an ultra-thin flaky silver powder and a preparation method and application thereof, wherein the preparation method comprises: adding a polymer, a reducing agent and a surface treatment agent to a silver nitrate solution, and obtaining nano silver seeds after a first stirring treatment; adjusting the pH of the silver nitrate solution to 3-4 to obtain a first reaction solution; adding an inorganic salt to the reducing agent solution, and obtaining a mixed solution after a second stirring treatment, and adding the nano silver seeds to the mixed solution to obtain a second reaction solution; injecting the first reaction solution and the second reaction solution into a reaction container for reaction to obtain a product solution; precipitating, filtering, separating, washing and drying the product solution to obtain an ultra-thin flaky silver powder. The present disclosure uses a non-organic phase as a reaction system, and uses inorganic salts and surface treatment agents to induce the preparation of morphology-controllable flaky silver powder. At the same time, the morphology and particle size of the silver powder can be easily controlled by adjusting the formula and the concentration of each component, reaction time, pH and other process parameters during the reaction process. The process is simple and easy to realize industrial large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a flowchart of a method for preparing ultra-thin flaky silver powder according to an embodiment of the present disclosure;

[0034] Figure 2 This is an electron microscope image of the flaky silver powder prepared in Example 1 of the present disclosure;

[0035] Figure 3 This is an electron microscope image of the flaky silver powder prepared in Example 2 of the present disclosure;

[0036] Figure 4 This is an electron microscope image of the flaky silver powder prepared in Example 3 of the present disclosure;

[0037] Figure 5 This is an electron microscope image of the flaky silver powder prepared in Comparative Example 1 of the present disclosure;

[0038] Figure 6 This is an electron microscope image of the flaky silver powder prepared in Comparative Example 2 of the present disclosure. DETAILED DESCRIPTION

[0039] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the present disclosure is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be understood that the specific embodiments described herein are only used to explain the present disclosure and are not used to limit the disclosure. The described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present disclosure.

[0040] like Figure 1 As shown, in one aspect of the present disclosure, a method for preparing ultra-thin flaky silver powder S100 is provided, which specifically comprises the following steps S110 to S150:

[0041] S110, adding a polymer, a reducing agent and a surface treatment agent to the silver nitrate solution, and performing a first stirring treatment to obtain nano silver seed crystals.

[0042] It should be noted that the present embodiment does not specifically limit the method of adding the polymer, reducing agent and surface treatment agent. For example, the corresponding reagents can be directly added to the silver nitrate solution, or the corresponding reagents can be first dissolved in a solvent to form a solution, and then the solution is added to the silver nitrate solution to mix the components evenly.

[0043] It should be further explained that the polymer, reducing agent and surface treatment agent should be quickly added to the silver nitrate solution, that is, the polymer solution, reducing agent solution and surface treatment agent solution should be quickly added to the nitrate solution and stirred for 0.5-1.5h to form nano silver seeds.

[0044] It should be understood that the nano silver seeds formed in this embodiment can be used as a crystal inducing agent to control the morphology of silver powder and the direction of crystal growth during the preparation of flaky silver powder, thereby promoting the formation of flaky silver powder.

[0045] In some preferred embodiments, when the polymer, reducing agent and surface treatment agent are all added in the form of solutions, the polymer, reducing agent and surface treatment agent are first dissolved in pure water to form corresponding solutions, and then the corresponding solutions are added to the silver nitrate solution in sequence. At this time, the volume ratio of the silver nitrate solution to the polymer solution, reducing agent and surface treatment agent is preferably (45-55):(4-6):(1-3):1. The crystal inducing agent formed within this ratio range is conducive to controlling the crystal growth direction.

[0046] As a further preferred embodiment, the volume ratio of the silver nitrate solution to the polymer solution, the reducing agent solution and the surface treatment agent solution is 50:5:2:1.

[0047] As a further preferred solution, the volume of the silver nitrate solution is preferably 100 mL, the volume of the polymer solution is preferably 10 mL, the volume of the reducing agent solution is preferably 4 mL, and the volume of the surface treatment agent is preferably 2 mL. Of course, in other preferred embodiments, other volumes can also be selected according to actual needs, and this is not specifically limited.

