Lithium manganese iron phosphate as well as preparation method and application thereof
By coating the core of ammonium iron manganese phosphate with multi-layer materials and controlling the particle distribution through hydrothermal reaction, the problem of insufficient lithium iron manganese phosphate battery performance is solved, the conductivity and structural stability are improved, the voltage platform is broadened and the voltage is improved. Lithium-ion battery performance.
Patent Information
- Application Number
- CN202410945204.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-29
AI Technical Summary
The insufficient electrical properties of lithium iron manganese phosphate (LMFP) cathode material make it difficult to fully realize its potential in lithium-ion batteries, limiting its commercial application.
By coating several layers of ammonium ferromanganese phosphate material on the outer core of ammonium ferromanganese phosphate, a structure is formed in which the moles of ferromanganese gradually increase from the core to the outside in the radial direction, and the particle size and particle size distribution are controlled by hydrothermal reaction and the introduction of crystal seeds. , improve the uniform distribution of Mn2+ and Fe2+ at the atomic level and improve the electrical properties.
It improves the conductivity, structural stability and electrochemical performance of lithium iron manganese phosphate, enhances the transmission channel of Li+, broadens the voltage platform, reduces the management difficulty of the battery management system, and improves the specific capacity and stability.
Smart Images

Figure CN118851131A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery material synthesis, and in particular to lithium manganese iron phosphate and a preparation method and application thereof. Background Art
[0002] With the transformation of energy policies, lithium-ion batteries have been fully and widely used in power storage, power batteries and 3C electronic products. Currently, the lithium-ion battery with the highest commercialization and market share is lithium iron phosphate lithium-ion battery.
[0003] The important factor affecting the lithium-ion battery is the lithium iron phosphate positive electrode material (LiFePO4, abbreviated as LFP positive electrode material), but the LFP positive electrode material - Fe 2+ The energy density of the material, with a radius of 0.074nm, a theoretical specific capacity of 170mAh / g and a voltage platform of 3.4V, is close to its theoretical upper limit, limiting its further industrial application.
[0004] The atomic numbers of Mn and Fe, which are adjacent to each other in the periodic table, are 25 and 26 respectively, and their electron configurations are 1s 2 2s 2 2p 6 3s 2 3p 6 4s 2 3d 5 , 1s 2 2s 2 2p 6 3s 2 3p 6 4s 2 3d 6 According to Hund's law and Pauli's principle, the system is most stable when the valence electron energy level is filled with electron vacancies, half filled, or fully filled. The corresponding valence electron energy level filling state is 4s 0 ,3d 5 , then Mn easily forms Mn 2+ (Electron configuration 1s 2 2s 2 2p 6 3s 2 3p 6 4s 0 3d 5 ), unstable Fe 2+ Easily oxidized to Fe 3+ (Electron configuration 1s 2 2s 2 2p 6 3s 2 3p 6 4s 0 3d 5), that is, the redox potential of Mn ions is higher than that of Fe ions, so the voltage platform of LiMnPO4 is as high as 4.1V. Compared with LFP positive electrode materials, the ionic radius of LiMnPO4 (Mn 2+ The radius is 0.080nm) and the theoretical specific capacity is similar (171mAh / g). Both of them belong to the olivine structure. The lithium manganese iron phosphate positive electrode material (LiMn x Fe 1-x PO4, abbreviated as LMFP positive electrode material) can break through the energy density limit of LFP positive electrode material, then LMFP positive electrode material will definitely become the ideal material for the new generation of lithium-ion batteries.
[0005] However, due to its low electrical conductivity and ion conduction coefficient, pure LMFP positive electrode material is almost an insulator, and it is difficult to fully exert its electrical performance, thus limiting its commercial application.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The object of the present invention is to provide a lithium manganese iron phosphate and a preparation method and application thereof, aiming to solve the electrical performance problem of lithium manganese iron phosphate (LMFP) positive electrode material.
[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0009] One aspect of the present invention relates to a method for preparing lithium manganese iron phosphate, comprising the following steps:
[0010] (a) coating a plurality of layers of ammonium manganese ferric phosphate material layers outside the ammonium manganese ferric phosphate core to obtain a precursor;
[0011] (b) mixing the precursor, the lithium source and the carbon source, grinding, first drying and sintering;
[0012] The manganese-iron molar ratio of the ammonium manganese ferric phosphate core and each layer of the ammonium manganese ferric phosphate material layer increases radially from the inside to the outside.
[0013] The method for preparing lithium manganese iron phosphate is simple and easy to implement. The prepared lithium manganese iron phosphate has good stability and excellent electrical properties, especially good electrical conductivity.
[0014] Another aspect of the present invention also relates to lithium manganese iron phosphate prepared by the lithium manganese iron phosphate preparation method.
[0015] The lithium manganese iron phosphate has a structure in which the manganese and iron moles increase radially from the inner core to the outer core, and has excellent electrochemical performance and a stable structure.
[0016] Another aspect of the present invention also relates to a positive electrode material, wherein the positive electrode material includes the lithium manganese iron phosphate prepared by the preparation method of the lithium manganese iron phosphate or the lithium manganese iron phosphate.
[0017] Another aspect of the present invention also relates to a secondary battery, comprising the positive electrode material.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The preparation method of lithium manganese iron phosphate provided by the present invention comprises coating a plurality of layers of ammonium manganese iron phosphate material layers outside the ammonium manganese iron phosphate core, wherein the manganese iron molar ratio of the ammonium manganese iron phosphate core and each layer of the ammonium manganese iron phosphate material increases radially from the inside to the outside, thereby forming lithium manganese iron phosphate in which the manganese iron molar ratio increases radially from the core to the outside. The lithium manganese iron phosphate prepared by the method has good stability and excellent electrical properties, especially good electrical conductivity.
