Low-temperature-resistant co-extrusion heavy packaging film and preparation method thereof
By using a specific composition ratio and an acid anhydride-modified polyolefin adhesive layer in the co-extruded heavy packaging film, the problem of insufficient film toughness in low-temperature environments in the existing technology is solved, and the toughening and barrier properties at low temperatures are improved. , suitable for high-speed FFS packaging.
Patent Information
- Application Number
- CN202410843293.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-29
AI Technical Summary
The existing three-layer co-extruded heavy-duty packaging film has insufficient toughness in low-temperature environments and is prone to brittleness, making it difficult to meet the packaging needs of low-temperature refrigeration.
It adopts a specific composition ratio of inner layer, middle layer and outer layer, including linear low density polyethylene, metallocene linear low density polyethylene, ethylene-vinyl acetate copolymer, high pressure low density polyethylene, color masterbatch and auxiliary agents. Polyolefin modified by acid anhydride is used as the adhesive layer to improve the adhesion and toughening effect, and ethylene-vinyl alcohol copolymer, ethylene-octene copolymer, etc. are added to the middle layer to improve the barrier properties.
It maintains the softness and toughness of the film in low-temperature environments, avoids brittleness, and improves mechanical properties and barrier properties. It is suitable for high-speed FFS packaging.
Smart Images

Figure CN118849580A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of co-extruded heavy-duty packaging films, in particular to a low-temperature-resistant co-extruded heavy-duty packaging film and a preparation method thereof. Background Art
[0002] Referring to a Chinese patent for a three-layer co-extruded heavy packaging film and its preparation method (Announcement No.: CN103029388B), the inner layer of the three-layer co-extruded heavy packaging film contains LLDPE and m-LLDPE; the middle layer is composed of m-LLDPE, LLDPE, MDPE, EVA and masterbatch; the outer layer contains LLDPE, LDPE and m-LLDPE. The three-layer co-extruded heavy packaging film preparation method of the present invention adopts the product prepared under certain process conditions using the above ratio. Compared with the prior art, it has the characteristics of superior mechanical properties, good stiffness, moderate film surface friction coefficient, and heat sealing window that can reach 180±50℃, which can fully meet the normal use of downstream packaging, and is particularly suitable for high-speed FFS packaging, with good economic and social benefits. In the above-mentioned prior art, the prepared packaging film still has a certain toughness, so its application in the low-temperature field is limited, especially in low-temperature refrigeration; for this reason, the present invention proposes a low-temperature resistant co-extruded heavy packaging film and its preparation method to solve the above-mentioned problems. Summary of the invention
[0003] 1. Technical issues to be resolved
[0004] In view of the deficiencies in the prior art, the present invention provides a low-temperature resistant co-extruded heavy-duty packaging film and a preparation method thereof, which solves the problems mentioned in the above background technology.
[0005] (II) Technical solution
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions: A low-temperature resistant co-extruded heavy packaging film, comprising an inner layer, a middle layer and an outer layer, wherein the inner layer and the middle layer, as well as the middle layer and the outer layer, are bonded by an adhesive layer;
[0007] Wherein, the inner layer is composed of the following components in parts by weight: 15 to 75 parts of linear low-density polyethylene, 15 to 75 parts of metallocene linear low-density polyethylene, and 5 to 10 parts of ethylene-vinyl acetate copolymer;
[0008] The intermediate layer is composed of the following components in parts by weight: 20-40 parts of high-pressure low-density polyethylene, 20-40 parts of linear low-density polyethylene, 3-10 parts of masterbatch, and 5-15 parts of auxiliary agent;
[0009] The outer layer is composed of the following components in parts by weight: 10 to 50 parts of linear low-density polyethylene, 15 to 50 parts of metallocene linear low-density polyethylene, and 10 to 30 parts of low-density polyethylene.
[0010] Preferably, the adhesive layer is anhydride-modified polyolefin.
[0011] Preferably, the auxiliary agent is selected from any one or more of ethylene-vinyl alcohol copolymer, ethylene-octene copolymer, polyvinylidene chloride, and poly(meta-xylylene adipamide).
