Novel welding method

By adding steps such as pre-bending, heat treatment and multiple cutting in the welding process, the welding process is optimized, the problems of micro-cracks and material waste in guide rail welding are solved, and cost reduction and product quality are improved.

CN118848434APending Publication Date: 2024-10-29FNS(NANJING) SURFACE ENG TECH CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202410949416.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

When welding 310 and Co21 with T800 on guide rail A105N, micro-cracks, slag inclusion defects and material waste are prone to occur, resulting in increased processing costs.

Method used

By increasing the welding process and detection means, we perform raw material pre-bending, transition layer welding, heat treatment, wire cutting and multiple grinding, optimize the welding process, control product thickness and deformation, and reduce material and processing costs.

Benefits of technology

It effectively reduces material waste and processing costs by more than 30%, improves product quality, and reduces operational complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004946741040000011
    Figure HDA0004946741040000011
  • Figure HDA0004946741040000012
    Figure HDA0004946741040000012
  • Figure HDA0004946741040000013
    Figure HDA0004946741040000013
Patent Text Reader

Abstract

The invention discloses a novel welding method. A guide rail A105N raw material is pre-bent; welding a transition layer: surfacing a side surface 310 and a front surface Co21; performing linear cutting after the surfacing of the side surface 310 and the surfacing of the Co21 transition layer on the front surface are finished; raising two ends of the guide rail for heat treatment; preheating before welding; surfacing machining is carried out, wherein T800 surfacing is carried out; raising two ends of the guide rail for heat treatment; arc starting and arc extinguishing ends are arranged on the two sides of the length direction of the guide rail, allowance is removed through cutting, a surfacing face of 310 is cut and welded, a T800 alloy face of the guide rail is linearly cut to be bright, and the middle of the guide rail in the thickness direction is divided into two parts; grinding: grinding the surface and the back surface of the T800 alloy on a grinding machine; linear cutting: carrying out linear cutting on assembly surfaces at two ends of the guide rail and cutting peripheral arc angles of the guide rail; the guide rail is polished to be bright, and a product meeting the requirement is obtained. Welding defects are reduced, the workpiece is subjected to reversible deformation pre-bending, the product thickness is controlled, and the material cost and the machining cost are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of welding, and in particular to a novel welding method. Background Art

[0002] Under the existing conditions, when the guide rail A105N is welded with 310+Co21+T800, micro cracks are easily generated in the 310 area after processing, and it is easy to be pulled apart and cracked under stress conditions. Welding T800 on Co21 is prone to slag inclusion defects. For guide rail products, the product size needs to be increased to reduce product deformation, but such operations cause waste and increase processing costs.

[0003] The welding of the original long guide rails requires more than double the thickness of the parent material, or divide it into different small sections, which undoubtedly increases the processing cost and material cost. Therefore, it is necessary to develop new welding methods to reduce welding defects and reduce material and processing costs. Summary of the invention

[0004] Purpose of the invention: In view of the shortcomings and defects of the prior art, the present invention provides a new welding method, which increases the welding process, optimizes the welding process, adds detection means at different stages of welding, reduces welding defects, performs anti-deformation pre-bending on the workpiece, controls the product thickness, and reduces material costs and processing costs.

[0005] Technical solution: A novel welding method of the present invention is characterized by comprising the following steps:

[0006] 1) Pre-bending of raw materials: Pre-bend the raw materials of guide rail A105N by 17mm-30mm;

[0007] 2) Transition layer welding: 310 on the side and Co21 on the front;

[0008] 3) Wire cutting of transition layer: Wire cutting is performed after the 310 surfacing of the side and the Co21 transition layer surfacing of the front;

[0009] 4) Heat treatment: The two ends of the guide rail are raised for heat treatment;

[0010] 5) OP40 preheating before welding: preheating temperature is 550℃;

[0011] 6) Overlay welding: T800 overlay welding;