[0020] (2) The preparation method of lithium manganese iron phosphate provided by the present invention, the precursor contains NH4 + When synthesizing LMFP cathode materials, NH4 + It will decompose and release in the form of gas, forming a porous structure, which is beneficial to the sintering process. + Automatically and easily "falls" into the isophosphite structure to form an olivine-structured LMFP cathode material, and improves the wettability of the electrolyte to the particles, improving the Li + The accessibility to the interior of the particles and the surface activity of the particles can improve the specific capacity of the LMFP cathode material.
[0021] (3) The preparation method of lithium manganese iron phosphate provided by the present invention can realize the solvation of insoluble ions by hydrothermal reaction, and regulate the particle size and particle size distribution by introducing crystal seeds to realize Mn 2+ , Fe 2+ Uniform distribution at the atomic level improves the electrical properties of LMFP positive electrode materials and enhances product stability.
[0022] (4) The lithium manganese iron phosphate provided by the present invention has a structure in which the manganese and iron moles increase radially from the inner core to the outer core, and has excellent electrochemical properties and a stable structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 This is the 0.1C charge and discharge curve provided by the present invention. DETAILED DESCRIPTION
[0025] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0026] One aspect of the present invention relates to a method for preparing lithium manganese iron phosphate, comprising the following steps:
[0027] (a) coating a plurality of layers of ammonium manganese ferric phosphate material layers outside the ammonium manganese ferric phosphate core to obtain a precursor;
[0028] (b) mixing the precursor, the lithium source and the carbon source, grinding, first drying and sintering;
[0029] The manganese-iron molar ratio of the ammonium manganese ferric phosphate core and each layer of the ammonium manganese ferric phosphate material layer increases radially from the inside to the outside.
[0030] The method for preparing lithium manganese iron phosphate comprises coating a plurality of layers of ammonium manganese iron phosphate material layers outside the ammonium manganese iron phosphate core, wherein the manganese iron molar ratio of the ammonium manganese iron phosphate core and each layer of the ammonium manganese iron phosphate material layer increases radially from the inside to the outside, thereby forming lithium manganese iron phosphate in which the manganese iron molar ratio increases radially from the core to the outside. The lithium manganese iron phosphate prepared by the method has good stability and excellent electrical properties, especially good electrical conductivity.
[0031] In order to prevent the sudden rise and fall problems of the dual voltage platform, the Mn / Fe molar ratio of each coating layer of lithium manganese iron phosphate from the inside to the outside increases slowly and equally, and the increase is controlled between 0.5 and 2.0 as much as possible.
[0032] From the inside to the outside along the radial direction, Mn with a slightly larger ionic radius 2+ The molar ratio gradually increases, which can broaden the Li + Transmission channel, and Mn 2+ The LMFP with a higher proportion and lower conductivity is placed in the outer layer, which can shorten the Li + The transmission distance is shortened, thereby improving the conductivity and enhancing the electrochemical performance of the LMFP cathode material.
[0033] From the inside to the outside along the radial direction, the Mn with a larger ionic radius 2+ The molar proportion increases, and the Fe with a small ionic radius 2+ The molar ratio is reduced, and the ion radius differentiation and ion concentration gradient are achieved, thereby improving the particle density and the compaction density of the LMFP positive electrode material.
[0034] By shaping a multilayer LMFP positive electrode material with differentiated Mn / Fe molar ratios from the inside to the outside, the difference between the 3.4V and 4.1V dual voltage platforms can be narrowed, the voltage platform difference can be smoothed and buffered, the voltage drop can be prevented, and the structural instability caused by it can be prevented, thus reducing the difficulty of management of the subsequent battery management system (BMS).
[0035] Furthermore, the chemical formula of the precursor is NH4Mn x Fe 1-x PO4, where the value of x is 0.6 to 0.8.
[0036] The precursor NH4Mn x Fe 1-x NH4 exists in PO4 + When synthesizing LMFP cathode materials, NH4 + It will decompose and release in the form of gas, forming a porous structure, which is beneficial to the sintering process. + Automatically and easily "falls" into the isophosphite structure to form an olivine-structured LMFP cathode material, and improves the wettability of the electrolyte to the particles, improving the Li + The accessibility to the interior of the particles and the surface activity of the particles can improve the specific capacity of the LMFP cathode material.
[0037] The present invention utilizes hydrothermal reaction to realize the solvation of insoluble ions, and adopts the method of introducing crystal seeds to adjust the particle size and particle size distribution, so as to realize Mn 2+ , Fe 2+ Uniform distribution at the atomic level improves the electrical properties of LMFP positive electrode materials and enhances product stability.
[0038] The precursor synthesis process is carried out under inert gas to avoid Mn 2+ , Fe 2+ It is oxidized during the synthesis process, thereby reducing the carbon loss and carbon escape caused by re-reduction during the subsequent preparation of LMFP positive electrode materials and improving the comprehensive utilization rate of carbon sources.
[0039] Furthermore, the preparation method of the ammonium manganese ferrous phosphate core comprises the following steps:
[0040] The mixed solution containing manganese source, iron source and phosphorus source is subjected to the first hydrothermal reaction; iron phosphate and ammonia water are added to the mixed system after the first hydrothermal reaction to perform the first reaction, the first solid-liquid separation, the first washing and the second drying. Taking full advantage of the characteristics of solution supersaturation and crystallization, iron phosphate is introduced into the mixed system after the first hydrothermal reaction to act as a crystal seed, break and disturb the metastable state of the supersaturated solution, thereby regulating the crystallization speed and particle size.