[0048] In other preferred embodiments, the silver nitrate solution can be formed by dissolving at least one of water-soluble silver salts such as silver nitrate, oxalate, silver fluoride, silver sulfate, and silver perchlorate in pure water. In addition, the concentration of the silver nitrate solution can be preferably 0.01-0.2M, for example, 0.01M, 0.02M, 0.05M, 0.07M, 0.1M, 0.15M, 0.2M, etc.

[0049] In other preferred embodiments, the reducing agent solution may be formed by dissolving at least one reducing agent selected from ascorbic acid, sodium ascorbate, glucose, formaldehyde, and sodium borohydride in pure water. In addition, the concentration of the reducing agent solution may preferably be 0.1-0.5M, for example, 0.1M, 0.2M, 0.3M, 0.4M, 0.5M, etc.

[0050] As a further preferred embodiment, in step S110, the reducing agent may preferably be sodium borohydride.

[0051] In this embodiment, by adding a reducing agent such as sodium borohydride to the crystal inducing agent, the silver nitrate can be partially reduced by utilizing its strong reducing property to form silver particles with a size of nanometer level.

[0052] In other preferred embodiments, the polymer solution may be formed by dissolving polyvinylpyrrolidone (PVP) in pure water. In addition, the concentration of the polymer solution may preferably be 0.01-0.1M, for example, 0.01M, 0.03M, 0.05M, 0.08M, 0.1M, etc.

[0053] In this embodiment, by adding a polymer solution to the crystal inducing agent, the dispersibility of the silver powder is increased, and the growth of the silver powder along the {111} direction of the crystal plane is controlled.

[0054] In other preferred embodiments, the surface treatment agent solution may be formed by dissolving H2O2 in pure water. In addition, the concentration of the surface treatment agent solution may preferably be 0.05-0.3 mM, for example, 0.05 mM, 0.1 mM, 0.2 mM, 0.3 mM.

[0055] In this embodiment, by adding H2O2 to the crystal inducing agent, it is helpful to control the morphology of the silver powder, etch the surface of the silver powder, and control the crystal growth direction.

[0056] S120, adjusting the pH of the silver nitrate solution to 3-4 to obtain a first reaction solution.

[0057] In some preferred embodiments, the volume of silver nitrate in step S120 is preferably 90-110 mL, for example, 90 mL, 100 mL, 120 mL, etc. Secondly, the concentration of silver nitrate may also be preferably 0.01-0.2M.

[0058] It should be noted that the present embodiment does not specifically limit the reagent used to adjust the pH of the solution. For example, nitric acid is used, that is, a certain amount of nitric acid is added to the silver nitrate solution, the pH of the solution is adjusted to 3-4, and after mechanical stirring and sufficient dissolution, a first reaction solution is obtained.

[0059] In other preferred embodiments, the pH value may be preferably 3, 3.5, 4, etc.

[0060] S130, adding an inorganic salt to the reducing agent solution, stirring for a second time to obtain a mixed solution, and adding nano silver seed crystals to the mixed solution to obtain a second reaction solution.

[0061] Specifically, an inorganic salt is added to the reducing agent solution and mechanically stirred for 10-20 min, for example, 10 min, 12 min, 15 min, 18 min, 20 min, etc., to fully dissolve the inorganic salt, and then the nanosilver seeds prepared in step S110 are added to the mixed solution.

[0062] In some preferred embodiments, the volume of the reducing agent solution may preferably be 90-110 mL, for example, 90 mL, 100 mL, 110 mL, etc., the concentration of the reducing agent solution may also preferably be 0.1-0.5 M, and the type of the reducing agent may preferably be at least one of ascorbic acid, sodium ascorbate, glucose, formaldehyde, and sodium borohydride.

[0063] As a further preferred solution, in step S130, the reducing agent solution may preferably be an ascorbic acid solution.

[0064] It should also be noted that the present embodiment does not specifically limit the method of adding the inorganic salt. For example, it can be directly added to the silver nitrate solution. Alternatively, the inorganic salt can be first dissolved in a solvent to form a solution, and then the solution is added to the silver nitrate solution to mix the components evenly.

[0065] In other preferred embodiments, the inorganic salt solution is a sulfate solution, preferably formed by dissolving at least one of iron sulfate, sodium sulfate, copper sulfate, and potassium sulfate in pure water, and its concentration may preferably be 0.2-1.2 mM, for example, 0.2 mM, 0.5 mM, 0.8 mM, 1.0 mM, 1.2 mM, etc.