[0012] 7) Post-weld heat treatment: raise both ends of the guide rail for heat treatment;

[0013] 8) Wire cutting: arc starting and arc stopping ends on both sides of the guide rail, and cut to remove the excess;

[0014] 9) Secondary wire cutting: cutting the cladding surface of welding 310;

[0015] 10) Three-time wire cutting: wire cutting guide rail T800 alloy surface exposed to light;

[0016] 11) Four times wire cutting: the guide rail is divided into two in the middle along the thickness direction;

[0017] 12) Grinding: Grinding on T800 alloy surface and back side;

[0018] 13) Five times of wire cutting: wire cutting of the assembly surfaces at both ends of the guide rail;

[0019] 14) Sixth wire cutting: cutting the arc angle around the guide rail;

[0020] 15) Secondary grinding: The guide rail is polished to obtain a product that meets the requirements.

[0021] Wherein, during the heat treatment in step 4), the heat treatment temperature is 720°C, the heating rate is 80°C / h, the temperature is kept for 4 hours, and the furnace is cooled.

[0022] Wherein, in the step 5), the PT developer must be polished clean before the OP40 is preheated before welding and entering the furnace.

[0023] Wherein, in step 6), the arc of T800 cladding on both sides must be closed on the same side.

[0024] Wherein, during the heat treatment in step 7), the heat treatment temperature is 720°C, the heating rate is 80°C / h, the temperature is kept for 4 hours, and the furnace is cooled.

[0025] Wherein, in the step 9), two sides of the cladding surface of the weld 310 are cut.

[0026] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: by increasing welding procedures, optimizing welding processes, adding detection means at different stages of welding, reducing welding defects, pre-bending the workpiece for reverse deformation, controlling product thickness, and reducing material costs and processing costs. According to testing, the present invention reduces material waste and processing costs by more than 30%; improves product quality and reduces operating requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The product defects of A105N welding 310+Co21+T800 in the prior art Figure 1 ;

[0028] Figure 2 The product defects of A105N welding 310+Co21+T800 in the prior art Figure 2 ;

[0029] Figure 3 This is a schematic diagram of the raw material pre-bending structure of the present invention;

[0030] Figure 4 is a schematic diagram of the heat treatment of the present invention;

[0031] Figure 5 It is a schematic diagram of the product of the present invention. DETAILED DESCRIPTION

[0032] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and specific implementation methods.

[0033] In the present invention, A105N is a steel material with the grade A105N; 310 is a steel material with the grade 310; Co21 is a cobalt-based material with the grade ERCoCr-E; OP40 is the name of the preheating process before welding; and T800 is a cobalt-based material with the grade T800.

[0034] The novel welding method of the present invention is characterized in that it comprises the following steps:

[0035] 1) Pre-bending of raw materials: Pre-bend the raw materials of guide rail A105N by 17mm-30mm;

[0036] 2) Transition layer welding: 310 on the side and Co21 on the front;

[0037] 3) Wire cutting of transition layer: Wire cutting is performed after the 310 surfacing of the side and the Co21 transition layer surfacing of the front;

[0038] 4) Heat treatment: The two ends of the guide rail are raised for heat treatment; the heat treatment temperature is 720℃, the heating rate is 80℃ / h, the temperature is kept for 4h, and the furnace is cooled;

[0039] 5) OP40 preheating before welding: the preheating temperature is 550℃; the PT developer must be polished clean before entering the furnace;

[0040] 6) Overlay welding: Perform T800 overlay welding; the arc of T800 overlay welding on both sides must be closed on the same side;

[0041] 7) Post-weld heat treatment: The two ends of the guide rail are raised for heat treatment; the heat treatment temperature is 720℃, the heating rate is 80℃ / h, the temperature is kept for 4h, and the furnace is cooled;

[0042] 8) Wire cutting: arc starting and arc stopping ends on both sides of the guide rail, and cut to remove the excess;

