Double-color injection molding in-mold decoration forming process

By changing the injection position and cooling structure of the mold, the two-color injection mold in-mold decoration molding process is realized, which solves the problems of low processing efficiency, high defective rate and environmental pollution in the existing technology, and realizes the two-color IMD process of efficient production and high-quality products.

CN118849327AActive Publication Date: 2024-10-29SHANGHAI TONGLING AUTOMOTIVE TECH INC

Patent Information

Application Number
CN202411194164.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-10-29
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The existing IML injection molding + masking spray process results in low processing efficiency, high defective rate, and serious environmental pollution. It cannot combine two-color injection molding with the IMD process, and cannot meet customer requirements for light transmission and texture decoration.

Method used

By changing the injection position of the mold and the cooling structure of the low-temperature plastic part, PC+ABS plastic with a low melting point is injected first, and then PC plastic with a higher melting point is injected. A two-color injection molding in-mold decoration molding process is adopted, including a black material layer. , mold rotation, two-shot injection of transparent layer, cooling and solidification, demoulding, eliminating the spraying process, improving production efficiency and product quality.

Benefits of technology

It achieves stable and continuous production on a single machine, meets customer requirements for light transmission and texture decoration, reduces defective rates and environmental pollution, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118849327A_ABST
    Figure CN118849327A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field, and discloses a double-color injection molding in-mold decoration forming process which comprises the following steps: S1, carrying out primary injection molding on a black material layer, putting black plastic into a hopper of an injection molding machine, and injecting the molten black plastic into a mold cavity of a mold to form the black material layer; the manufacturing method comprises the following steps of S1, mold rotation, S3, secondary injection of a transparent layer, placing a light-transmitting texture IMD membrane in a mold cavity of the mold, and injecting molten transparent plastic into the mold cavity of the mold to form the transparent layer, S4, cooling and curing, and S5, demolding. By changing the glue feeding position of the mold and a cooling structure of a low-temperature plastic part, the problem of poor light transmission caused by glue flushing is solved; the double-color IMD process is firstly put forward, stable and continuous production of a single machine is achieved, the requirements of clients for light transmission and texture decoration are met, and the problems that a conventional process is low in production efficiency, high in reject ratio and serious in environmental pollution are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of IMD in-mold decoration, in particular to a two-color injection in-mold decoration molding process. Background Art

[0002] Plastic products are widely used in the automotive, home appliance, communication, toy, and home furnishing industries. With the public's aesthetic and usage requirements, there is a need to continuously improve the texture decoration effect. The emergence of IMD (In-Mold Decoration) technology has solved this problem. The IMD process not only makes the surface of plastic products have rich texture and gloss, but also has the characteristics of scratch resistance, slowing aging, and extending service life.

[0003] As consumers' requirements for product aesthetics continue to increase, elements such as sound, light, and electricity are applied to products such as automobiles, home appliances, communications, toys, and home furnishings. Plastic products with both lighting effects and appearance texture effects have come into being.

[0004] The earliest processing technology for this type of product was "IML injection molding + masking spraying". The IML injection molding process is first used to obtain a translucent plastic product, and then the non-translucent area is sprayed with paint to prevent light from passing through. This processing method is still widely used. However, this process is characterized by IML single-piece injection molding, resulting in low processing efficiency. The semi-finished products after molding still need turnover and secondary masking spraying, baking and other processes. During the process, the stability of the spraying tooling is affected and the preset theoretical overlap cannot be completely consistent, which will bring the trouble of high defective rate (qualified rate ≤ 85%), and the environmental pollution in the painting process is serious.

[0005] In addition, the conventional two-color injection molding process is to first inject PC with a higher melting point, and then inject PC / ABS with a lower melting point. The existence of the IMD film transfer device makes it impossible to rotate the cavity during production, so it is impossible to combine two-color injection molding with the IMD process. Therefore, we need to propose a two-color injection mold decoration molding process. Summary of the invention

[0006] The purpose of the present invention is to provide a two-color injection molded in-mold decoration molding process. By changing the mold glue feeding position and the cooling structure of the low-temperature plastic part, the problem of poor light transmittance caused by glue punching is solved, and the PC+ABS plastic with a low melting point is injected first, and then the PC plastic with a higher melting point is injected. The two-color IMD process is first introduced to achieve stable and continuous production of a single machine, which not only meets the customer's requirements for light transmittance and texture decoration, but also solves the problems of low production efficiency, high defective rate and serious environmental pollution of conventional processes, so as to solve the problems raised in the above background technology.