[0041] Further, the temperature of the first hydrothermal reaction is 100-150°C, including but not limited to any point value of 100°C, 110°C, 120°C, 130°C, 140°C or 150°C or a range value between any two of them.
[0042] Furthermore, the time of the first hydrothermal reaction is 2.0 to 6.0 h, including but not limited to any one of 2.0 h, 3.0 h, 4.0 h, 5.0 h or 6.0 h or a range between any two of them.
[0043] Furthermore, the pH of the first reaction is 2.0 to 6.0, including but not limited to any point value of 5.0, 5.3, 5.5, 5.8, 6.0, 6.3 or 6.5 or a range value between any two of them. If it is not within this range, co-precipitation and crystallization may not be possible, and the precipitation may affect the crystallinity, generate a potential series of crystal impurities, and affect the performance indicators of LMFP.
[0044] Furthermore, the molar ratio of manganese to iron in the ammonium manganese ferrophosphate core is (0.00-0.05):(9.95-10.00), including but not limited to 0.01:9.99, 0.02:9.98, 0.03:9.97, 0.04:9.96 or 0.05:9.95.
[0045] Furthermore, at least one layer (for example, it can be, but not limited to, 1 layer, 2 layers, 3 layers, 4 layers, 6 layers, 8 layers, 10 layers, 12 layers, 15 layers or 20 layers, any one of the point values or the range value between any two) of ammonium manganese iron phosphate material layer is coated outside the ammonium manganese iron phosphate core.
[0046] Furthermore, the ratio of the molar amount of iron in the iron phosphate added when preparing the ammonium manganese iron phosphate core to the molar amount of manganese and iron in the ammonium manganese iron phosphate material layer is (0.01-0.05): (0.20-0.30), including but not limited to 0.01:0.30, 0.02:0.28, 0.03:0.24, 0.04:0.22 or 0.05:0.20.
[0047] Further, the coating includes:
[0048] The mixed solution containing the manganese source, the iron source and the phosphorus source is subjected to a second hydrothermal reaction; the ammonium manganese ferrous phosphate core and ammonia water are added to the mixed system after the second hydrothermal reaction to carry out a second reaction, a second solid-liquid separation, a second washing and a third drying.
[0049] Furthermore, the coating is repeated several times, and several layers of ammonium manganese ferric phosphate material layers are coated outside the ammonium manganese ferric phosphate core.
[0050] If one layer of ammonium manganese ferrous phosphate material layer is coated on the outside of the ammonium manganese ferrous phosphate core, only one coating is required; if two layers of ammonium manganese ferrous phosphate material layers are coated on the outside of the ammonium manganese ferrous phosphate core, two coatings are required; if three layers of ammonium manganese ferrous phosphate material layers are coated on the outside of the ammonium manganese ferrous phosphate core, three coatings are required; and so on, when multiple layers of ammonium manganese ferrous phosphate material layers are required to be coated, multiple coatings are required accordingly, and it is only necessary to ensure that the manganese-iron molar ratio in the ammonium manganese ferrous phosphate material layer conforms to the rule of increasing successively from the inside to the outside along the radial direction, and the present invention does not make a specific limitation on the amplitude of the increase.
[0051] In some specific embodiments, the first ammonium manganese iron phosphate material layer, the second ammonium manganese iron phosphate material layer, the third ammonium manganese iron phosphate material layer, the fourth ammonium manganese iron phosphate material layer, the fifth ammonium manganese iron phosphate material layer, the sixth ammonium manganese iron phosphate material layer and the seventh ammonium manganese iron phosphate material layer are sequentially coated outside the ammonium manganese iron phosphate core, and the manganese iron molar ratio in the ammonium manganese iron phosphate core is (0.00-0.05): (9.95-10.00), and the manganese iron molar ratio in the first ammonium manganese iron phosphate material layer is 1~2:8~9, the molar ratio of manganese and iron in the second ammonium manganese iron phosphate material layer is 2~3:7~8, the molar ratio of manganese and iron in the third ammonium manganese iron phosphate material layer is 3~4:6~7, the molar ratio of manganese and iron in the fourth ammonium manganese iron phosphate material layer is 4~5:5~6, the molar ratio of manganese and iron in the fifth ammonium manganese iron phosphate material layer is 5~6:4~5, the molar ratio of manganese and iron in the sixth ammonium manganese iron phosphate material layer is 6~7:3~4, and the molar ratio of manganese and iron in the seventh ammonium manganese iron phosphate material layer is 7~8:2~3.
[0052] Furthermore, the temperature of the second hydrothermal reaction is 100-150°C.
[0053] Furthermore, the second hydrothermal reaction time is 2.0 to 6.0 hours.
[0054] Furthermore, the pH of the second reaction is 2.0 to 6.0, including but not limited to any point value of 5.0, 5.3, 5.5, 5.8, 6.0, 6.3 or 6.5 or a range value between any two of them. If it is not within this range, co-precipitation and crystallization may not be possible, and the precipitation may affect the crystallinity, produce a potential series of crystal impurities, and affect the performance indicators of LMFP.
[0055] Furthermore, the ratio of the molar number of the lithium source to the sum of the molar numbers of manganese and iron in the precursor is 1.00 to 1.03:1, including but not limited to 1.00:1, 1.01:1, 1.02:1 or 1.03:1.
[0056] Furthermore, the mass of the carbon source is 10wt% to 20wt% of the sum of the masses of the precursor and the lithium source, including but not limited to any point value of 10wt%, 12wt%, 14wt%, 16wt%, 18wt% or 20wt% or a range value between any two of them.
