Hard carbon negative electrode material, preparation method thereof and sodium ion battery

Through pre-carbonization, normal temperature reduction and high-temperature carbonization of biomass carbon sources, combined with nitrogen-doped carbon coating, the gram capacity and efficiency problems of hard carbon materials in sodium-ion batteries have been solved, and the preparation and industrial production of high-performance materials have been achieved.

CN118851153APending Publication Date: 2024-10-29CHONGQING MANNSTE NEW MATERIAL TECHNOLOGY CO LTD

Patent Information

Application Number
CN202410940462.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing hard carbon materials in sodium-ion batteries have low gram capacity and low first-cycle Coulombic efficiency, resulting in limited applications. The preparation process is complex, energy consumption is high, and the cost is high.

Method used

The biomass carbon source is used through pre-carbonization, normal temperature reduction and high-temperature carbonization, combined with nitrogen-doped carbon coating, to form a highly ordered hard carbon material, which reduces surface defects and improves the embedding efficiency of sodium ions.

Benefits of technology

It significantly improves the gram capacity and first-cycle Coulombic efficiency of hard carbon materials, simplifies the process, reduces costs, is suitable for industrial production, and realizes the preparation of negative electrode materials for high-performance sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851153A_ABST
    Figure CN118851153A_ABST
Patent Text Reader

Abstract

The invention provides a hard carbon negative electrode material and a preparation method thereof, and a sodium ion battery, and relates to the technical field of negative electrode materials, the preparation method of the hard carbon negative electrode material comprises the following steps: sequentially carrying out pre-carbonization and normal temperature reduction treatment on a biomass carbon source to obtain a biomass precursor, the biomass precursor is taken and subjected to coating treatment through a nitrogen-containing carbon source, then high-temperature carbonization is performed, and the hard carbon negative electrode material is obtained; the pre-carbonization temperature is 250 DEG C to 800 DEG C, and the high-temperature carbonization temperature is 900 DEG C to 1500 DEG C. The technical problems that an existing hard carbon negative electrode material is low in gram volume and low in first-circle coulombic efficiency are solved, and the technical effects that the sodium ion battery has excellent electrochemical performance, and the gram volume and the first-circle coulombic efficiency are obviously improved are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of negative electrode materials, and in particular to a hard carbon negative electrode material and a preparation method thereof, and a sodium ion battery. Background Art

[0002] At present, electrochemical energy storage technology has attracted widespread attention due to its advantages such as low pollution, long life and high efficiency. In particular, lithium-ion batteries based on high power and energy density, as well as long life, have been widely researched and developed, and have dominated the power supply market in recent years. However, the high cost and insufficient resources of lithium have seriously affected its application in the field of energy storage. Unlike lithium salts, sodium salts are widely distributed and have abundant reserves. Sodium-ion batteries, with their low cost, superior low-temperature performance and advanced safety performance, show great development potential in large-scale energy storage applications.

[0003] Hard carbon (HC) has multiple characteristics such as high cost-effectiveness and wide sources of raw materials. It is currently the most commercially promising negative electrode material for sodium-ion batteries. However, the preparation process of hard carbon is long and the structure-activity relationship is relatively complex. Although hard carbon has good sodium storage performance, it still has the defects of low gram capacity and low first-cycle coulombic efficiency, which seriously hinders the application of hard carbon materials in sodium-ion batteries. Patent CN116675217A discloses a method using biomass as raw material, crushing the biomass raw material and pre-carbonizing it. After the pre-carbonization, the material is placed in a plasma chemical vapor deposition chamber for plasma coating treatment. After the coating is completed, high-temperature carbonization is performed to finally obtain biomass hard carbon. This patent repairs the defects on the surface of the carbon material through plasma treatment, and effectively improves the first efficiency of the hard carbon material through carbon deposition. However, the above preparation method has the disadvantages of high energy consumption, complicated process, high technical level requirements and high cost.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One of the purposes of the present invention is to provide a method for preparing a hard carbon negative electrode material, which is not only simple in process and low in cost, suitable for industrial scale-up production, but also can effectively improve the gram capacity and first-cycle coulombic efficiency of the material.

[0006] A second object of the present invention is to provide a hard carbon negative electrode material having a higher gram capacity and a higher first-cycle coulombic efficiency.

[0007] The third object of the present invention is to provide a sodium ion battery with excellent electrochemical performance, and significantly improved gram capacity and initial efficiency.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] In a first aspect, a method for preparing a hard carbon negative electrode material comprises the following steps:

[0010] The biomass carbon source is sequentially subjected to pre-carbonization and room temperature reduction treatment to obtain a biomass precursor, the biomass precursor is coated with a nitrogen-containing carbon source, and then subjected to high temperature carbonization to obtain the hard carbon negative electrode material;

[0011] The temperature of the pre-carbonization is 250°C to 800°C, and the temperature of the high-temperature carbonization is 900°C to 1500°C.