[0007] To achieve the above object, the present invention provides the following technical solution: a two-color injection mold decoration molding process, comprising the following steps:

[0008] S1, one shot injection molding of black material layer: black plastic is placed into the hopper of the injection molding machine, and then the molten black plastic is injected into the cavity of the mold to form a black material layer;

[0009] S2, mold rotation: after the first injection is completed, the mold is opened and closed, the black material layer is left on the rear mold, and the mold is rotated 180° as a whole;

[0010] S3, second shot injection of transparent layer: put the transparent plastic into the hopper of the injection molding machine, and put the light-transmitting texture IMD film in the cavity of the mold, and then inject the molten transparent plastic into the cavity of the mold to form a transparent layer, so that the transparent layer is closely connected with the black material layer and covers the light-transmitting texture IMD film;

[0011] S4, cooling and solidification: The heat inside the mold is taken away by the circulating cooling medium, so that the transparent layer and the black material layer are completely solidified to form the desired product;

[0012] S5, demoulding: After the transparent layer and the black material layer are completely solidified, the clamping mechanism is released, and the product is pushed out of the mold through the ejection mechanism.

[0013] Preferably, before step S1, it is necessary to perform pre-injection molding preparation, which includes:

[0014] Injection molding machine preparation: prepare a two-color injection molding machine, that is, one with two injection devices and two mold cavities to inject different colors of plastic respectively;

[0015] Mold preparation: prepare the two-color injection mold and ensure that the mold has a suitable cavity and runner design to facilitate the subsequent injection of black plastic and transparent plastic;

[0016] Injection molding material preparation: Injection molding materials include transparent plastic, black plastic, and translucent textured IMD diaphragm. Among them, transparent plastic is made of PC plastic, and black plastic is made of PC+ABS plastic.

[0017] Preferably, in step S1 and step S3, before the first shot of injecting the black material layer and the second shot of injecting the transparent layer, the injection temperature, injection pressure, injection speed, holding time, holding pressure, and cooling time parameters of the injection molding machine are adjusted. During the process of injecting the black material layer, the operating status of the injection molding machine and the filling condition of the mold are closely monitored to ensure that no bubbles or material shortages occur.

[0018] Preferably, when the black material layer is injected in one shot, the parameters of the injection molding machine are set as follows:

[0019] Injection temperature: 230-250℃;

[0020] Injection pressure: 40-120MPa;

[0021] Injection speed: 3-5g / s;

[0022] Holding time: 18-25s;

[0023] Holding pressure: 40%-50% of injection pressure;

[0024] Cooling time: 5-15s.

[0025] Preferably, when the transparent layer is injected in two shots, the parameters of the injection molding machine are set as follows:

[0026] Injection temperature: 240-260℃;

[0027] Injection pressure: 50-130MPa;

[0028] Injection speed: 4-6g / s;

[0029] Holding time: 20-30s;

[0030] Holding pressure: 45%-55% of injection pressure;

[0031] Cooling time: 5-15s.

[0032] Preferably, in step S4, the two-color injection mold is equipped with a cooling system, and a coolant channel for cooling water or cooling oil to flow is provided in the cooling system. The molten black plastic and transparent plastic are in direct contact with the mold cavity, and the heat is transferred to the mold by heat conduction. The cooling water or cooling oil flowing in the coolant channel takes away the heat, so that the molten black plastic and transparent plastic are converted into a solid state, so that the product has a stable shape and performance.

[0033] Preferably, in step S5, when the product is taken out of the mold, in order to avoid damage or scratches to the product by the ejection mechanism, the ejection mechanism uses an ejector plate, and when pushing out the product, the ejection force should also be controlled to avoid damage to the mold or deformation of the product due to strong ejection, and to avoid failure to eject the product smoothly due to weak ejection.

[0034] Preferably, the two-color injection mold includes a fixed plate and a movable plate, the fixed plate is connected to a coring column, the movable plate is movably mounted on the coring column, two front molds are mounted on the fixed plate, a turntable is mounted on the movable plate, and two rear molds are mounted on the turntable.