[0043] 9) Secondary wire cutting: cutting the cladding surface (both sides) of welding 310;

[0044] 10) Three-time wire cutting: wire cutting guide rail T800 alloy surface exposed to light;

[0045] 11) Four times wire cutting: the guide rail is divided into two in the middle along the thickness direction;

[0046] 12) Grinding: Grinding on T800 alloy surface and back side;

[0047] 13) Five times of wire cutting: wire cutting of the assembly surfaces at both ends of the guide rail;

[0048] 14) Sixth wire cutting: cutting the arc angle around the guide rail;

[0049] 15) Secondary grinding: The guide rail is polished to obtain a product that meets the requirements.

[0050] The present invention pre-bends the raw material of the guide rail A105N by 17mm-30mm to ensure the welding deformation, control the welding heat input, and match the deformation to achieve the deformation after welding to meet the requirements. After the transition layer welding is completed, the present invention promptly performs stress relief heat treatment on the workpiece. The product is subjected to high temperature and long-term aging to ensure the elimination of welding stress, which not only guarantees the minimization of the subsequent deformation of the workpiece, but also reduces the requirements for subsequent heat input. At the end of the final welding of the product, the present invention performs stress relief treatment on the product again to reduce the rebound during the processing and ensure the effective coating thickness and performance of the product.

Claims

1. A new welding method, characterized in that: The steps include: 1) Pre-bending of raw materials: Pre-bend the raw materials of guide rail A105N by 17mm-30mm; 2) Transition layer welding: 310 on the side and Co21 on the front; 3) Wire cutting of transition layer: Wire cutting is performed after the 310 surfacing of the side and the Co21 transition layer surfacing of the front; 4) Heat treatment: The two ends of the guide rail are raised for heat treatment; 5) Preheating before welding: preheating temperature is 550℃; 6) Overlay welding: T800 overlay welding; 7) Post-weld heat treatment: raise both ends of the guide rail for heat treatment; 8) Wire cutting: arc starting and arc stopping ends on both sides of the guide rail, and cut to remove the excess; 9) Secondary wire cutting: cutting the cladding surface of welding 310; 10) Three-time wire cutting: wire cutting guide rail T800 alloy surface exposed to light; 11) Four times wire cutting: the guide rail is divided into two in the middle along the thickness direction; 12) Grinding: Grinding on T800 alloy surface and back side; 13) Five times of wire cutting: wire cutting of the assembly surfaces at both ends of the guide rail; 14) Sixth wire cutting: cutting the arc angle around the guide rail; 15) Secondary grinding: The guide rail is polished to obtain a product that meets the requirements.

2. The novel welding method according to claim 1 is characterized in that: During the heat treatment in step 4), the heat treatment temperature is 720°C, the heating rate is 80°C / h, the temperature is kept for 4 hours, and the furnace is cooled.

3. The novel welding method according to claim 1 is characterized in that: In the step 5), the PT developer must be polished clean before being preheated and put into the furnace before welding.

4. The novel welding method according to claim 1 is characterized in that: In step 6), the arc of T800 welding on both sides must be terminated on the same side.

5. The novel welding method according to claim 1 is characterized in that: During the heat treatment in step 7), the heat treatment temperature is 720°C, the heating rate is 80°C / h, the temperature is kept for 4 hours, and the furnace is cooled.

6. The novel welding method according to claim 1 is characterized in that: In the step 9), both sides of the cladding surface of the weld 310 are cut.

Citation Information

Patent Citations

  • Built up welding technique of restoring roller for shape bar

    CN101003104A

  • F92 base metal weld deposit cobalt based hard alloy process

    CN101367148A

  • Overlaying welding method of large area carbide alloy of workpiece wear layer

    CN101433990A

  • Machining method for annular track of mechanical arm

    CN106363349A

  • Variable-polarity double-tungsten-electrode welding method for chemical tube sheets

    CN112846459A