Starch-based hard carbon negative electrode material and preparation method and application thereof
Through the synergistic effect of acidic substances and citrate, it catalyzes the dehydration and cross-linking reactions of starch, combined with segmented carbonization treatment, to solve the foaming and melting problems of starch-based hard carbon materials during heat treatment, and improves the performance of hard carbon anodes. The electrochemical properties and production efficiency of the material are suitable for high-performance sodium-ion batteries.
Patent Information
- Application Number
- CN202410848532.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
AI Technical Summary
In the existing technology, when starch is used as a carbon source to prepare hard carbon anode materials, starch is prone to cross-linking, foaming, fusion, and expansion during heat treatment, resulting in low production efficiency and poor electrochemical performance, making it difficult to achieve high performance and low cost. of hard carbon material.
Acidic substances and citrate are used as synergistic additives to reduce pre-oxidation steps by catalyzing the dehydration and cross-linking reactions of starch, maintaining the natural morphology of starch, and forming a closed pore structure through segmented carbonization treatment to increase the compaction density of the material. and electrochemical performance.
It achieves high compaction density, volumetric energy density, rate performance and cycle stability of hard carbon anode materials, ensures high first-cycle Coulombic efficiency and reversible specific capacity of sodium-ion batteries, and solves the problem of melting of starch-based materials during the carbonization process. And the foaming problem.
Smart Images

Figure CN118851143A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of negative electrode materials and relates to a starch-based hard carbon negative electrode material and a preparation method and application thereof. Background Art
[0002] Sodium-ion batteries and lithium-ion batteries have the same working principle and similar production and manufacturing technologies. The abundance of sodium in the earth's crust is much higher than that of lithium, and it is widely distributed and inexpensive. Vigorously developing sodium-ion battery technology can, to a certain extent, alleviate some of the problems caused by the shortage of lithium resources. Sodium-ion batteries are a beneficial supplement to lithium-ion batteries. The successful commercialization of lithium-ion batteries is inseparable from the development of graphite negative electrode materials. Similarly, for sodium-ion batteries to be commercialized, a negative electrode material with excellent performance and low cost must be developed. At present, disordered carbon represented by hard carbon has become a very promising negative electrode material in the industrialization of sodium-ion batteries due to its abundant raw materials, simple synthesis and low working potential.
[0003] So far, the methods reported to improve the performance of hard carbon materials include increasing the interlayer spacing of hard carbon; optimizing the pore structure of hard carbon to promote the storage of sodium ions or sodium clusters in a suitable pore structure; introducing heteroatoms (oxygen, nitrogen, sulfur, phosphorus, etc.) or defects to increase more adsorption sites, etc. However, large-scale production of high-performance hard carbon materials still faces arduous challenges. High-capacity materials are often activated by physical or chemical methods and have a high specific surface area, but their high production cost and low initial coulombic efficiency have greatly limited the practical use of hard carbon negative electrodes in sodium ion batteries. Therefore, how to solve the above problems by designing better materials to improve electrochemical performance is still the focus of the current development of hard carbon negative electrode materials.
[0004] The precursors of hard carbon negative electrode materials come from a wide range of sources, including asphalt, resin and biomass. Among them, biomass has become the fastest industrialized material technology system in the hard carbon industry due to its excellent performance, wide sources and sustainable development of derived carbon. Starch can be produced from various high-yield food crops such as corn, potatoes, sweet potatoes and cassava, and has a stable supply system. In addition, starch has purification steps such as soaking and washing during the production process, so that starch has fewer impurities and better uniformity than other biomass materials. Therefore, the consistency of starch in preparing raw hard carbon is better than other biomass materials. For example, CN116621158A discloses asphalt / starch derived hard carbon, its preparation method, and negative electrode material containing it. Its preparation method includes the following steps: S1 asphalt, starch, ammonium salt, and catalyst are blended to obtain a pretreated product; S2 the pretreated product is placed in an atmosphere, heated to react, and an intermediate is obtained; S3 a protective gas is introduced into the intermediate, and carbonization is performed to obtain asphalt / starch derived hard carbon. For example, CN116692832A discloses a hard carbon negative electrode material and its preparation method and application. The preparation of the hard carbon negative electrode material includes the following steps: (1) starch, dispersant, and modifier are mixed in water, and a carbon precursor is obtained after drying; (2) the carbon precursor is subjected to high-temperature dehydration and carbonization treatment in sequence to obtain a hard carbon substrate; (3) the hard carbon substrate is mixed with a fluorine-containing substance in water or an organic solvent, and a hard carbon substrate with a fluorine-containing substance coated on the surface is obtained after drying; (4) the hard carbon substrate with a fluorine-containing substance coated on the surface is placed in a mixed atmosphere containing hydrocarbons, and carbon filling is performed on the surface to obtain the hard carbon negative electrode material. The hard carbon negative electrode material prepared by the above method has a stable structure, and the fluorine-containing substance coated on the surface of the hard carbon substrate forms an interfacial activation layer. The negative electrode material filled with carbon free radicals can effectively improve the initial coulomb efficiency and cycle performance of the battery. However, when starch is selected as the carbon source in the above literature, the starch will cross-link and foam during the heat treatment process, and the volume will expand several times, which seriously reduces the production efficiency.