[0012] Furthermore, the biomass carbon source includes at least one of coconut shells, straws, bamboo, rice husks, corn cobs and walnut shells.

[0013] Furthermore, the pre-carbonization process further includes a step of roughly crushing the biomass carbon source;

[0014] Preferably, the average particle size after coarse crushing is 2 mm to 8 mm.

[0015] Furthermore, the pre-carbonization time is 1h to 4h;

[0016] Preferably, the protective atmosphere for pre-carbonization includes at least one of nitrogen, argon and helium.

[0017] Furthermore, the reduction treatment further includes a step of purifying the pre-carbonized product;

[0018] Preferably, the purification method includes purification by acid washing;

[0019] Preferably, the acid used in the acid solution includes at least one of hydrofluoric acid, sulfuric acid, nitric acid, hydrochloric acid and phosphoric acid;

[0020] Preferably, the concentration of the acid solution is 0.5 mol / L to 6 mol / L;

[0021] Preferably, the purification time is 1 h to 8 h.

[0022] Furthermore, the reducing agent used in the reduction treatment includes at least one of sodium bisulfite, sodium sulfite and sodium borohydride;

[0023] Preferably, the reduction treatment time is 0.5h to 4h.

[0024] Furthermore, the nitrogen-containing carbon source includes at least one of dopamine, polyvinyl pyrrolidone, polypyrrole, polyphenylpyrrole, polyacrylamide and polyaniline;

[0025] Preferably, the coating treatment comprises coating treatment by dipping;

[0026] Preferably, the concentration of the impregnation solution is 0.5wt% to 20wt%;

[0027] Preferably, the solvent of the impregnation solution includes at least one of water, ethanol, propanol, butanol, benzyl alcohol, isopropanol, dimethyl ether, tetrahydrofuran, diethylene glycol dimethyl ether and phenyl ethyl ether;

[0028] Preferably, the immersion time is 0.5 h to 24 h.

[0029] Furthermore, the heating rate of the high temperature carbonization is 2°C / min to 10°C / min;

[0030] Preferably, the high temperature carbonization time is 2h to 8h;

[0031] Preferably, the protective atmosphere for high-temperature carbonization includes at least one of nitrogen, argon and helium.

[0032] In a second aspect, a hard carbon negative electrode material is prepared by any of the preparation methods described above.

[0033] In a third aspect, a sodium ion battery is provided, wherein the negative electrode of the sodium ion battery comprises the hard carbon negative electrode material described above.

[0034] Compared with the prior art, the present invention has at least the following beneficial effects:

[0035] The preparation method of the hard carbon negative electrode material provided by the present invention can effectively improve the structural order of the hard carbon material through pre-carbonization (low-temperature carbonization) treatment; through reduction treatment at room temperature, the oxygen-containing functional groups in the material can be eliminated, which is conducive to the formation of closed-pore microstructures, thereby improving the electrochemical performance of the hard carbon material; through high-temperature carbonization, the microcrystalline structure of the hard carbon material is more ordered and becomes a graphite-like state, and sodium ions can be inserted; at the same time, the present invention uses biomass as a precursor to synthesize a hard carbon material with a relatively low specific surface area, combined with nitrogen-doped carbon coating, after high-temperature carbonization, on the one hand, it can form a coated carbon layer on the surface of the bio-based hard carbon, effectively reduce surface defects, reduce the excessive consumption of sodium ions during the formation of the SEI film, and improve the first-cycle coulomb efficiency of the hard carbon material; on the other hand, by introducing nitrogen atoms, the interplanar spacing of the carbon layer can be effectively increased, which is conducive to the embedding and extraction of sodium ions, and also provides additional storage sites for sodium ions; compared with pure carbon coating, the present invention uses nitrogen-doped carbon coating to simultaneously improve the first efficiency and specific capacity of the material. In summary, the preparation method of the hard carbon negative electrode material of the present invention is not only simple and easy to operate, low in cost, and easy to scale up for industrial production, but also, through the coordination of each step and its process parameters, effectively improves the gram capacity and first-cycle coulombic efficiency of the material, thereby achieving the purpose of preparing high-performance hard carbon negative electrode materials for sodium ion batteries.

[0036] The hard carbon negative electrode material provided by the present invention has a higher gram capacity and a higher first-cycle coulombic efficiency, and is suitable for high-performance sodium ion batteries.

[0037] The sodium ion battery provided by the present invention has excellent electrochemical performance, and the gram capacity and the initial efficiency are significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 This is an electron microscope image of the hard carbon negative electrode material provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0040] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] According to a first aspect of the present invention, there is provided a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0042] The biomass carbon source is sequentially subjected to pre-carbonization and room temperature reduction treatment to obtain a biomass precursor, the biomass precursor is coated with a nitrogen-containing carbon source, and then subjected to high temperature carbonization to obtain a hard carbon negative electrode material;

[0043] In the present invention, the pre-carbonization temperature may be 250°C to 800°C, and typical but non-limiting temperatures include 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, and 800°C.