[0057] Furthermore, the particle size D of the slurry after grinding is 50 =0.25-0.45 μm, including but not limited to any point value of 0.25 μm, 0.27 μm, 0.29 μm, 0.31 μm, 0.33 μm, 0.35 μm, 0.37 μm, 0.39 μm, 0.41 μm, 0.43 μm or 0.45 μm or the range value between any two of them.
[0058] Furthermore, the heating rate of the sintering is 3-6°C / min, including but not limited to any point value of 3°C / min, 4°C / min, 5°C / min or 6°C / min or a range value between any two of them.
[0059] Furthermore, the sintering holding temperature is 500-800°C, including but not limited to any point value of 500°C, 550°C, 600°C, 650°C, 700°C, 750°C or 800°C or a range value between any two of them.
[0060] Furthermore, the sintering holding time is 5 to 10 hours, including but not limited to any one of 5 hours, 6 hours, 7 hours, 8 hours, 9 hours or 10 hours or a range between any two of them.
[0061] Through sintering, the ammonium ions are ensured to decompose stably and slowly, releasing ammonia gas, forming a three-dimensional porous structure (outward); the Li source is decomposed to provide a driving force for the lithium ions to embed inward (inward); a structurally stable crystalline structure is formed; the appropriate specific surface area is conducive to improving the active sites of the material and improving the electrical performance.
[0062] Limiting the sintering conditions to a certain range can ensure that the release rate of ammonium ions is within a reasonable range. If the ammonium ions are released too quickly, a strong airflow will be formed, which will hinder the bidirectional transmission inside and outside, slow down the speed of lithium ions with low ion mobility being embedded in the lattice, and cannot ensure the uniformity of lithium ion embedding, affecting the performance of LMFP; releasing ammonium ions too quickly will lead to excessive porosity and excessive specific surface area, which is not conducive to the processing technology such as battery homogenization. If appropriate sintering conditions are not adopted, the crystallinity cannot be improved, and the relative density of the material cannot be guaranteed, which will affect the electrical properties and compaction density.
[0063] Furthermore, the first solid-liquid separation and the second solid-liquid separation are performed by centrifugal filtration.
[0064] Furthermore, the rotation speed of the centrifugal filtration is 5000-10000 rpm, including but not limited to any point value of 5000 rpm, 5500 rpm, 6000 rpm, 6500 rpm, 7000 rpm, 7500 rpm, 8000 rpm, 8500 rpm, 9000 rpm, 9500 rpm or 10000 rpm or the range value between any two of them.
[0065] Furthermore, the centrifugal filtration time is 10 to 20 minutes, including but not limited to any point value of 10 minutes, 12 minutes, 14 minutes, 16 minutes, 18 minutes or 20 minutes, or a range value between any two of them.
[0066] The present invention does not limit the specific type of manganese source, and conventional manganese sources in the art can be used to implement the technical solution of the present invention. In some specific embodiments, the manganese source includes but is not limited to at least one of manganese chloride, manganese sulfate, manganese oxalate, manganese acetate or manganese carbonate.
[0067] The present invention does not limit the specific type of the iron source, and conventional iron sources in the art can be used to implement the technical solution of the present invention. In some specific embodiments, the iron source includes but is not limited to at least one of ferrous chloride, ferrous sulfate, ferrous oxalate or ferrous nitrate.
[0068] The present invention does not limit the specific type of phosphorus source, and conventional phosphorus sources in the art can be used to implement the technical solution of the present invention. In some specific embodiments, the phosphorus source includes but is not limited to at least one of ammonium phosphate, diammonium phosphate or diammonium hydrogen phosphate.
[0069] The present invention does not limit the specific type of lithium source, and conventional lithium sources in the field can be used to implement the technical solution of the present invention. In some specific embodiments, the lithium source includes but is not limited to at least one of lithium carbonate, lithium oxalate, lithium acetate, lithium nitrate or lithium hydroxide.
[0070] The present invention does not limit the specific type of carbon source, and conventional carbon sources in the art can be used to implement the technical solution of the present invention. In some specific embodiments, the carbon source includes but is not limited to at least one of glucose, sucrose, soluble starch or cellulose.
[0071] Furthermore, the first drying includes but is not limited to: spray drying.
[0072] Furthermore, the inlet air temperature of the spray drying is 200-300°C, including but not limited to any point value of 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C or 300°C or a range value between any two of them.
[0073] Furthermore, the outlet air temperature of the spray drying is 85-100°C, including but not limited to any point value of 85°C, 90°C, 95°C or 100°C or a range value between any two of them.
[0074] Furthermore, the second drying includes but is not limited to: vacuum drying.
[0075] Furthermore, the third drying includes but is not limited to: vacuum drying.
[0076] Furthermore, the organic solvent used to dissolve the manganese source, the iron source and the phosphorus source includes but is not limited to: at least one of ethylene glycol, ethanol, n-butanol or cyclohexane.
[0077] Furthermore, the first hydrothermal reaction, the second hydrothermal reaction and the sintering are carried out under the protection of an inert gas. The hydrothermal reaction is carried out under the protection of an inert gas to prevent the Mn 2+ , Fe 2+ Oxidized.
[0078] Furthermore, the inert gas includes but is not limited to: nitrogen and / or argon.
[0079] Another aspect of the present invention also relates to lithium manganese iron phosphate prepared by the lithium manganese iron phosphate preparation method.
[0080] The lithium manganese iron phosphate has a structure in which the manganese and iron moles increase radially from the inner core to the outer core, and has excellent electrochemical performance and a stable structure.