[0005] Therefore, it is currently worth studying how to solve the problems of starch melting, compaction, foaming, and expansion when preparing hard carbon negative electrode materials using starch as a carbon source, and to improve the electrochemical performance of starch-based hard carbon negative electrode materials. Summary of the invention
[0006] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a starch-based hard carbon negative electrode material and a preparation method and use thereof. The present invention effectively solves the problem of fusion (adhesion and compaction between materials) during the carbonization of starch through the synergistic effect of the first additive of acidic substance and the second additive of citrate, reduces the process steps of starch pre-oxidation, and allows the starch to maintain a relatively high natural morphology during the carbonization process, so that the obtained hard carbon negative electrode material increases the compaction density of the negative electrode sheet, increases the volume energy density of the battery cell, and also has good rate performance and cycle stability.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing a starch-based hard carbon negative electrode material, the preparation method comprising the following steps:
[0009] Mixing the first additive, the second additive and starch, and carbonizing to obtain the starch-based hard carbon negative electrode material;
[0010] Wherein, the first additive includes an acidic substance; and the second additive includes citrate.
[0011] It should be noted that the starch raw material in the present invention is food-grade starch, including but not limited to potato starch, sweet potato starch, tapioca starch, corn starch, wheat starch or pea starch.
[0012] The preparation method provided by the present invention catalyzes the dehydration process of starch material through the synergistic effect of the first additive of acidic substance and the second additive of citrate; at the same time, the starch undergoes a cross-linking reaction with the first additive and the second additive during the carbonization process, the number of hydroxyl groups in the starch raw material molecules after cross-linking is reduced, and the probability of 1,6-glycosidic bond formation is reduced, thereby solving the problems of foaming, melting and the like generated in the subsequent processing of the starch raw material, reducing the process steps of starch pre-oxidation, and allowing the starch to maintain a relatively high natural morphology during the carbonization process; the second additive containing citrate will produce metal oxides during the carbonization process, which will heat the starch raw material When the treated carbon material is purified, these generated metal oxides are washed and removed, resulting in pores on the surface and inside the carbon material; thereby, the obtained hard carbon negative electrode material improves the compaction density of the negative electrode plate and the volume energy density of the battery cell. The hard carbon negative electrode material contains a large number of closed closed pores and has good rate performance and cycle stability. When the prepared negative electrode material is used in sodium ion batteries, the rapid diffusion of solvated sodium ions in the carbon material during the charge and discharge process is guaranteed, and the battery has a high rate performance; it can also ensure that the carbon material has a high sodium storage capacity, and the battery has a high first-week coulomb efficiency and reversible specific capacity.
[0013] In the present invention, the first additive, the second additive and starch are indispensable and work together to reduce the fusion between particles, while the reversible specific capacity of the material is above 310 mAh / g; if only the second additive of citrate is contained, the reversible specific capacity of the material cannot be above 310 mAh / g; if only the first additive of acidic substance is contained, the problem of reducing the fusion between particles cannot be solved.
[0014] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0015] Preferably, the mixed raw materials further include a solvent.
[0016] The present invention does not impose any particular limitation on the type of solvent, and is applicable to any type of solvent that can dissolve the first additive, the second additive and starch and does not cause adverse reactions, including but not limited to water and / or ethanol.
[0017] Preferably, the mass ratio of the total mass of the starch, the first additive and the second additive to the solvent is 10:(0.5-4):3, for example 10:0.5:3, 10:0.75:3, 10:1:3, 10:1.25:3, 10:1.5:3, 10:2:3, 10:2.5:3, 10:3:3, 10:3.5:3 or 10:4:3, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0018] The present invention mixes starch and the first additive and the second additive by liquid phase mixing, which is more conducive to the uniform and sufficient reaction of each component, reduces the fusion between material particles, and retains the natural morphology of the material; and by further adjusting the mass ratio of the total mass of the first additive and the second additive to the mass of the solvent to 10: (0.5-4): 3, not only the melting and foaming problems of starch during carbonization are solved, but also the material has a higher first effect and reversible specific capacity, so that the Rayleigh structure and spiral structure distribution inside the obtained hard carbon negative electrode material are the most ideal.
[0019] Preferably, the mass ratio of the first additive to the second additive is (1-2):1, for example 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1 or 2:1, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] In the present invention, if the mass ratio of the first additive to the second additive is too large, that is, too much of the first additive is added, it is not conducive to reducing production costs and will reduce the carbon yield; and if the mass ratio is too small, that is, too little of the first additive is added, it will lead to low coulombic efficiency and reversible specific capacity of the material in the first electrochemical cycle.
[0021] Preferably, the acidic substance includes any one of boric acid, phenylboric acid or citric acid or a combination of at least two thereof, preferably includes boric acid and / or phenylboric acid.