[0035] Preferably, the two injection barrels of the two-color injection molding machine are aligned with the two front molds respectively, one of the front molds is equipped with a mold transfer device, and the light-transmitting texture IMD diaphragm is installed on the mold transfer device.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] The present invention solves the problem of poor light transmittance caused by glue punching by changing the glue feeding position of the mold and the cooling structure of the low-temperature plastic part, and realizes the injection molding of PC+ABS plastic with a low melting point first, and then the injection molding of PC plastic with a higher melting point. It is the first to launch a two-color IMD process and realize stable and continuous production of a single machine, which not only meets the customer's requirements for light transmittance and texture decoration, but also solves the problems of low production efficiency, high defective rate and serious environmental pollution of conventional processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a flowchart of the present invention;

[0039] Figure 2 It is a structural schematic diagram of the double-color injection mold of the present invention. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] See also Figure 1-2 The present invention provides a technical solution: a two-color injection mold decoration molding process, comprising the following steps:

[0042] S1, one shot injection molding of black material layer: black plastic is placed into the hopper of the injection molding machine, and then the molten black plastic is injected into the cavity of the mold to form a black material layer;

[0043] S2. Mold rotation: After the first injection is completed, the mold is opened and closed, and the black material layer is left on the rear mold, and the mold as a whole is rotated 180°; that is, the mold and the black material layer are rotated 180° together, so that the black material layer can be moved to the position of the second injection, so as to facilitate the addition of the transparent layer.

[0044] S3, second shot injection of transparent layer: put the transparent plastic into the hopper of the injection molding machine, and put the light-transmitting texture IMD film in the cavity of the mold, and then inject the molten transparent plastic into the cavity of the mold to form a transparent layer, so that the transparent layer is closely connected with the black material layer and covers the light-transmitting texture IMD film;

[0045] The transparent layer is connected between the light-transmitting texture IMD film and the black material layer.

[0046] In step S1 and step S3, before the first shot of the black material layer and the second shot of the transparent layer, the injection temperature, injection pressure, injection speed, holding time, holding pressure, and cooling time parameters of the injection molding machine are adjusted. During the process of injection molding the black material layer, the operating status of the injection molding machine and the filling status of the mold are closely monitored to ensure that no bubbles or material shortages occur.

[0047] By adjusting the injection molding machine parameters, it is ensured that the molten plastic can be evenly and completely filled into the mold cavity.

[0048] When injecting the black material layer in one shot, the parameters of the injection molding machine are set as follows:

[0049] Injection temperature: 230-250℃;

[0050] Injection pressure: 40-120MPa;

[0051] Injection speed: 3-5g / s;

[0052] Holding time: 18-25s;

[0053] Holding pressure: 40%-50% of injection pressure;

[0054] Cooling time: 5-15s.

[0055] The choice of injection speed depends on the size and shape of the product. A faster injection speed can shorten the production cycle, but may increase internal stress. And the temperature of the mold must be controlled to ensure uniform flow and solidification of the plastic.

[0056] The injection molded black material layer determines the basic shape and internal structure of the product.

[0057] When injecting the transparent layer in two shots, the parameters of the injection molding machine are set as follows:

[0058] Injection temperature: 240-260℃;

[0059] Injection pressure: 50-130MPa;

[0060] Injection speed: 4-6g / s;

[0061] Holding time: 20-30s;

[0062] Holding pressure: 45%-55% of injection pressure;

[0063] Cooling time: 5-15s.

[0064] The injection pressure and speed of the transparent layer should be slightly higher than those of the black layer to ensure the uniformity and glossiness of the transparent layer. When injecting the transparent layer in the second shot, the mold temperature may need to be slightly higher than the mold temperature when injecting the black layer in the first shot to improve transparency and reduce internal stress. However, excessively high mold temperature may cause material degradation or discoloration.

[0065] The purpose of injecting the transparent layer is:

[0066] Enhanced appearance: The transparent layer can provide a unique appearance effect to the product, such as high gloss, transparent or translucent visual effects;

[0067] Enhanced functionality: A clear layer may be used to protect an interior decorative layer, such as text, graphics or color, from wear and tear or contamination.

[0068] S4, cooling and solidification: The heat inside the mold is taken away by the circulating cooling medium, so that the transparent layer and the black material layer are completely solidified to form the desired product;

[0069] In step S4, the two-color injection mold is equipped with a cooling system, in which a coolant channel for cooling water or cooling oil to flow is provided. The molten black plastic and transparent plastic are in direct contact with the mold cavity and transfer the heat to the mold by heat conduction. The cooling water or cooling oil flowing in the coolant channel takes away the heat, so that the molten black plastic and transparent plastic are transformed into a solid state, so that the product has a stable shape and performance.

[0070] During the cooling process, the flow rate of the coolant must also be controlled, but the speed directly affects the quality and production efficiency of the product. Too fast cooling may increase the internal stress of the product, while too slow cooling may extend the production cycle. The cooling speed of each part of the mold should be as consistent as possible to avoid problems such as deformation or warping of the product.