[0012] Preferably, the inner layer is composed of the following components in parts by weight: 45 parts of linear low-density polyethylene, 45 parts of metallocene linear low-density polyethylene, and 10 parts of ethylene-vinyl acetate copolymer;
[0013] The intermediate layer is composed of the following components in parts by weight: 40 parts of high-pressure low-density polyethylene, 40 parts of linear low-density polyethylene, 10 parts of masterbatch, and 10 parts of auxiliary agent;
[0014] The outer layer is composed of the following components in parts by weight: 50 parts of linear low-density polyethylene, 40 parts of metallocene linear low-density polyethylene, and 10 parts of low-density polyethylene.
[0015] A method for preparing a low-temperature resistant co-extruded heavy-duty packaging film, specifically comprising the following preparation steps:
[0016] S1. Weigh and measure each raw material;
[0017] S2, pouring the weighed raw materials into three groups of extruders corresponding to the inner layer, the middle layer and the outer layer respectively, fusing and extruding to form film bubbles;
[0018] S3, cooling the film bubble to form a flat film sheet;
[0019] S4, the film is rolled up, and after reaching a certain roll weight, the semi-finished film roll is unrolled;
[0020] S5. Cut the semi-finished film roll obtained, and let it stand for 48 to 72 hours to obtain a low-temperature resistant co-extruded heavy packaging film.
[0021] Preferably, in step S2, the melt pressure at the outlet of the outer layer extruder is 385-395 MPa, the melt pressure at the outlet of the middle layer extruder is 500-540 MPa, and the melt pressure at the outlet of the inner layer extruder is 370-390 MPa.
[0022] Preferably, in step S2, the extrusion speed of the inner layer and the outer layer is 36.2-37.5 r / min; the extrusion speed of the middle layer is 18.2-20.2 r / min.
[0023] Preferably, the co-extruded heavy packaging film has a thickness of 120 to 200 μm.
[0024] (III) Beneficial effects
[0025] The present invention provides a low-temperature resistant co-extruded heavy packaging film and a preparation method thereof. Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The low-temperature resistant co-extruded heavy-duty packaging film and its preparation method use anhydride-modified polyolefin as an adhesive layer to improve the adhesion between the materials, making the multi-layer co-extruded film more uniform and firmly composited together. At the same time, the toughness of the film can be modified to improve its toughening effect, so that the film can remain soft in a low-temperature environment and will not crack.
[0027] (2) The low-temperature resistant co-extruded heavy-duty packaging film and its preparation method, by adding ethylene-vinyl acetate copolymer to the inner layer, the co-extruded film is volume-enhanced and modified, thereby improving the mechanical properties of the co-extruded film and enhancing its volume-enhancing effect; by adding any one or more of ethylene-vinyl alcohol copolymer, ethylene-octene copolymer, polyvinylidene chloride, and poly(meta-xylylene adipamide) to the middle layer, sufficient barrier properties are provided for the packaging film. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The invention provides a packaging film peeling force value test for a low-temperature resistant co-extruded heavy packaging film and a preparation method thereof. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] The embodiment of the present invention provides the following technical solutions:
[0031] Example 1
[0032] A method for preparing a low-temperature resistant co-extruded heavy-duty packaging film, specifically comprising the following preparation steps:
[0033] S1. Weigh and measure the raw materials; wherein the inner layer is composed of the following components in parts by weight: 75 parts of linear low-density polyethylene, 20 parts of metallocene linear low-density polyethylene, and 5 parts of ethylene-vinyl acetate copolymer;
[0034] The intermediate layer is composed of the following components in parts by weight: 40 parts of high-pressure low-density polyethylene, 40 parts of linear low-density polyethylene, 5 parts of masterbatch, and 15 parts of ethylene-vinyl alcohol copolymer;
[0035] The outer layer is composed of the following components in parts by weight: 40 parts of linear low-density polyethylene, 50 parts of metallocene linear low-density polyethylene, and 10 parts of low-density polyethylene;
[0036] 3 parts of anhydride-modified polyolefin;
[0037] S2, pour the weighed raw materials into the three groups of extruders corresponding to the inner layer, the middle layer and the outer layer respectively, fuse and extrude to form film bubbles; wherein the melt pressure at the outlet of the outer layer extruder is 385MPa, the melt pressure at the outlet of the middle layer extruder is 500MPa, and the melt pressure at the outlet of the inner layer extruder is 370MPa; the extrusion speed of the inner layer and the outer layer is 36.25r / min; the extrusion speed of the middle layer is 18.2r / min;
[0038] S3, cooling the film bubble to form a flat film sheet;
[0039] S4, the film is rolled up, and after reaching a certain roll weight, the semi-finished film roll is unrolled;
[0040] S5. Cut the obtained semi-finished film roll and let it stand for 48 hours to obtain a low-temperature resistant co-extruded heavy-duty packaging film with a thickness of 120 μm.