[0066] As a further preferred solution, in step S130, the inorganic salt solution may preferably be a potassium sulfate solution.

[0067] In this embodiment, the inorganic salt plays a role in modifying the morphology of the silver flakes, which can make the morphology of the flaky silver powder more regular and the surface of the silver flakes smoother.

[0068] In other preferred embodiments, the nanosilver seeds are added to the mixed solution in the form of a nanosilver seed solution, and the concentration of the nanosilver seed solution may preferably be 0.5-2wt%, for example, 0.5wt%, 1wt%, 1.5wt%, 2wt%.

[0069] S140, injecting the first reaction solution and the second reaction solution into a reaction container for reaction to obtain a product solution.

[0070] Specifically, the first reaction solution and the second reaction solution are injected into a constant temperature reactor at a rate of 0.1 L / min-0.5 L / min by a peristaltic pump, the reaction temperature is 20-30° C., and the reaction is stirred for 8-12 minutes to obtain a light yellow solution, i.e., the product solution.

[0071] In some preferred embodiments, the reaction temperature is preferably 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 28°C, 30°C, and the reaction time is preferably 8 min, 9 min, 10 min, etc.

[0072] S150, precipitating, filtering, separating, washing and drying the product solution to obtain ultra-thin flaky silver powder.

[0073] Specifically, the product solution obtained in step S140 is precipitated for 24 hours, filtered and separated, washed with pure water for 2-4 times, and dried to obtain pure ultra-thin flaky silver powder.

[0074] In this embodiment, a non-organic phase is used as the reaction system, and inorganic salts and surface treatment agents are induced to prepare morphology-controllable flaky silver powder. At the same time, the shape of the silver powder flakes can be adjusted by controlling the amount of each component to obtain ultra-thin flaky silver powder. The silver powder has a stable morphology and can meet the conductivity and printing performance of the conductive paste.

[0075] In another aspect of the present disclosure, an ultra-thin flaky silver powder is provided. The ultra-thin flaky silver powder is prepared by the preparation method described above. For the specific preparation process, please refer to the above description and will not be repeated here.

[0076] In some preferred embodiments, the thickness of the ultra-thin flaky silver powder (hereinafter referred to as the flake thickness) is 110-280 nm, preferably 110-130 nm. The particle size D10 of the ultra-thin flaky silver powder is 0.8-1.3 μm, preferably 0.9-1.2 μm, more preferably 0.94-1.18 μm, the particle size D50 is 1.4-2.8 μm, preferably 1.5-2.75 μm, more preferably 1.56-2.72 μm, the particle size D90 is 2.8-8.6 μm, preferably 2.9-8.5 μm, preferably 3.01-8.45 μm, and the particle size D95 is 3-12 μm, preferably 3.5-11.9μm, more preferably 3.56-11.83μm, particle size D98 is 4-16μm, preferably 4.6-15.8μm, preferably 4.66-15.74μm, particle size D100 is 7-29μm, preferably 7.4-28.3μm, more preferably 7.48-28.18μm, span is 1.2-2.8μm, preferably 1.25-2.7μm, more preferably 1.30-2.66μm.

[0077] Another aspect of the present disclosure provides a method for applying ultra-thin flaky silver powder to any one of photovoltaic, non-photovoltaic ITO, membrane switch, and touch screen.

[0078] It should be understood that the ultra-thin flaky silver powder can be added to the conductive paste as a conductive component, and various devices can be formed by printing the conductive paste on a substrate. For example, a membrane switch can be formed by printing a contact circuit on a film such as polycarbonate, polyvinyl chloride or polyethylene with a conductive paste.

[0079] The preparation method of ultra-thin flaky silver powder and the parameters of the silver powder will be further described below in conjunction with several specific examples:

[0080] Example 1

[0081] The method for preparing the ultra-thin flaky silver powder in this example comprises the following steps:

[0082] S1. Rapidly add 10 mL 0.05 M PVP, 4 mL 0.15 M NaBH4, and 2 mL 0.1 mM H2O2 to 100 mL pure water containing 0.05 M AgNO3 and stir for 1 hour to obtain nanosilver seeds.