[0022] Furthermore, when the acidic substance provided by the present invention includes boric acid or phenylboric acid, citrate effectively solves the fusion problem in the starch carbonization process through synergistic coordination, so that the obtained hard carbon negative electrode material improves the compaction density of the negative electrode plate and the volume energy density of the battery cell; at the same time, the incorporated boron element has a special electron-deficient structure, which can make the electron cloud distribution of the formed hard carbon material more even, which is beneficial to the transport of sodium ions and improves the rate performance of the battery cell; if the acidic substance is citric acid, the main component of citric acid after carbonization is carbon element, which does not have the characteristics of boron element, and has a lower capacity and poorer rate performance than the material with added boron element.
[0023] Preferably, the citrate salt comprises magnesium citrate.
[0024] Preferably, the mixed material is dried before carbonizing.
[0025] Preferably, the drying temperature is 85-120°C, for example 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C or 120°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the drying time is 12 to 24 hours, such as 12 hours, 15 hours, 18 hours, 20 hours or 24 hours, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0027] Preferably, the carbonization includes medium-temperature carbonization and high-temperature carbonization.
[0028] Preferably, low-temperature carbonization is performed followed by medium-temperature carbonization.
[0029] In the present invention, a low-temperature carbonization process can be carried out; and after adjusting the type and ratio of raw materials, the low-temperature carbonization process may not be carried out; at the same time, the present invention does not impose any restrictions on the atmosphere of low-temperature carbonization, and the present invention is applicable to conventional air atmosphere, oxygen atmosphere or protective atmosphere (protective atmosphere includes nitrogen atmosphere and inert gas atmosphere, inert gas includes argon and helium, etc.); that is, the low-temperature carbonization process in the present application is not a pre-oxidation process, and can be carried out in a non-oxygen atmosphere (such as a protective atmosphere, a nitrogen atmosphere or an inert gas atmosphere, etc.), which promotes cross-linking and polycondensation reactions between the components.
[0030] In the present invention, the thermal expansion phenomenon of the starch material during the carbonization process is better controlled through the segmented carbonization process, and the carbon yield is also improved; the low-temperature carbonization promotes the cross-linking and polycondensation reactions between the various components; and then the medium-temperature carbonization is carried out, which is conducive to the formation of a magnesium oxide template, providing a template for manufacturing sodium storage pores; the final high-temperature carbonization achieves an increase in the carbonization degree of the material, increases the conductivity of the material, reduces surface defects, promotes the shrinkage and development of larger pores toward sodium storage pores, reduces the specific surface area of the material, and improves the first effect and reversible specific capacity of the material.
[0031] Preferably, the temperature of the low-temperature carbonization is 120-220°C, for example 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C or 220°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the low-temperature carbonization time is 6 to 60 h, for example 6 h, 10 h, 15 h, 20 h, 25 h, 30 h, 35 h, 40 h, 45 h, 50 h, 55 h or 60 h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, the heating rate of the medium-temperature carbonization is 1 to 5°C / min, for example, 1°C / min, 2°C / min, 3°C / min, 4°C / min or 5°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the carbonization atmosphere of the medium-temperature carbonization is a protective atmosphere.
[0035] Preferably, the medium-temperature carbonization temperature is 500-600°C, for example, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C or 600°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] Preferably, the medium-temperature carbonization time is 2 to 4 hours, such as 2 hours, 3 hours or 4 hours, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0037] Preferably, the medium-temperature carbonized material is washed before being carbonized at high temperature.
[0038] Preferably, the washing comprises sequentially performing acid washing and water washing.
[0039] In the present invention, the material after medium-temperature carbonization is firstly acid-washed and water-washed to remove the ash (inorganic matter without electrochemical activity) and magnesium oxide template in the material, and then high-temperature carbonization is performed to achieve high capacity, high rate performance and high cycle stability.
[0040] Preferably, the heating rate of the high temperature carbonization is 1 to 5°C / min, for example, 1°C / min, 2°C / min, 3°C / min, 4°C / min or 5°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] Preferably, the carbonization atmosphere of the high-temperature carbonization is a protective atmosphere.
[0042] Preferably, the temperature of the high temperature carbonization is 1200-1400°C, for example, 1200°C, 1250°C, 1300°C, 1350°C or 1400°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0043] Preferably, the high-temperature carbonization time is 1 to 4 hours, such as 1 hour, 2 hours, 3 hours or 4 hours, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0044] As a preferred technical solution, the preparation method comprises the following steps:
[0045] mixing an acidic substance, a citrate, a starch and a solvent, and drying the mixed substance;
[0046] Low temperature carbonization at 120-220°C in an oxygen-containing atmosphere for 6-60 hours, then continue to heat up to 500-600°C at a heating rate of 1-5°C / min in an oxygen-containing atmosphere and then carbonize at medium temperature for 2-4 hours;
[0047] The medium-temperature carbonized material is sequentially acid-washed and water-washed, and then heated to 1200-1400° C. at a heating rate of 1-5° C. / min in a protective atmosphere for high-temperature carbonization for 1-4 hours to obtain the starch-based hard carbon material;
[0048] Wherein, the acidic substance includes any one of boric acid, phenylboric acid or citric acid or a combination of at least two thereof; the mass ratio of the total mass of the starch and the pickling substance citrate to the mass ratio of the solvent is 10:(1.5-4):3.