[0041] Example 2
[0042] A method for preparing a low-temperature resistant co-extruded heavy-duty packaging film, specifically comprising the following preparation steps:
[0043] S1. Weigh and measure the raw materials; wherein the inner layer is composed of the following components in parts by weight: 42 parts of linear low-density polyethylene, 50 parts of metallocene linear low-density polyethylene, and 8 parts of ethylene-vinyl acetate copolymer;
[0044] The intermediate layer is composed of the following components in parts by weight: 30 parts of high-pressure low-density polyethylene, 40 parts of linear low-density polyethylene, 10 parts of masterbatch, and 10 parts of ethylene-octene copolymer;
[0045] The outer layer is composed of the following components in parts by weight: 35 parts of linear low-density polyethylene, 50 parts of metallocene linear low-density polyethylene, and 15 parts of low-density polyethylene;
[0046] 8 parts of anhydride-modified polyolefin;
[0047] S2, pour the weighed raw materials into the three groups of extruders corresponding to the inner layer, the middle layer and the outer layer, respectively, fuse and extrude to form film bubbles; wherein the melt pressure at the outlet of the outer layer extruder is 390MPa, the melt pressure at the outlet of the middle layer extruder is 520MPa, and the melt pressure at the outlet of the inner layer extruder is 380MPa; the extrusion speed of the inner layer and the outer layer is 37.1r / min; the extrusion speed of the middle layer is 19.2r / min;
[0048] S3, cooling the film bubble to form a flat film sheet;
[0049] S4, the film is rolled up, and after reaching a certain roll weight, the semi-finished film roll is unrolled;
[0050] S5. Cut the obtained semi-finished film roll and let it stand for 52 hours to obtain a low-temperature resistant co-extruded heavy-duty packaging film with a thickness of 160 μm.
[0051] Example 3
[0052] A method for preparing a low-temperature resistant co-extruded heavy-duty packaging film, specifically comprising the following preparation steps:
[0053] S1. Weigh and measure each raw material; wherein the inner layer is composed of the following components in parts by weight: 45 parts of linear low-density polyethylene, 45 parts of metallocene linear low-density polyethylene, and 10 parts of ethylene-vinyl acetate copolymer;
[0054] The middle layer is composed of the following components in parts by weight: 40 parts of high-pressure low-density polyethylene, 40 parts of linear low-density polyethylene, 10 parts of masterbatch, and 10 parts of poly(m-xylylene adipamide);
[0055] The outer layer is composed of the following components in parts by weight: 50 parts of linear low-density polyethylene, 40 parts of metallocene linear low-density polyethylene, and 10 parts of low-density polyethylene;
[0056] 3 parts of anhydride-modified polyolefin;
[0057] S2, pour the weighed raw materials into the three groups of extruders corresponding to the inner layer, the middle layer and the outer layer, respectively, fuse and extrude to form film bubbles; wherein the melt pressure at the outlet of the outer layer extruder is 395MPa, the melt pressure at the outlet of the middle layer extruder is 540MPa, and the melt pressure at the outlet of the inner layer extruder is 390MPa; the extrusion speed of the inner layer and the outer layer is 37.5r / min; the extrusion speed of the middle layer is 20.2r / min;
[0058] S3, cooling the film bubble to form a flat film sheet;
[0059] S4, the film is rolled up, and after reaching a certain roll weight, the semi-finished film roll is unrolled;
[0060] S5. Cut the obtained semi-finished film roll and let it stand for 48 to 72 hours to obtain a low-temperature resistant co-extruded heavy-duty packaging film with a thickness of 200 μm.