[0081] Furthermore, the D of the lithium manganese iron phosphate 50= 0.80-1.40 μm, including but not limited to any point value of 0.80 μm, 1.00 μm, 1.20 μm or 1.40 μm or the range value between any two. After sintering, LMFP has soft agglomeration and a large number of pores inside. If it is not properly deagglomerated to form a reasonable particle size distribution, the porosity will be too high, the energy density cannot be improved, and it is not conducive to the effective and comprehensive infiltration of the electrolyte, resulting in a series of risks such as large internal resistance and severe charge and discharge polarization.
[0082] In some specific embodiments, the chemical formula of the lithium manganese iron phosphate includes but is not limited to LiMn 0.6 Fe 0.4 PO4 or LiMn 0.7 Fe 0.3 PO4.
[0083] Another aspect of the present invention also relates to a positive electrode material, wherein the positive electrode material includes the lithium manganese iron phosphate prepared by the preparation method of the lithium manganese iron phosphate or the lithium manganese iron phosphate.
[0084] Another aspect of the present invention also relates to a secondary battery, comprising the positive electrode material.
[0085] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0086] Example 1
[0087] The method for preparing lithium manganese iron phosphate provided in this embodiment comprises the following steps:
[0088] Step S1: The purified Mn and Fe sources are graded in proportion and mixed with an organic solvent to obtain mixture A1, mixture A2, mixture A3, mixture A4, mixture A5, mixture A6, mixture A7 and mixture A8 respectively;
[0089] Step S2: Mix the mixture A1 in step S1 and the P source, and perform a hydrothermal reaction to dissolve them completely to form a suspension B1;
[0090] Step S3: adding iron phosphate to the suspension B1, and adjusting the pH by adding ammonia water to control the crystallization rate, regulate the crystal size, produce precipitation, and then centrifuge to produce a filtrate and a precipitate C1;
[0091] Step S4: washing the precipitate C1 with deionized water for multiple times, and then drying to obtain the product G1 (ammonium manganese iron phosphate core);
[0092] Step S5: Mix the mixture A2 in step S1 with the P source and the organic solvent, and reuse the filtrate produced in step S3 to perform a hydrothermal reaction to dissolve all of them to form a suspension B2;
[0093] Step S6: Add the product G1 produced in step S4 to the suspension B2, the ratio of the molar amount of iron in the ferric phosphate added in step 3 to the molar amount of manganese iron in the product G1 is 0.05:0.20, and adjust the pH by adding ammonia water to control the crystallization speed, regulate the grain size, produce precipitation, and then centrifuge and filter to produce a filtrate and a precipitate C2;
[0094] Step S7: washing the precipitate C2 with deionized water for multiple times, and then drying to obtain the product G2;
[0095] Step S8: by repeating the operations similar to step S5, step S6 and step S7, a product G8 (precursor) is finally obtained;
[0096] Step S9: mixing the product G8 obtained in step S8 with a Li source and a carbon source, and wet grinding the mixture to obtain a grinding slurry;
[0097] Step S10: drying, sintering and crushing the polishing slurry obtained in step S9 to obtain LMFP.
[0098] In step S1, the Mn / Fe molar ratios of mixture A1, mixture A2, mixture A3, mixture A4, mixture A5, mixture A6, mixture A7, and mixture A8 are 1:9, 2:8, 3:7, 4:6, 5:5, 6:4, 7:3, and 8:2, respectively;
[0099] In step S3, ammonia water is added to control the pH to 6.0;
[0100] In steps S3 and S6, the centrifuge speed is 8000 rpm and the centrifugation time is 15 min;
[0101] In steps S4 and S7, vacuum drying is used for drying;
[0102] In step S6, adding ammonia water to adjust the pH to 6.0;
[0103] The temperature of the hydrothermal reaction involved in this embodiment is 100°C, the time is 2.0h, and the hydrothermal reaction is carried out under the protection of inert gas;
[0104] In step S9, the ratio of the molar number of the lithium source to the sum of the molar numbers of manganese and iron in the precursor is 1.02:1; the mass of the carbon source is 15wt% of the sum of the mass of the precursor and the lithium source;
[0105] In step S9, the particle size D of the polishing slurry is 50 =0.35μm;
[0106] In step S10, the drying is performed by spray drying, and the inlet air temperature of the spray drying is 250° C. and the outlet air temperature is 95° C.;
[0107] In step S10, sintering is performed under the protection of an inert gas, wherein the inert gas is nitrogen; sintering is performed according to a process of a heating rate of 5°C / min, a holding temperature of 650°C, and a holding time of 7h;
[0108] In step S10, the crushed particle size is D 50 =1.20μm;
[0109] In this embodiment, the Mn source is manganese sulfate; the Fe source is ferrous sulfate; the P source is ammonium phosphate; the Li source is lithium carbonate; and the carbon source is glucose.