[0083] S2. Add a certain amount of nitric acid to 100 mL of 0.05 M AgNO3 solution to adjust the pH to 3.5, and stir mechanically to fully dissolve to obtain a first reaction solution.

[0084] S3, prepare 100 mL of 0.15 M ascorbic acid solution, add 1.0 mM potassium sulfate solution, and mechanically stir for 15 min to fully dissolve it to obtain a mixed solution; add the nano silver seeds prepared in step S1 to the mixed solution at a concentration of 0.5 wt %, to obtain a second reaction solution.

[0085] S4. The first reaction solution and the second reaction solution were injected into the thermostatic reactor at a rate of 0.2 L / min by a peristaltic pump. The reaction temperature was 23° C. and the reaction was stirred for 10 min to obtain a light yellow solution.

[0086] S5. The light yellow solution obtained in step S5 is precipitated for 24 hours, filtered and separated, washed with pure water for 2-4 times, and dried to obtain pure silver flakes.

[0087] like Figure 2 As shown, the silver powder has a flaky structure and a high flaking rate. As shown in Table 1, the laser particle size D10 = 0.94 μm, the laser particle size D50 = 1.56 μm, the laser particle size D90 = 3.01 μm, the laser particle size D95 = 3.56 μm, the laser particle size D98 = 4.66 μm, the laser particle size D100 = 7.48 μm, the span is 1.31, and the flake thickness is 110 nm.

[0088] Example 2

[0089] The method for preparing the ultra-thin flaky silver powder in this example comprises the following steps:

[0090] S1. Rapidly add 10 mL 0.05 M PVP, 4 mL 0.15 M NaBH4, and 2 mL 0.1 mM H2O2 to 100 mL pure water containing 0.1 M AgNO3 and stir for 1 hour to obtain nanosilver seeds.

[0091] S2. Add a certain amount of nitric acid to 100 mL of 0.05 M AgNO3 solution to adjust the pH to 3.5, and stir mechanically to fully dissolve to obtain a first reaction solution.

[0092] S3, prepare 100 mL of 0.15 M ascorbic acid solution, add 1.0 mM potassium sulfate solution, and mechanically stir for 15 min to fully dissolve it to obtain a mixed solution; add the nano silver seeds prepared in step S1 to the mixed solution at a concentration of 0.5 wt %, to obtain a second reaction solution.

[0093] S4. The first reaction solution and the second reaction solution were injected into the thermostatic reactor at a rate of 0.2 L / min by a peristaltic pump. The reaction temperature was 23° C. and the reaction was stirred for 10 min to obtain a light yellow solution.

[0094] S5. The light yellow solution obtained in step S5 is precipitated for 24 hours, filtered and separated, washed with pure water for 2-4 times, and dried to obtain pure silver flakes.

[0095] like Figure 3 As shown, the silver powder has a flaky structure. As shown in Table 1, the laser particle size D10 = 0.95 μm, the laser particle size D50 = 1.72 μm, the laser particle size D90 = 3.19 μm, the laser particle size D95 = 3.84 μm, the laser particle size D98 = 4.68 μm, the laser particle size D100 = 8.13 μm, the span is 1.30, and the flake thickness is 280 nm.

[0096] Compared with Example 1, the concentration of silver nitrate is increased in Example 2, and the prepared flaky silver powder is thicker than the flaky silver powder in Example 1.

[0097] Example 3

[0098] The method for preparing the ultra-thin flaky silver powder in this example comprises the following steps:

[0099] S1. Rapidly add 10 mL 0.05 M PVP, 4 mL 0.15 M NaBH4, and 2 mL 0.1 mM H2O2 to 100 mL pure water containing 0.05 M AgNO3 and stir for 1 hour to obtain nanosilver seeds.

[0100] S2. Add a certain amount of nitric acid to 100 mL of 0.05 M AgNO3 solution to adjust the pH to 3.5, and stir mechanically to fully dissolve to obtain a first reaction solution.

[0101] S3, prepare 100 mL of 0.15 M ascorbic acid solution, add 1.0 mM potassium sulfate solution, and mechanically stir for 15 min to fully dissolve it to obtain a mixed solution; add the nano silver seeds prepared in step S1 to the mixed solution at a concentration of 1.5 wt % to obtain a second reaction solution.