[0061] Comparative Example 1
[0062] A method for preparing a low-temperature resistant co-extruded heavy-duty packaging film, specifically comprising the following preparation steps:
[0063] S1. Weigh and measure the raw materials; wherein the inner layer is composed of the following components in parts by weight: 75 parts of linear low-density polyethylene, 20 parts of metallocene linear low-density polyethylene, and 5 parts of ethylene-vinyl acetate copolymer;
[0064] The intermediate layer is composed of the following components in parts by weight: 40 parts of high-pressure low-density polyethylene, 40 parts of linear low-density polyethylene, 5 parts of masterbatch, and 15 parts of ethylene-vinyl alcohol copolymer;
[0065] The outer layer is composed of the following components in parts by weight: 40 parts of linear low-density polyethylene, 50 parts of metallocene linear low-density polyethylene, and 10 parts of low-density polyethylene;
[0066] S2, pour the weighed raw materials into the three groups of extruders corresponding to the inner layer, the middle layer and the outer layer respectively, fuse and extrude to form film bubbles; wherein the melt pressure at the outlet of the outer layer extruder is 385MPa, the melt pressure at the outlet of the middle layer extruder is 500MPa, and the melt pressure at the outlet of the inner layer extruder is 370MPa; the extrusion speed of the inner layer and the outer layer is 36.25r / min; the extrusion speed of the middle layer is 18.2r / min;
[0067] S3, cooling the film bubble to form a flat film sheet;
[0068] S4, the film is rolled up, and after reaching a certain roll weight, the semi-finished film roll is unrolled;
[0069] S5. Cut the obtained semi-finished film roll and let it stand for 48 hours to obtain a low-temperature resistant co-extruded heavy-duty packaging film with a thickness of 120 μm.
[0070] Comparative Example 2
[0071] A method for preparing a low-temperature resistant co-extruded heavy-duty packaging film, specifically comprising the following preparation steps:
[0072] S1. Weigh and measure the raw materials; wherein the inner layer is composed of the following components in parts by weight: 75 parts of linear low-density polyethylene and 20 parts of metallocene linear low-density polyethylene;
[0073] The middle layer is composed of the following components in parts by weight: 40 parts of high-pressure low-density polyethylene, 40 parts of linear low-density polyethylene, and 5 parts of masterbatch;
[0074] The outer layer is composed of the following components in parts by weight: 40 parts of linear low-density polyethylene, 50 parts of metallocene linear low-density polyethylene, and 10 parts of low-density polyethylene;
[0075] 3 parts of anhydride-modified polyolefin;
[0076] S2, pour the weighed raw materials into the three groups of extruders corresponding to the inner layer, the middle layer and the outer layer respectively, fuse and extrude to form film bubbles; wherein the melt pressure at the outlet of the outer layer extruder is 385MPa, the melt pressure at the outlet of the middle layer extruder is 500MPa, and the melt pressure at the outlet of the inner layer extruder is 370MPa; the extrusion speed of the inner layer and the outer layer is 36.25r / min; the extrusion speed of the middle layer is 18.2r / min;
[0077] S3, cooling the film bubble to form a flat film sheet;
[0078] S4, the film is rolled up, and after reaching a certain roll weight, the semi-finished film roll is unrolled;
[0079] S5. Cut the obtained semi-finished film roll and let it stand for 48 hours to obtain a low-temperature resistant co-extruded heavy-duty packaging film with a thickness of 120 μm.
[0080] Performance Test:
[0081] Tensile performance test: The test was carried out using a tensile testing machine in accordance with GB / T 1040-2006 at room temperature with a tensile speed of 50 mm / min, a clamp interval length of 50 mm, and a test temperature of 23°C; the sample size was 175 mm x 15 mm.
[0082] Peel force value test: Use a tensile testing machine to test according to CB / T 1040.3-2006. Test the packaging film at room temperature. The tensile speed is 50mm / min, the clamp interval length is 50mm, and the test temperature is 23℃. The sample size is 175mm x 15mm.
[0083] Low temperature resistance test: The samples were placed in a freezing chamber at -10°C and taken out after 24 hours of constant temperature. The dart impact quality and tensile strength of the samples were tested according to GB / T1040.3-2006 and GB / T9639.1-2008. The sample size was 160 mm × 20 mm. The results are shown in Table 1.
[0084] Barrier performance test: Test the light transmittance / haze of the sample according to GB / T 2410-2008; the results are shown in Table 1:
[0085] Table 1
[0086] Dart impact mass / g Tensile strength (longitudinal / transverse) / MPa transparency / % Haze / % Example 1 184 52 / 40 91% 2.6 Example 2 185 53 / 41 92% 2.7 Example 3 183 51 / 40 91% 2.6 Comparative Example 1 132 29 / 20 84% 3.1 Comparative Example 2 153 34 / 23 81% 4.3
[0087] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.