[0110] Example 2
[0111] The method for preparing lithium manganese iron phosphate provided in this embodiment comprises the following steps:
[0112] Step S1: The purified Mn and Fe sources are graded in proportion and mixed with an organic solvent to obtain a mixture A1 and a mixture A2 respectively;
[0113] Step S2: Mix the mixture A1 in step S1 and the P source, and perform a hydrothermal reaction to dissolve them completely to form a suspension B1;
[0114] Step S3: adding iron phosphate to the suspension B1, and adjusting the pH by adding ammonia water to control the crystallization rate, regulate the crystal size, produce precipitation, and then centrifuge to produce a filtrate and a precipitate C1;
[0115] Step S4: washing the precipitate C1 with deionized water for multiple times, and then drying to obtain the product G1 (ammonium manganese iron phosphate core);
[0116] Step S5: Mix the mixture A2 in step S1 with the P source and the organic solvent, and reuse the filtrate produced in step S3 to perform a hydrothermal reaction to dissolve all of them to form a suspension B2;
[0117] Step S6: Add the product G1 produced in step S4 to the suspension B2, the ratio of the molar amount of iron in the ferric phosphate added in step 3 to the molar amount of manganese iron in the product G1 is 0.01:0.23, and adjust the pH by adding ammonia water to control the crystallization rate, regulate the grain size, produce precipitation, and then centrifuge and filter to produce a filtrate and a precipitate C2;
[0118] Step S7: washing the precipitate C2 with deionized water for multiple times, and then drying to obtain the product G2 (precursor);
[0119] Step S8: mixing the product G2 obtained in step S7 with a Li source and a carbon source, and wet grinding the mixture to obtain a grinding slurry;
[0120] Step S9: Dry, sinter and crush the polishing slurry obtained in step S8 to obtain LMFP.
[0121] In step S1, the Mn / Fe molar ratios of mixture A1 and mixture A2 are 5:5 and 7:3, respectively;
[0122] In step S3, ammonia water is added to control the pH to 5.0;
[0123] In steps S3 and S6, the centrifuge speed is 5000 rpm and the centrifugation time is 10 min;
[0124] In steps S4 and S7, vacuum drying is used for drying;
[0125] In step S6, adding ammonia water to adjust the pH to 5.0;
[0126] The temperature of the hydrothermal reaction involved in this embodiment is 150°C, the time is 6.0h, and the hydrothermal reaction is carried out under the protection of inert gas;
[0127] In step S8, the ratio of the molar number of the lithium source to the sum of the molar numbers of manganese and iron in the precursor is 1.00:1; the mass of the carbon source is 10wt% of the sum of the mass of the precursor and the lithium source;
[0128] In step S8, the particle size D of the polishing slurry is 50 =0.25μm;
[0129] In step S9, the drying is performed by spray drying, and the inlet air temperature of the spray drying is 200° C. and the outlet air temperature is 85° C.;
[0130] In step S9, sintering is performed under the protection of an inert gas, wherein the inert gas is argon; sintering is performed according to a process of a heating rate of 3°C / min, a holding temperature of 500°C, and a holding time of 5h;
[0131] In step S9, the crushed particle size is D 50 =0.80μm;
[0132] In this embodiment, the Mn source is manganese chloride; the Fe source is ferrous chloride; the P source is ammonium dihydrogen phosphate; in step S9, the Li source is lithium oxalate; and the carbon source is sucrose.
[0133] Example 3
[0134] The method for preparing lithium manganese iron phosphate provided in this embodiment comprises the following steps:
[0135] Step S1: The purified Mn and Fe sources are graded in proportion and mixed with an organic solvent to obtain mixture A1, mixture A2, mixture A3 and mixture A4 respectively;
[0136] Step S2: Mix the mixture A1 in step S1 and the P source, and perform a hydrothermal reaction to dissolve them completely to form a suspension B1;
[0137] Step S3: adding iron phosphate to the suspension B1, and adjusting the pH by adding ammonia water to control the crystallization rate, regulate the crystal size, produce precipitation, and then centrifuge to produce a filtrate and a precipitate C1;
[0138] Step S4: washing the precipitate C1 with deionized water for multiple times, and then drying to obtain the product G1 (ammonium manganese iron phosphate core);
[0139] Step S5: Mix the mixture A2 in step S1 with the P source and the organic solvent, and reuse the filtrate produced in step S3 to perform a hydrothermal reaction to dissolve all of them to form a suspension B2;
[0140] Step S6: Add the product G1 produced in step S4 to the suspension B2, the ratio of the molar amount of iron in the ferric phosphate added in step 3 to the molar amount of manganese iron in the product G1 is 0.03:0.25, and adjust the pH by adding ammonia water to control the crystallization speed, regulate the grain size, produce precipitation, and then centrifuge and filter to produce a filtrate and a precipitate C2;
[0141] Step S7: washing the precipitate C2 with deionized water for multiple times, and then drying to obtain the product G2;
[0142] Step S8: by repeating the operations similar to step S5, step S6 and step S7, product G4 (precursor) is finally obtained;
[0143] Step S9: mixing the product G4 obtained in step S8 with a Li source and a carbon source, and wet grinding the mixture to obtain a grinding slurry;
[0144] Step S10: drying, sintering and crushing the polishing slurry obtained in step S9 to obtain LMFP.
[0145] In step S1, the Mn / Fe molar ratios of mixture A1, mixture A2, mixture A3 and mixture A4 are 2.1:7.9, 4.1:5.9, 6.1:3.9 and 8.1:1.9 respectively;
[0146] In step S3, ammonia water is added to control the pH value between 6.5;
[0147] In steps S3 and S6, the centrifuge speed is 10000 rpm and the centrifugation time is 20 min;
[0148] In steps S4 and S7, vacuum drying is used for drying;
[0149] In step S6, adding ammonia water to adjust the pH to 6.5;
[0150] The temperature of the hydrothermal reaction involved in this embodiment is 130°C, the time is 5h, and the hydrothermal reaction is carried out under the protection of inert gas;
[0151] In step S9, the ratio of the molar number of the lithium source to the sum of the molar numbers of manganese and iron in the precursor is 1.03:1; the mass of the carbon source is 20wt% of the sum of the mass of the precursor and the lithium source;
[0152] In step S9, the particle size D of the polishing slurry is 50 =0.45μm;
[0153] In step S10, the drying is preferably spray drying, and the inlet air temperature of the spray drying is 300° C. and the outlet air temperature is 100° C.;
[0154] In step S10, sintering is performed under the protection of an inert gas, wherein the inert gas is nitrogen; sintering is performed according to a process of a heating rate of 6°C / min, a holding temperature of 800°C, and a holding time of 10h;
[0155] In step S10, the crushed particle size is D 50 =1.40μm;
[0156] In this embodiment, the Mn source is manganese oxalate; the Fe source is ferrous oxalate; the P source is diammonium hydrogen phosphate; in step S9, the Li source is lithium acetate; and the carbon source is soluble starch.