[0102] S4. The first reaction solution and the second reaction solution were injected into the thermostatic reactor at a rate of 0.2 L / min by a peristaltic pump. The reaction temperature was 23° C. and the reaction was stirred for 10 min to obtain a light yellow solution.

[0103] S5. The light yellow solution obtained in step S5 is precipitated for 24 hours, filtered and separated, washed with pure water for 2-4 times, and dried to obtain pure silver flakes.

[0104] like Figure 4 As shown, the silver powder has a flaky structure. Compared with Example 1, the amount of the seed inducer is adjusted in Example 3. The increased concentration of the seed inducer makes the stacking phenomenon of the flaky silver powder more obvious than that in Example 1.

[0105] As shown in Table 1, the laser particle size D10 = 1.18 μm, the laser particle size D50 = 2.72 μm, the laser particle size D90 = 8.45 μm, the laser particle size D95 = 11.83 μm, the laser particle size D98 = 15.74 μm, the laser particle size D100 = 28.18 μm, the span is 2.66, and the sheet thickness is 130 nm.

[0106] Comparative Example 1

[0107] The method for preparing the ultra-thin flaky silver powder in this example comprises the following steps:

[0108] S1. Rapidly add 10 mL 0.05 M PVP and 4 mL 0.15 M NaBH4 to 100 mL pure water containing 0.1 M AgNO3 and stir for 1 hour to obtain nanosilver seeds.

[0109] S2. Add a certain amount of nitric acid to 100 mL of 0.05 M AgNO3 solution to adjust the pH to 3.5, and stir mechanically to fully dissolve to obtain a first reaction solution.

[0110] S3, prepare 100 mL of 0.15 M ascorbic acid solution, add 1.0 mM potassium sulfate solution, and mechanically stir for 15 min to fully dissolve it to obtain a mixed solution; add the nano silver seeds prepared in step S1 to the mixed solution at a concentration of 0.5 wt %, to obtain a second reaction solution.

[0111] S4. The first reaction solution and the second reaction solution were injected into the thermostatic reactor at a rate of 0.2 L / min by a peristaltic pump. The reaction temperature was 23° C. and the reaction was stirred for 10 min to obtain a light yellow solution.

[0112] S5. The light yellow solution obtained in step S5 is precipitated for 24 hours, filtered and separated, washed with pure water for 2-4 times, and dried to obtain pure silver flakes.

[0113] like Figure 5 As shown in Table 1, the silver powder is almost elliptical. As shown in Table 1, the laser particle size D10 = 1.07 μm, the laser particle size D50 = 1.87 μm, the laser particle size D90 = 3.39 μm, the laser particle size D95 = 4.20 μm, the laser particle size D98 = 6.60 μm, the laser particle size D100 = 16.73 μm, the span is 1.24, and the sheet thickness is 450 nm.

[0114] Compared with Examples 1-3, in the preparation process of the seed inducer in step S1 of this comparative example 1, H2O2 was not added, the prepared flaky silver powder had a low flake rate, and the thickness of the silver powder was much higher than that of the flaky silver powder in Examples 1-3.

[0115] Comparative Example 2

[0116] The method for preparing the ultra-thin flaky silver powder in this example comprises the following steps:

[0117] S1. Rapidly add 10 mL 0.05 M PVP, 4 mL 0.15 M NaBH4, and 2 mL 0.1 mM H2O2 to 100 mL pure water containing 0.1 M AgNO3 and stir for 1 hour to obtain nanosilver seeds.

[0118] S2. Add a certain amount of nitric acid to 100 mL of 0.05 M AgNO3 solution to adjust the pH to 3.5, and stir mechanically to fully dissolve to obtain a first reaction solution.

[0119] S3, preparing 100 mL of 0.15 M ascorbic acid solution, mechanically stirring for 15 min to fully dissolve it, to obtain a mixed solution; adding the nano silver seeds prepared in step S1 to the mixed solution at a concentration of 0.5 wt %, to obtain a second reaction solution.

[0120] S4. The first reaction solution and the second reaction solution were injected into the thermostatic reactor at a rate of 0.2 L / min by a peristaltic pump. The reaction temperature was 23° C. and the reaction was stirred for 10 min to obtain a light yellow solution.

[0121] S5. The light yellow solution obtained in step S5 is precipitated for 24 hours, filtered and separated, washed with pure water for 2-4 times, and dried to obtain pure silver flakes.