[0088] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0089] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A low temperature resistant co-extruded heavy packaging film, comprising an inner layer, an intermediate layer and an outer layer, characterized in that: The inner layer and the middle layer, as well as the middle layer and the outer layer, are bonded together by an adhesive layer; Wherein, the inner layer is composed of the following components in parts by weight: 15 to 75 parts of linear low-density polyethylene, 15 to 75 parts of metallocene linear low-density polyethylene, and 5 to 10 parts of ethylene-vinyl acetate copolymer; The intermediate layer is composed of the following components in parts by weight: 20-40 parts of high-pressure low-density polyethylene, 20-40 parts of linear low-density polyethylene, 3-10 parts of masterbatch, and 5-15 parts of auxiliary agent; The outer layer is composed of the following components in parts by weight: 10 to 50 parts of linear low-density polyethylene, 15 to 50 parts of metallocene linear low-density polyethylene, and 10 to 30 parts of low-density polyethylene.
2. The low temperature resistant co-extruded heavy packaging film according to claim 1, characterized in that: The adhesive layer is anhydride-modified polyolefin, and its weight proportion is 3 to 8 parts.
3. The low temperature resistant co-extruded heavy packaging film according to claim 1, characterized in that: The auxiliary agent is selected from any one or more of ethylene-vinyl alcohol copolymer, ethylene-octene copolymer, polyvinylidene chloride, and poly(m-xylylene adipamide).
4. The low temperature resistant co-extruded heavy packaging film according to claim 1, characterized in that: The inner layer is composed of the following components in parts by weight: 45 parts of linear low-density polyethylene, 45 parts of metallocene linear low-density polyethylene, and 10 parts of ethylene-vinyl acetate copolymer; The intermediate layer is composed of the following components in parts by weight: 40 parts of high-pressure low-density polyethylene, 40 parts of linear low-density polyethylene, 10 parts of masterbatch, and 10 parts of auxiliary agent; The outer layer is composed of the following components in parts by weight: 50 parts of linear low-density polyethylene, 40 parts of metallocene linear low-density polyethylene, and 10 parts of low-density polyethylene.
5. A method for preparing a low-temperature resistant co-extruded heavy packaging film according to claim 1, characterized in that: The specific preparation steps include: S1. Weigh and measure each raw material; S2, pouring the weighed raw materials into three groups of extruders corresponding to the inner layer, the middle layer and the outer layer respectively, fusing and extruding to form film bubbles; S3, cooling the film bubble to form a flat film sheet; S4, the film is rolled up, and after reaching a certain roll weight, the semi-finished film roll is unrolled; S5. Cut the semi-finished film roll obtained, and let it stand for 48 to 72 hours to obtain a low-temperature resistant co-extruded heavy packaging film.
6. The method for preparing a low temperature resistant co-extruded heavy packaging film according to claim 5, characterized in that: In the step S2, the melt pressure at the outlet of the outer layer extruder is 385-395 MPa, the melt pressure at the outlet of the middle layer extruder is 500-540 MPa, and the melt pressure at the outlet of the inner layer extruder is 370-390 MPa.
7. The method for preparing a low temperature resistant co-extruded heavy packaging film according to claim 5, characterized in that: In the step S2, the extrusion speed of the inner layer and the outer layer is 36.2-37.5 r / min; the extrusion speed of the middle layer is 18.2-20.2 r / min.
8. The method for preparing a low temperature resistant co-extruded heavy packaging film according to claim 5, characterized in that: The co-extruded heavy packaging film has a thickness of 120 to 200 μm.
Citation Information
Patent Citations
FFS (Form-Fill-Seal) two-layer coextruded repackaging film and preparation method thereof
CN103009738A
Three-layer coextrusion heavy packaging membrane and fabrication method thereof
CN103029388A
Flame-retardant anti-poison high-temperature-resistant polypropylene co-extrusion film and preparation method thereof
CN111409317A
Low-temperature-resistant three-layer co-extrusion heavy packaging film
CN115635750A
High-barrier heavy-packaging one-way breathable bag and preparation method thereof
CN115648765A
Cited By
EVOH high-barrier film for ensiling bag and preparation method of EVOH high-barrier film