[0049] In a second aspect, the present invention provides a starch-based hard carbon negative electrode material, wherein the starch-based hard carbon negative electrode material is prepared by the preparation method described in the first aspect.
[0050] Preferably, the 002 peak interlayer spacing d of the starch-based hard carbon material is 002and 100 diffraction peak half-peak width Y 1001 / 2 The ratio is 0.07<d 002 / Y 1001 / 2 <0.12, for example, the d 002 / Y 1001 / 2 It can be 0.08, 0.09, 0.1 or 0.11, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0051] Preferably, the 002 peak interlayer spacing d of the starch-based hard carbon negative electrode material 002 Satisfies: 0.38nm<d 002 <0.42nm, for example, the d 002 It can be 0.39 nm, 0.4 nm or 0.41 nm, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0052] Preferably, the 100° diffraction peak half-peak width Y of the starch-based hard carbon negative electrode material is 1001 / 2 Satisfy: 3.57°<Y 1001 / 2 <4.42°, for example, the Y 1001 / 2 It can be 3.6°, 3.7°, 3.8°, 3.9°, 4°, 4.1°, 4.2°, 4.3° or 4.4°, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0053] Preferably, the D50 of the starch-based hard carbon negative electrode material satisfies: 5μm<D50<20μm, for example, 5.5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm or 19.5μm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0054] Preferably, the specific surface area BET of the starch-based hard carbon negative electrode material satisfies: 5m 2 / g<BET<15m 2 / g, for example 5.5m 2 / g, 6m 2 / g, 7m 2 / g, 8m 2 / g, 9m 2 / g, 10m 2 / g, 11m 2 / g, 12m 2 / g, 13m 2 / g, 14m 2 / g or 14.5m 2 / g, etc., but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0055] Preferably, the true density of the starch-based hard carbon negative electrode material in helium satisfies: 1.6 g / cm 2 ≤True density≤2.3g / cm 2 , for example 1.6 g / cm 2 , 1.65g / cm 2 , 1.7g / cm 2 , 1.75g / cm 2 , 1.8g / cm 2 , 1.85g / cm 2 , 1.9g / cm 2 , 1.95g / cm 2 , 2g / cm 2 , 2.05g / cm 2 , 2.1g / cm 2 , 2.2g / cm 2 or 2.3g / cm 2 etc., preferably 1.7 g / cm 2 ≤True density≤2.1g / cm 2 , but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0056] In a third aspect, the present invention further provides a battery, comprising the starch-based hard carbon negative electrode material as described in the second aspect.
[0057] The battery includes a lithium ion battery or a sodium ion battery.
[0058] When the starch-based hard carbon negative electrode material provided by the present invention is used in a sodium ion battery, it not only improves the compaction density of the negative electrode plate and the volume energy density of the battery cell, but also has good rate performance and cycle stability; it also ensures the rapid diffusion of solvated sodium ions inside the carbon material during the charge and discharge process, and the battery has a higher rate performance; it can also ensure that the carbon material has a high sodium storage capacity, and the battery has a high first-cycle coulomb efficiency and reversible specific capacity.
[0059] Compared with the prior art, the present invention has the following beneficial effects:
[0060] The preparation method provided by the present invention catalyzes the dehydration process of starch material through the synergistic effect of the first additive of acidic substance and the second additive of citrate; at the same time, the starch undergoes a cross-linking reaction with the first additive and the second additive during the carbonization process, the number of hydroxyl groups in the starch raw material molecules after cross-linking is reduced, and the probability of 1,6-glycosidic bond formation is reduced, thereby solving the problems of foaming, melting and the like generated in the subsequent processing of the starch raw material, reducing the process steps of starch pre-oxidation, and allowing the starch to maintain a relatively high natural morphology during the carbonization process; the second additive containing citrate will produce metal oxides during the carbonization process, which will heat the starch raw material When the treated carbon material is purified, these generated metal oxides are washed and removed, resulting in pores on the surface and inside the carbon material; thereby, the obtained hard carbon negative electrode material improves the compaction density of the negative electrode plate and the volume energy density of the battery cell. The hard carbon negative electrode material contains a large number of closed closed pores and has good rate performance and cycle stability. When the prepared negative electrode material is used in sodium ion batteries, the rapid diffusion of solvated sodium ions in the carbon material during the charge and discharge process is guaranteed, and the battery has a high rate performance; it can also ensure that the carbon material has a high sodium storage capacity, and the battery has a high first-week coulomb efficiency and reversible specific capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 This is the SEM image of the starch-based hard carbon negative electrode material provided in Example 2.
[0062] Figure 2 This is an SEM image of the starch-based hard carbon negative electrode material provided in Example 7.
[0063] Figure 3 This is the SEM image of the starch-based hard carbon negative electrode material provided in Comparative Example 1.