[0071] Optionally, the cooling system also includes a temperature monitoring device for real-time monitoring of temperature changes of the mold and plastic so as to adjust production parameters in a timely manner.

[0072] S5, demoulding: After the transparent layer and the black material layer are completely solidified, the clamping mechanism is released, and the product is pushed out of the mold through the ejection mechanism.

[0073] This process eliminates the spraying process, improves production efficiency, and reduces the scrap rate of semi-finished products.

[0074] The movable mold part and the fixed mold part of the mold are tightly fitted together through the clamping mechanism to ensure that the molten plastic is filled into the mold cavity under high pressure.

[0075] In step S5, when the product is taken out of the mold, in order to avoid damage or scratches to the product by the ejection mechanism, the ejection mechanism uses an ejector plate. When ejecting the product, the ejection force should also be controlled to avoid damage to the mold or deformation of the product due to strong ejection, and to avoid failure to eject the product smoothly due to weak ejection.

[0076] The two parts of the mold should be kept synchronized during the opening and closing process to avoid damage to the mold or the product;

[0077] The mold closing process should be carried out smoothly to avoid excessive impact or vibration, which helps protect the mold and product.

[0078] After demoulding, the finished product undergoes necessary post-processing, such as deburring, grinding, painting, etc., to improve the appearance and texture of the product, and undergoes quality inspection to ensure that the product meets the design requirements and quality standards.

[0079] Translucent texture IMD film is a film material with specific texture and light transmittance, which is used to combine with plastic during the injection molding process to form a product surface with decorative effect. Translucent texture IMD film contains design elements such as text and patterns, which are combined with plastic materials through the injection molding process to form an integrated decorative effect.

[0080] Before step S1, preparations before injection molding are required, including:

[0081] Injection molding machine preparation: prepare a two-color injection molding machine, that is, one with two injection devices and two mold cavities to inject different colors of plastic respectively;

[0082] Mold preparation: prepare the two-color injection mold and ensure that the mold has a suitable cavity and runner design to facilitate the subsequent injection of black plastic and transparent plastic;

[0083] Injection molding material preparation: Injection molding materials include transparent plastic, black plastic, and translucent textured IMD diaphragm. Among them, transparent plastic is made of PC plastic, and black plastic is made of PC+ABS plastic.

[0084] PC plastic and PC+ABS plastic need to be heated into a molten state before injection molding and then injected into the mold through an injection molding machine.

[0085] PC plastic has excellent transparency, heat resistance and mechanical properties, and is suitable for products that require high transparency and durability. PC+ABS plastic combines the transparency of PC with the toughness and impact resistance of ABS to form a material that is both transparent and has excellent mechanical properties. Combined with transparent PC plastic and light-transmitting texture IMD film, it forms a complex product with two-color effects and decorative textures.

[0086] like Figure 2As shown, the two-color injection mold includes a fixed plate and a movable plate, the fixed plate is connected to a coring column, the movable plate is movably mounted on the coring column, and two front molds are installed on the fixed plate, a turntable is installed on the movable plate, and two rear molds are installed on the turntable.

[0087] Two injection barrels of the two-color injection molding machine are respectively aligned with two front molds, one of the front molds is equipped with a mold transfer device, and the light-transmitting texture IMD diaphragm is installed on the mold transfer device.

[0088] The two-color injection mold is also equipped with an infrared detector to monitor and control the temperature of the mold to ensure the stability of the injection process and the quality of the product; the infrared temperature measurement technology can irradiate the surface of the injection mold without contact, receive the infrared radiation energy emitted by the mold surface through the detector, and calculate and determine its surface temperature. This helps to understand and control the temperature status of the mold in real time and ensure the smooth progress of the injection process.

[0089] The mold transfer device can ensure the precise positioning of the IMD diaphragm during the injection molding process to prevent displacement or misalignment, thereby ensuring the appearance and quality of the product.

[0090] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A two-color injection mold decoration molding process, characterized in that: The following steps are involved: S1, one shot injection molding of black material layer: black plastic is placed into the hopper of the injection molding machine, and then the molten black plastic is injected into the cavity of the mold to form a black material layer; S2, mold rotation: after the first injection is completed, the mold is opened and closed, the black material layer is left on the rear mold, and the mold is rotated 180° as a whole; S3, second shot injection of transparent layer: put the transparent plastic into the hopper of the injection molding machine, and put the light-transmitting texture IMD film in the cavity of the mold, and then inject the molten transparent plastic into the cavity of the mold to form a transparent layer, so that the transparent layer is closely connected with the black material layer and covers the light-transmitting texture IMD film; S4, cooling and solidification: The heat inside the mold is taken away by the circulating cooling medium, so that the transparent layer and the black material layer are completely solidified to form the desired product; S5. Demolding: After the transparent layer and the black material layer are completely solidified, the mold locking mechanism is released and the product is pushed out of the mold through the ejection mechanism.