[0122] like Figure 6 As shown in Table 1, the silver powder is in the form of flakes with a rough surface. As shown in Table 1, the laser particle size D10 = 1.55 μm, the laser particle size D50 = 1.95 μm, the laser particle size D90 = 4.91 μm, the laser particle size D95 = 6.80 μm, the laser particle size D98 = 12.42 μm, the laser particle size D100 = 18.43 μm, the span is 1.25, and the flake thickness is 470 nm.

[0123] Compared with Examples 1-3, in the preparation process of the seed inducer in step S1 of this comparative example 2, no inorganic salt is added, the surface of the prepared flaky silver powder is rough, and the flaking rate is low, and the thickness of the silver powder is much higher than the thickness of the flaky silver powder in Examples 1-3.

[0124] Table 1 Silver powder particle size and sheet thickness obtained in each embodiment and comparative example

[0125]

[0126] The present disclosure proposes an ultra-thin flaky silver powder and a preparation method and application thereof, which have the following beneficial effects compared with the prior art: the present disclosure adopts a liquid phase chemical reduction method to obtain ultra-thin flaky silver powder, which has the advantages of simple equipment, low preparation cost, low energy consumption, etc. During the reaction process, the morphology and particle size of the silver powder can be easily controlled by adjusting the formulation components and the concentration of each component, the reaction time, the pH value and other process parameters, which is conducive to obtaining ultra-thin flaky silver powder. The process is simple and easy to realize industrial large-scale production.

[0127] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present disclosure, but the present disclosure is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and substance of the present disclosure, and these modifications and improvements are also considered to be within the scope of protection of the present disclosure.

Claims

1. A method for preparing ultra-thin flaky silver powder, characterized in that: The preparation method comprises: Adding a polymer, a reducing agent and a surface treatment agent into a silver nitrate solution, and performing a first stirring treatment to obtain nano silver seed crystals; Adjusting the pH of the silver nitrate solution to 3-4 to obtain a first reaction solution; Adding an inorganic salt to the reducing agent solution, stirring for a second time to obtain a mixed solution, and adding the nano silver seed crystals to the mixed solution to obtain a second reaction solution; injecting the first reaction solution and the second reaction solution into a reaction container to react and obtain a product solution; The product solution is precipitated, filtered, separated, washed and dried to obtain ultra-thin flaky silver powder.

2. The preparation method according to claim 1, characterized in that: The polymer is polyvinyl pyrrolidone.

3. The preparation method according to claim 1, characterized in that: The surface treatment agent is H2O2.

4. The preparation method according to claim 1, characterized in that: The reducing agent includes at least one of ascorbic acid, sodium ascorbate, glucose, formaldehyde, and sodium borohydride; and / or, The inorganic salt is sulfate.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The nano silver seeds are added to the mixed solution in the form of a nano silver seed solution, and the concentration of the nano silver seed solution is 0.5-2 wt %.

6. The preparation method according to any one of claims 1 to 4, characterized in that: The polymer, the reducing agent, the surface treatment agent and the inorganic salt are all added in the form of a solution; wherein, The concentration of the silver nitrate solution is 0.01-0.2M; The concentration of the reducing agent solution is 0.1-0.5M; The concentration of the inorganic salt solution is 0.2-1.2 mM; The concentration of the surface treatment agent solution is 0.05-0.3 mM; The concentration of the polymer solution is 0.01-0.1M.

7. The preparation method according to claim 6, characterized in that: The volume ratio of the silver nitrate solution to the polymer solution, the reducing agent solution and the surface treatment agent solution is (45-55):(4-6):(1-3):

1.

8. The preparation method according to any one of claims 1 to 4, characterized in that: The first stirring treatment lasts for 0.5-1.5 hours; and / or, The second stirring treatment lasts for 10-20 minutes; and / or, The reaction temperature is 20-30°C and the reaction time is 8-12 minutes.

9. An ultra-thin flaky silver powder, characterized in that: The ultra-thin flaky silver powder is prepared by the preparation method according to any one of claims 1 to 8; wherein The thickness of the ultra-thin flaky silver powder is 110-280 nm.

10. The ultra-thin flaky silver powder as claimed in claim 9 is used in any one of photovoltaic, non-photovoltaic ITO, membrane switch and touch screen.