[0064] Figure 4 This is the SEM image of the starch-based hard carbon negative electrode material provided in Comparative Example 3.
[0065] Figure 5 This is a comparison chart of the charge and discharge cycle performance of the batteries provided in Example 2, Example 7, Comparative Example 1 and Comparative Example 3. DETAILED DESCRIPTION
[0066] The technical scheme of the present invention is further illustrated by specific examples below. Those skilled in the art should understand that the examples are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0067] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.
[0068] In the description of the embodiments of the present application, technical terms such as "first" and "second" are only used to distinguish different objects and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features.
[0069] Example 1
[0070] This embodiment provides a starch-based hard carbon negative electrode material, and the preparation method of the starch-based hard carbon negative electrode material is as follows:
[0071] 500 g corn starch, 100 g citric acid (first additive), 50 g magnesium citrate (second additive) and 150 g pure water were weighed in a ratio of 10:2:1:3. The citric acid, magnesium citrate and pure water were first mixed and stirred into a colorless transparent solution. The solution was then poured into the corn starch and mixed and stirred for 20 min. The mixed material was dried in an oven at 85°C for 12 hours.
[0072] Afterwards, the activation reaction was carried out at 150°C in an air atmosphere for 6 hours (low-temperature carbonization). The activated material was pre-carbonized at 500°C at a rate of 3°C / min for 2 hours in an argon atmosphere (medium-temperature carbonization). Then, 2 mol / L hydrochloric acid and pure water were used to wash the material in turn (acid washing and water washing). The washed material was heated to 1400°C at a rate of 3°C / min for high-temperature carbonization for 3 hours (high-temperature carbonization). After natural cooling, the starch-based hard carbon negative electrode material was obtained.
[0073] Example 2
[0074] This embodiment provides a starch-based hard carbon negative electrode material, and the preparation method of the starch-based hard carbon negative electrode material is as follows:
[0075] 500 g corn starch, 100 g citric acid (first additive), 50 g magnesium citrate (second additive) and 150 g pure water were weighed in a ratio of 10:2:1:3. The citric acid, magnesium citrate and pure water were first mixed and stirred into a colorless transparent solution. The solution was then poured into the corn starch and mixed and stirred for 20 min. The mixed material was dried in an oven at 85°C for 12 hours.
[0076] Afterwards, the activation reaction was carried out at 220°C in an air atmosphere for 60 hours (low-temperature carbonization). The activated material was pre-carbonized at 500°C at a rate of 3°C / min for 2 hours in an argon atmosphere (medium-temperature carbonization). Then, 2 mol / L hydrochloric acid and pure water were used to wash the material in turn (acid washing and water washing). After washing, the material was heated to 1400°C at a rate of 3°C / min for high-temperature carbonization for 3 hours (high-temperature carbonization). After natural cooling, the starch-based hard carbon negative electrode material was obtained.
[0077] Example 3
[0078] This embodiment provides a starch-based hard carbon negative electrode material, and the preparation method of the starch-based hard carbon negative electrode material is as follows:
[0079] 500 g corn starch, 100 g citric acid (first additive), 50 g magnesium citrate (second additive) and 150 g pure water were weighed in a ratio of 10:2:1:3. The citric acid, magnesium citrate and pure water were first mixed and stirred into a colorless transparent solution. The solution was then poured into the corn starch and mixed and stirred for 20 min. The mixed material was dried in an oven at 85°C for 12 hours.
[0080] Thereafter, in an argon atmosphere, the temperature was raised to 500°C at a rate of 3°C / min for pre-carbonization for 2 hours (medium-temperature carbonization), and then 2 mol / L hydrochloric acid and pure water were used for washing (acid washing and water washing) in sequence. After washing, the material was heated to 1400°C at a rate of 3°C / min for high-temperature carbonization for 3 hours (high-temperature carbonization), and the starch-based hard carbon negative electrode material was obtained after natural cooling.
[0081] Example 4
[0082] This embodiment provides a starch-based hard carbon negative electrode material, and the preparation method of the starch-based hard carbon negative electrode material is as follows:
[0083] 500 g corn starch, 50 g citric acid (first additive), 25 g magnesium citrate (second additive) and 150 g pure water were weighed in a ratio of 10:1:0.5:3. The citric acid, magnesium citrate and pure water were first mixed and stirred into a colorless transparent solution. The solution was then poured into the corn starch and mixed and stirred for 20 min. The mixed material was dried in an oven at 85°C for 12 hours.
[0084] Afterwards, the activation reaction was carried out at 150°C in an air atmosphere for 6 hours (low-temperature carbonization). The activated material was pre-carbonized at 500°C at a rate of 3°C / min for 2 hours in an argon atmosphere (medium-temperature carbonization). Then, 2 mol / L hydrochloric acid and pure water were used to wash the material in turn (acid washing and water washing). The washed material was heated to 1300°C at a rate of 3°C / min for high-temperature carbonization for 3 hours (high-temperature carbonization). After natural cooling, the starch-based hard carbon negative electrode material was obtained.