[0157] Example 4
[0158] The method for preparing lithium manganese iron phosphate provided in this embodiment comprises the following steps:
[0159] Step S1: The purified Mn and Fe sources are graded in proportion and mixed with an organic solvent to obtain mixture A1, mixture A2, mixture A3, mixture A4, mixture A5, mixture A6, mixture A7, mixture A8, mixture A9, mixture A10, mixture A11 and mixture A12 respectively;
[0160] Step S2: Mix the mixture A1 in step S1 and the P source, and perform a hydrothermal reaction to dissolve them completely to form a suspension B1;
[0161] Step S3: adding iron phosphate to the suspension B1, and adjusting the pH by adding ammonia water to control the crystallization rate, regulate the crystal size, produce precipitation, and then centrifuge to produce a filtrate and a precipitate C1;
[0162] Step S4: washing the precipitate C1 with deionized water for multiple times, and then drying to obtain the product G1 (ammonium manganese iron phosphate core);
[0163] Step S5: Mix the mixture A2 in step S1 with the P source and the organic solvent, and reuse the filtrate produced in step S3 to perform a hydrothermal reaction to dissolve all of them to form a suspension B2;
[0164] Step S6: Add the product G1 produced in step S4 to the suspension B2, the ratio of the molar amount of iron in the ferric phosphate added in step 3 to the molar amount of manganese iron in the product G1 is 0.03:0.24, and adjust the pH by adding ammonia water to control the crystallization speed, regulate the grain size, produce precipitation, and then centrifuge and filter to produce a filtrate and a precipitate C2;
[0165] Step S7: washing the precipitate C2 with deionized water for multiple times, and then drying to obtain the product G2;
[0166] Step S8: by repeating the operations similar to step S5, step S6 and step S7, product G12 (precursor) is finally obtained;
[0167] Step S9: mixing the product G12 obtained in step S8 with a Li source and a carbon source, and wet grinding the mixture to obtain a grinding slurry;
[0168] Step S10: drying, sintering and crushing the polishing slurry obtained in step S9 to obtain LMFP.
[0169] In step S1, the Mn / Fe molar ratios of mixture A1, mixture A2, mixture A3, mixture A4, mixture A5, mixture A6, mixture A7, mixture A8, mixture A9, mixture A10, mixture A11 and mixture A12 are 3:7, 3.5:6.5, 4:6, 4.5:5.5, 5:5, 5.5:4.5, 6:4, 6.5:3.5, 7:3, 7.5:2.5, 8:2 and 8.5:1.5, respectively;
[0170] In step S3, ammonia water is added to control the pH to 5.5;
[0171] In steps S3 and S6, the centrifuge speed is 9000 rpm and the centrifugation time is 17 min;
[0172] In steps S4 and S7, vacuum drying is used for drying;
[0173] In step S6, adding ammonia water to adjust the pH to 5.5;
[0174] The temperature of the hydrothermal reaction involved in this embodiment is 140°C, the time is 5.0h, and the hydrothermal reaction is carried out under the protection of inert gas;
[0175] In step S9, the ratio of the molar number of the lithium source to the sum of the molar numbers of manganese and iron in the precursor is 1.02:1; the mass of the carbon source is 14wt% of the sum of the mass of the precursor and the lithium source;
[0176] In step S9, the particle size D of the polishing slurry is 50 =0.40 μm;
[0177] In step S10, the drying is spray drying, and the inlet air temperature of the spray drying is 270° C. and the outlet air temperature is 95° C.;
[0178] In step S10, sintering is performed under the protection of an inert gas, wherein the inert gas is argon; sintering is performed according to a process of a heating rate of 4°C / min, a holding temperature of 600°C, and a holding time of 9h;
[0179] In step S10, the crushed particle size is D 50 =1.00μm;
[0180] In this embodiment, the Mn source is manganese acetate; the Fe source is ferrous nitrate; the P source is ammonium phosphate; in step S9, the Li source is lithium nitrate; and the carbon source is cellulose.
[0181] Comparative Example 1
[0182] In conventional lithium manganese iron phosphate in the art, the molar ratio of manganese to iron is equal from the inside to the outside along the radial direction.
[0183] Comparative Example 2
[0184] The difference between the comparative example and Example 1 is that the temperature of the hydrothermal reaction is 95°C.
[0185] Comparative Example 3
[0186] The difference between the comparative example and Example 1 is that ammonia water is added in step S3 and step S6 to adjust the pH to 7.
[0187] Comparative Example 4
[0188] The difference between the comparative example and the embodiment 1 is that the holding temperature of the sintering in step S10 is 850°C.
[0189] Experimental example
[0190] The prepared lithium manganese iron phosphate was subjected to performance testing, and the test method was based on the group standard, the file number was T / CIAPS0029-2023, and the file name was "Lithium manganese iron phosphate positive electrode material for lithium-ion batteries". The results are shown in Table 1.