2. A two-color injection molding in-mold decoration molding process according to claim 1, characterized in that: Before step S1, preparations before injection molding are required, including: Injection molding machine preparation: prepare a two-color injection molding machine, that is, a machine with two injection devices and two mold cavities to inject different colors of plastic respectively; Mold preparation: prepare the two-color injection mold and ensure that the mold has a suitable cavity and runner design to facilitate the subsequent injection of black plastic and transparent plastic; Injection molding material preparation: Injection molding materials include transparent plastic, black plastic, and light-transmitting textured IMD diaphragm. Among them, transparent plastic is made of PC plastic, and black plastic is made of PC+ABS plastic.

3. A two-color injection molding in-mold decoration molding process according to claim 1, characterized in that: In step S1 and step S3, before the first shot of the black material layer and the second shot of the transparent layer, the injection temperature, injection pressure, injection speed, holding time, holding pressure, and cooling time parameters of the injection molding machine are adjusted. During the process of injection molding the black material layer, the operating status of the injection molding machine and the filling status of the mold are closely monitored to ensure that no bubbles or material shortages occur.

4. A two-color injection molding in-mold decoration molding process according to claim 3, characterized in that: When the black material layer is injected in one shot, the parameters of the injection molding machine are set as follows: Injection temperature: 230-250℃; Injection pressure: 40-120MPa; Injection speed: 3-5g / s; Holding time: 18-25s; Holding pressure: 40%-50% of injection pressure; Cooling time: 5-15s.

5. A two-color injection molding process for in-mold decoration according to claim 3, characterized in that: When injecting the transparent layer in two shots, the parameters of the injection molding machine are set as follows: Injection temperature: 240-260℃; Injection pressure: 50-130MPa; Injection speed: 4-6g / s; Holding time: 20-30s; Holding pressure: 45%-55% of injection pressure; Cooling time: 5-15s.

6. A two-color injection molding in-mold decoration molding process according to claim 1, characterized in that: In step S4, the two-color injection mold is equipped with a cooling system, in which a coolant channel for cooling water or cooling oil to flow is provided. The molten black plastic and transparent plastic are in direct contact with the mold cavity and transfer the heat to the mold by heat conduction. The cooling water or cooling oil flowing in the coolant channel takes away the heat, so that the molten black plastic and transparent plastic are transformed into a solid state, so that the product has a stable shape and performance.

7. A two-color injection molding in-mold decoration molding process according to claim 1, characterized in that: In step S5, when the product is taken out of the mold, in order to avoid damage or scratches to the product by the ejection mechanism, the ejection mechanism uses an ejector plate. When ejecting the product, the ejection force should also be controlled to avoid damage to the mold or deformation of the product due to strong ejection, and to avoid failure to eject the product smoothly due to weak ejection.

8. A two-color injection molding in-mold decoration molding process according to claim 1, characterized in that: The two-color injection mold includes a fixed plate and a movable plate, the fixed plate is connected with a coring column, the movable plate is movably mounted on the coring column, two front molds are mounted on the fixed plate, a turntable is mounted on the movable plate, and two rear molds are mounted on the turntable.

9. A two-color injection molding in-mold decoration molding process according to claim 8, characterized in that: Two injection barrels of the two-color injection molding machine are respectively aligned with two front molds, one of the front molds is equipped with a mold transfer device, and the light-transmitting texture IMD diaphragm is installed on the mold transfer device.

Citation Information

Patent Citations

  • Plug-in assembly double-color injection molding process

    CN110936551A

  • Double-shot film pasting injection molding process

    CN111216309A

  • Double-color injection molding film upholstery light transmission process

    CN111745885A

  • In-mold decoration (IMD) inner opening decoration plate processing technology based on secondary parting and double-ring type fine positioning

    CN116653217A

  • Method for forming laser carving pattern on plastic product by laser carving and in-mold transfer technique, and product of the same

    JP2010155378A

Cited By

  • Mold for double-color injection molding of optical lens and injection molding method thereof

    CN120735242A

  • Method for controlling rotating cavity in double-color injection molding process

    CN121340572A