[0085] Example 5
[0086] This embodiment provides a starch-based hard carbon negative electrode material, and the preparation method of the starch-based hard carbon negative electrode material is as follows:
[0087] 500 g corn starch, 25 g boric acid (first additive), 12.5 g magnesium citrate (second additive) and 150 g pure water were weighed in a ratio of 10:0.5:0.25:3. Boric acid, magnesium citrate and pure water were first mixed and stirred into a colorless transparent solution. The solution was then poured into the corn starch and mixed and stirred for 20 min. The mixed material was dried in an oven at 85° C. for 12 hours.
[0088] The dried material was pre-carbonized at 500°C at 3°C / min for 2 hours (medium-temperature carbonization) under an argon atmosphere, and then washed with 2 mol / L hydrochloric acid and pure water in turn. The washed material was heated to 1300°C at 3°C / min for 3 hours (high-temperature carbonization), and the starch-based hard carbon negative electrode material was obtained after natural cooling.
[0089] Example 6
[0090] This embodiment provides a starch-based hard carbon negative electrode material, and the preparation method of the starch-based hard carbon negative electrode material is as follows:
[0091] Weigh 500g corn starch, 25g boric acid, 25g citric acid, 12.5g magnesium citrate and 150g pure water in a ratio of 10:0.5:0.5:0.25:3, first mix the boric acid, citric acid, magnesium citrate and pure water to form a colorless transparent solution, then pour the solution into the corn starch and continue mixing and stirring for 20 minutes, and dry the mixed material in an oven at 85°C for 12 hours;
[0092] The dried material was pre-carbonized at 500°C at 3°C / min for 2 hours (medium-temperature carbonization) under an argon atmosphere, and then washed with 2 mol / L hydrochloric acid and pure water in turn. The washed material was heated to 1400°C at 3°C / min for 3 hours (high-temperature carbonization), and the starch-based hard carbon negative electrode material was obtained after natural cooling.
[0093] Example 7
[0094] This embodiment provides a starch-based hard carbon negative electrode material, and the preparation method of the starch-based hard carbon negative electrode material is as follows:
[0095] Weigh 500g corn starch, 50g boric acid (first additive), 50g citric acid (first additive), 50g magnesium citrate and 150g pure water in a ratio of 10:1:1:1:3, first mix the boric acid, citric acid, magnesium citrate and pure water to form a colorless transparent solution, then pour the solution into the corn starch and continue mixing and stirring for 20 minutes. Dry the mixed materials in an oven at 85°C for 12 hours;
[0096] The dried material was pre-carbonized at 500°C at 3°C / min for 2 hours in an argon atmosphere, and then washed with 2 mol / L hydrochloric acid and pure water in turn. The washed material was carbonized at 1400°C at 3°C / min for 3 hours, and the starch-based hard carbon negative electrode material was obtained after natural cooling.
[0097] Example 8
[0098] The difference between this embodiment and embodiment 5 is that in this embodiment, the mass of boric acid is 12.5 g, and the mass of magnesium citrate is 12.5 g (the mass ratio of starch, boric acid and magnesium citrate is 10:0.25:0.25).
[0099] The rest of the preparation methods and parameters were the same as those in Example 5.
[0100] Example 9
[0101] The difference between this embodiment and embodiment 5 is that in this embodiment, the mass of boric acid is 100 g, and the mass of magnesium citrate is 100 g (the mass ratio of starch, boric acid and magnesium citrate is 10:2:2).
[0102] The rest of the preparation methods and parameters were the same as those in Example 5.
[0103] Comparative Example 1
[0104] This comparative example provides a starch-based hard carbon negative electrode material, and the preparation method of the starch-based hard carbon negative electrode material is as follows:
[0105] Take 1 kg of starch and dry it in a vacuum oven at 100°C for 24 hours. Under a nitrogen atmosphere, heat the dried corn starch to 450°C at 2°C / min for pre-carbonization for 2 hours, continue to heat it to 1400°C at 2°C / min for high-temperature carbonization for 1 hour, and obtain the starch-based hard carbon negative electrode material after natural cooling.
[0106] Comparative Example 2
[0107] The difference between this comparative example and Example 5 is that this comparative example does not contain the first additive boric acid.
[0108] The rest of the preparation methods and parameters were the same as those in Example 5.
[0109] Comparative Example 3
[0110] The difference between this comparative example and Example 1 is that this comparative example does not contain the second additive magnesium citrate.
[0111] The rest of the preparation methods and parameters were the same as those in Example 5.
[0112] Figure 1The SEM image of the starch-based hard carbon negative electrode material provided in Example 2 is shown.
[0113] Figure 2 The SEM image of the starch-based hard carbon negative electrode material provided in Example 7 is shown.
[0114] Figure 3 The SEM image of the starch-based hard carbon negative electrode material provided in Comparative Example 1 is shown.
[0115] Figure 4 The SEM image of the starch-based hard carbon negative electrode material provided in Comparative Example 3 is shown.