[0191] Table 1
[0192]
[0193] It can be seen from Table 1 that the compacted density of Examples 1 to 4 is basically stable at 2.20 to 2.30 g / cm 3 , the overall resistivity is ≤15.0Ω*cm, and the overall 0.1C discharge capacity is ≥152mAh / g. By comparing Examples 1 to 4 with Comparative Example 1, it can be seen that although the compaction density of Comparative Example 1 is not much different from that of the embodiment, the 0.1 discharge capacity is low and the resistivity is as high as about 40Ω*cm. This is because the ionic resistivity of LiMnPO4 itself is very high, which affects the Li + Spontaneous effective transmission, resulting in performance deviation. Comparing Examples 1 to 4 with Comparative Examples 2 and 3, the comparative examples failed to effectively control the crystallization parameters and crystal morphology of the precursor, resulting in the adverse effects of the precursor being transmitted to the rear-end LMFP positive electrode material, making the compaction density, resistivity and electrical properties less than ideal. Comparing Examples 1 to 4 with Comparative Example 4, although the compaction density of the comparative example is very high, the resistivity and 0.1C discharge specific capacity are seriously deteriorated. This is because the sintering temperature is too high, which will cause the particles to grow excessively and agglomerate, reducing the necessary porosity of the LMFP positive electrode material, resulting in Li + The "tortuous" transmission channel affects the wettability of the electrolyte, and ultimately increases the compaction density at the expense of physical parameters and electrical performance indicators, which is counterproductive and not worth the cost.
[0194] Figure 1 0.1C charge-discharge curves of Example 1 and Comparative Example 1. Figure 1 It can be seen from the discharge process that when the high voltage platform of Example 1 transitions to the low voltage platform, the overall transition is buffered and smooth, and the platform specific capacity accounts for a high proportion, while the smoothness of the voltage platform transition of Comparative Example 1 is low, the sudden drop is serious, and the platform specific capacity accounts for a low proportion; near the tail of the voltage platform, the discharge curve of Comparative Example 1 is severely polarized and decays rapidly to the cut-off voltage. This is because the resistivity is large, resulting in a large effective transmission distance of lithium ions during the discharge process, and the stress generated by the electrical and thermal lattice expansion cannot be effectively and timely released, resulting in severe discharge polarization and low electrical performance.
[0195] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A method for preparing lithium manganese iron phosphate, characterized in that: The following steps are involved: (a) coating a plurality of layers of ammonium manganese ferric phosphate material layers outside the ammonium manganese ferric phosphate core to obtain a precursor; (b) mixing the precursor, the lithium source and the carbon source, grinding, first drying and sintering; The manganese-iron molar ratio of the ammonium manganese ferric phosphate core and each layer of the ammonium manganese ferric phosphate material layer increases radially from the inside to the outside.
2. The method for preparing lithium iron manganese phosphate according to claim 1, characterized in that: The preparation method of the ammonium manganese ferric phosphate core comprises the following steps: A mixed solution containing a manganese source, an iron source and a phosphorus source is subjected to a first hydrothermal reaction; iron phosphate and aqueous ammonia are added to the mixed system after the first hydrothermal reaction to perform a first reaction, a first solid-liquid separation, a first washing and a second drying.
3. The method for preparing lithium manganese iron phosphate according to claim 2, characterized in that: Includes at least one of the following technical features: (1) The temperature of the first hydrothermal reaction is 100-150° C.; (2) The time of the first hydrothermal reaction is 2.0 to 6.0 hours; (3) The pH of the first reaction is 2.0 to 6.
0.
4. The method for preparing lithium iron manganese phosphate according to claim 2, characterized in that: The coating comprises: The mixed solution containing the manganese source, the iron source and the phosphorus source is subjected to a second hydrothermal reaction; the ammonium manganese ferrous phosphate core and ammonia water are added to the mixed system after the second hydrothermal reaction to carry out a second reaction, a second solid-liquid separation, a second washing and a third drying.
5. The method for preparing lithium iron manganese phosphate according to claim 4, characterized in that: Includes at least one of the following technical features: (1) The temperature of the second hydrothermal reaction is 100-150° C.; (2) The time of the second hydrothermal reaction is 2.0 to 6.0 hours; (3) The pH of the second reaction is 2.0 to 6.
0.
6. The method for preparing lithium manganese iron phosphate according to claim 1, characterized in that: Includes at least one of the following technical features: (1) Repeat the coating for several times to coat the ammonium manganese ferric phosphate core with several layers of the ammonium manganese ferric phosphate material layer; (2) the ratio of the molar number of the lithium source to the sum of the molar numbers of manganese and iron in the precursor is 1.00 to 1.03:1; (3) The mass of the carbon source is 10 wt% to 20 wt% of the sum of the mass of the precursor and the lithium source.
7. The method for preparing lithium manganese iron phosphate according to claim 1, characterized in that: Includes at least one of the following technical features: (1) The heating rate of the sintering is 3 to 6°C / min; (2) The sintering holding temperature is 500-800° C.; (3) The sintering holding time is 5 to 10 hours.
8. Lithium manganese iron phosphate prepared by the method for preparing lithium manganese iron phosphate according to any one of claims 1 to 7.
9. A positive electrode material, characterized in that: The invention relates to the lithium manganese iron phosphate prepared by the method for preparing the lithium manganese iron phosphate according to any one of claims 1 to 7 or the lithium manganese iron phosphate according to claim 8.
10. A secondary battery, characterized in that: Comprising the positive electrode material according to claim 9.
Citation Information
Patent Citations
Multi-phosphate positive electrode material, preparation method thereof and secondary battery
CN115036476A
Preparation method of ammonium manganese iron phosphate precursor and lithium manganese iron phosphate
CN118164461A
Ammonium manganese iron phosphate precursor and preparation method therefor, lithium manganese iron phosphate positive electrode active material, and secondary battery
WO2024045174A1