[0116] from Figure 1 and Figure 2 It can be seen that the starch-based hard carbon negative electrode material obtained by the preparation method provided by the present invention has no adhesion between the material particles, and the biomass morphology remains intact and is spherical.
[0117] from Figure 3 and Figure 4 It can be seen that when starch is used as the raw material for preparation without adding any additives, the starch-based hard carbon material obtained will lose the natural morphology of starch and appear as large irregular fragments; when only the second additive is added, most of the particles of the starch-based material obtained are obviously fused, and only a small number of particles maintain their natural morphology, which cannot completely solve the problems of starch fusion and adhesion.
[0118] Table 1 shows the specific surface area and D50 of the starch-based hard carbon negative electrode materials provided by Examples 1-9 and Comparative Examples 1-3.
[0119] Table 1
[0120]
[0121]
[0122] The hard carbon negative electrode materials, acetylene black conductive agent, and PVDF (polyvinylidene fluoride) prepared in Examples 1-9 and Comparative Examples 1-3 were respectively dissolved in NMP (N-methylpyrrolidone) in a mass ratio of 91.6:1.8:6.6 to form a slurry, which was then coated on aluminum foil to obtain an electrode. The electrode was then placed in a drying oven at 110°C and dried for 4 hours. Finally, button batteries were assembled in a glove box filled with argon atmosphere, and sodium metal foil was used as a counter electrode and a reference electrode.
[0123] The sodium ion batteries provided in Examples 1-9 and Comparative Examples 1-3 were subjected to performance tests under the following test conditions:
[0124] The test method for the first effect is as follows: the button half-cell is tested on the test equipment with a voltage range of 0-2V. In the first week, it is discharged to 0V at a rate of 0.1C, and then charged to 2V at a rate of 0.2C. The first effect is the ratio of the first week charging capacity to the first week discharge point capacity. The test results are shown in Table 2.
[0125] Cycle and rate test method: The batteries provided in Example 2, Example 7, Comparative Example 1 and Comparative Example 3 were charged and discharged at a rate of 3C until the capacity retention rate decayed to less than 85%, and the cycle times of different materials were compared. The test results are as follows: Figure 5 As shown, Figure 5 This is a comparison chart of the charge and discharge cycle performance of the batteries provided in Example 2, Example 7, Comparative Example 1 and Comparative Example 3.
[0126] Table 2
[0127]
[0128]
[0129] From Table 1, Table 2 and Figure 5 We can get:
[0130] From the data results of Examples 1-7, it can be seen that the starch-based hard carbon negative electrode material provided by the present invention solves the problems of foaming and melting of starch raw materials in subsequent processing processes. The obtained hard carbon negative electrode material ensures that the carbon material has a high sodium storage capacity, and the battery has a high first-week coulombic efficiency and reversible specific capacity.
[0131] From the data results of Examples 1 and 8 and 9, it can be seen that the present invention can better realize the performance of the hard carbon negative electrode material by regulating the mass ratio of the total mass of the starch, the first additive and the second additive to the solvent to be 10:(0.5-4):3; when it is not within this numerical range, the starch melting problem will be difficult to be completely solved, thereby limiting the performance of the hard carbon negative electrode material, and the reversible specific capacity, first efficiency, cycle performance and rate performance are all reduced.
[0132] From the data results of Example 1 and Comparative Examples 1-3, it can be seen that the present invention catalyzes the dehydration process of the starch material through the synergistic effect of the first additive of the acidic substance and the second additive of the citrate; at the same time, the starch undergoes a cross-linking reaction with the first additive and the second additive during the carbonization process, thereby solving the problems of foaming and melting of the starch raw material in the subsequent processing process, so that the obtained hard carbon negative electrode material has excellent specific surface area, particle size and electrochemical properties.
[0133] In summary, the preparation method provided by the present invention catalyzes the dehydration process of starch material through the synergistic effect of the first additive of acidic substance and the second additive of citrate; at the same time, the starch undergoes a cross-linking reaction with the first additive and the second additive during the carbonization process, thereby solving the problems of foaming, melting and the like generated in the subsequent processing of the starch raw material, reducing the process steps of starch pre-oxidation, and allowing the starch to maintain a relatively high natural morphology during the carbonization process; the second additive containing citrate will produce metal oxides during the carbonization process, and when the carbon material after heat treatment of the starch raw material is purified, these generated metal oxides are washed and removed, so that pores are generated on the surface and inside of the carbon material; thereby, the obtained hard carbon negative electrode material increases the compaction density of the negative electrode sheet and the volume energy density of the battery cell, and the hard carbon negative electrode material contains a large number of closed closed pores and has good rate performance and cycle stability; when the prepared negative electrode material is used in a sodium ion battery, the rapid diffusion of solvated sodium ions in the carbon material during the charge and discharge process is ensured, and the battery has a relatively high rate performance; it can also ensure that the carbon material has a relatively high sodium storage capacity, and the battery has a relatively high first-cycle coulomb efficiency and reversible specific capacity.
[0134] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a starch-based hard carbon negative electrode material, characterized in that: The preparation method comprises the following steps: Mixing the first additive, the second additive and starch, and carbonizing to obtain the starch-based hard carbon negative electrode material; Wherein, the first additive includes an acidic substance; and the second additive includes citrate.
2. The preparation method according to claim 1, characterized in that: The mixed raw materials also include a solvent; Preferably, the mass ratio of the total mass of the starch, the first additive and the second additive to the solvent is 10:(0.5-4):3; Preferably, the mass ratio of the first additive to the second additive is (1-2):1; Preferably, the acidic substance comprises any one of boric acid, phenylboric acid or citric acid or a combination of at least two thereof, preferably comprises boric acid and / or phenylboric acid; Preferably, the citrate comprises magnesium citrate; Preferably, the mixed material is dried and then carbonized; Preferably, the drying temperature is 85 to 120° C. and the drying time is 12 to 24 hours.
3. The preparation method according to claim 1 or 2, characterized in that: The carbonization includes medium temperature carbonization and high temperature carbonization; Preferably, low-temperature carbonization is performed followed by medium-temperature carbonization.
4. The preparation method according to claim 3, characterized in that: The temperature of the low-temperature carbonization is 120-220° C.; the time of the low-temperature carbonization is 6-60 hours.
5. The preparation method according to claim 3 or 4, characterized in that: The heating rate of the medium temperature carbonization is 1 to 5°C / min; Preferably, the carbonization atmosphere of the medium-temperature carbonization is a protective atmosphere; Preferably, the temperature of the medium-temperature carbonization is 500-600° C.; and the time of the medium-temperature carbonization is 2-4 hours.
6. The preparation method according to any one of claims 3 to 5, characterized in that: washing the medium-temperature carbonized material and then subjecting it to high-temperature carbonization; Preferably, the washing comprises acid washing and water washing in sequence; Preferably, the heating rate of the high temperature carbonization is 1 to 5°C / min; Preferably, the carbonization atmosphere of the high-temperature carbonization is a protective atmosphere; Preferably, the temperature of the high-temperature carbonization is 1200-1400° C., and the time of the high-temperature carbonization is 1-4 hours.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: mixing an acidic substance, a citrate, a starch and a solvent, and drying the mixed substance; Low temperature carbonization at 120-220°C in an oxygen-containing atmosphere for 6-60 hours, then continue to heat up to 500-600°C at a heating rate of 1-5°C / min in an oxygen-containing atmosphere and then carbonize at medium temperature for 2-4 hours; The medium-temperature carbonized material is sequentially acid-washed and water-washed, and then heated to 1200-1400° C. at a heating rate of 1-5° C. / min in a protective atmosphere for high-temperature carbonization for 1-4 hours to obtain the starch-based hard carbon material; Wherein, the acidic substance includes any one of boric acid, phenylboric acid or citric acid or a combination of at least two thereof; the mass ratio of the total mass of the starch and the pickling substance citrate to the mass ratio of the solvent is 10:(0.5-4):
3.
8. A starch-based hard carbon negative electrode material, characterized in that: The starch-based hard carbon negative electrode material is prepared by the preparation method according to any one of claims 1 to 7.
9. The starch-based hard carbon negative electrode material according to claim 8, characterized in that: The 002 peak interlayer spacing d of the starch-based hard carbon material 002 and 100 diffraction peak half-peak width Y 1001 / 2 The ratio is 0.07<d 002 / Y 1001 / 2 <0.12; Preferably, the 002 peak interlayer spacing d of the starch-based hard carbon negative electrode material 002 Satisfies: 0.38nm<d 002 <0.42nm; Preferably, the 100° diffraction peak half-peak width Y of the starch-based hard carbon negative electrode material is 1001 / 2 Satisfy: 3.57°<Y 1001 / 2 <4.42°; Preferably, the D50 of the starch-based hard carbon negative electrode material satisfies: 5 μm<D50<20 μm; Preferably, the specific surface area BET of the starch-based hard carbon negative electrode material satisfies: 5m 2 / g<BET<15m 2 / g; Preferably, the true density of the starch-based hard carbon negative electrode material in helium satisfies: 1.6 g / cm 2 ≤True density≤2.3g / cm 2 , preferably 1.7 g / cm 2 ≤True density≤2.1g / cm 2 .
10. A battery, characterized in that: The battery comprises the starch-based hard carbon negative electrode material as claimed in claim 8 or 9; The battery includes a lithium ion battery or a sodium ion battery.
Citation Information
Patent Citations
Preparation method for starch-based porous hard carbon negative electrode material of lithium ion battery
CN105633380A
Hard carbon material, preparation method thereof and application of hard carbon material in sodium-ion battery
CN114524425A
Preparation method of starch-based hard carbon negative electrode material, negative electrode material and sodium ion battery
CN115536002A
Hard carbon negative electrode material, preparation method thereof and secondary battery
CN115838165A
Sodium-ion battery positive electrode material and preparation method thereof
CN116154116A
Cited By
Biomass-based hard carbon negative electrode material and preparation method and application thereof
CN121307030A
Biomass-based hard carbon negative electrode material and preparation method and application thereof
CN121307030B