[0044] In the present invention, the temperature of high temperature carbonization may be 900°C to 1500°C, and typical but non-limiting temperatures are, for example, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, and 1500°C.

[0045] The preparation method of the hard carbon negative electrode material provided by the present invention can effectively improve the structural order of the hard carbon material through pre-carbonization (low-temperature carbonization) treatment; through reduction treatment at room temperature, the oxygen-containing functional groups in the material can be eliminated, which is conducive to the formation of closed-pore microstructures, thereby improving the electrochemical performance of the hard carbon material; through high-temperature carbonization, the microcrystalline structure of the hard carbon material is more ordered and becomes a graphite-like state, and sodium ions can be inserted; at the same time, the present invention uses biomass as a precursor to synthesize a hard carbon material with a relatively low specific surface area, combined with nitrogen-doped carbon coating, after high-temperature carbonization, on the one hand, it can form a coated carbon layer on the surface of the bio-based hard carbon, effectively reduce surface defects, reduce the excessive consumption of sodium ions during the formation of the SEI film, and improve the first-cycle coulomb efficiency of the hard carbon material; on the other hand, by introducing nitrogen atoms, the interplanar spacing of the carbon layer can be effectively increased, which is conducive to the embedding and extraction of sodium ions, and also provides additional storage sites for sodium ions; compared with pure carbon coating, the present invention uses nitrogen-doped carbon coating to simultaneously improve the first efficiency and specific capacity of the material.

[0046] In summary, the preparation method of the hard carbon negative electrode material of the present invention is not only simple and easy to operate, low in cost, and easy to scale up for industrial production, but also, through the coordination of each step and its process parameters, effectively improves the gram capacity and first-cycle coulombic efficiency of the material, thereby achieving the purpose of preparing high-performance hard carbon negative electrode materials for sodium ion batteries.

[0047] In a preferred embodiment, the biomass carbon source includes but is not limited to at least one of coconut shells, straw, bamboo, rice husks, corn cobs and walnut shells.

[0048] In the present invention, the step of coarsely crushing the biomass carbon source is also included before pre-carbonization. The average particle size of the biomass carbon source after coarse crushing can be 2mm to 8mm. Its typical but non-limiting average particle size is, for example, 2mm, 3mm, 4mm, 5mm, 6mm, 7mm, and 8mm, which is more conducive to improving the effect of subsequent pre-carbonization.

[0049] In a preferred embodiment, the pre-carbonization time can be 1h to 4h, and typical but non-limiting times are, for example, 1h, 2h, 3h, and 4h. At the specific pre-carbonization temperature and time, the carbon source can be fully pre-carbonized, which is more conducive to improving the structural order of the hard carbon material.

[0050] In the present invention, the protective atmosphere used in the pre-carbonization process includes but is not limited to at least one of nitrogen, argon and helium.

[0051] In a preferred embodiment, the step of purifying the pre-carbonized product is further included before the reduction treatment, and the purification method includes but is not limited to purification by acid washing.

[0052] In the present invention, the pre-carbonized material is immersed in an acid solution for 1 to 8 hours, and then washed with deionized water until it becomes neutral, thereby achieving material purification and effectively reducing the ash content in the biomass material.

[0053] In a preferred embodiment, the acid used in the acid solution includes but is not limited to at least one of hydrofluoric acid, sulfuric acid, nitric acid, hydrochloric acid and phosphoric acid; the concentration of the acid solution can be 0.5mol / L to 6mol / L, and its typical but non-limiting concentrations are, for example, 0.5mol / L, 1mol / L, 1.5mol / L, 2mol / L, 2.5mol / L, 3mol / L, 3.5mol / L, 4mol / L, 4.5mol / L, 5mol / L, 5.5mol / L, and 6mol / L, which is more conducive to fully reducing the ash content in the biomass material.

[0054] In a preferred embodiment, the reducing agent used in the reduction treatment includes but is not limited to at least one of sodium bisulfite, sodium sulfite and sodium borohydride; the time of the reduction treatment can be 0.5h to 4h, and its typical but non-limiting time is, for example, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, and 4h.

[0055] The reduction is carried out at room temperature. The specific reducing agent and the reduction time in the present invention are more conducive to fully eliminating the oxygen-containing functional groups in the material and are more conducive to improving the formation effect of the closed-cell microstructure.

[0056] In a preferred embodiment, the nitrogen-containing carbon source includes, but is not limited to, at least one of dopamine, polyvinyl pyrrolidone, polypyrrole, polyphenylpyrrole, polyacrylamide and polyaniline.

[0057] In the present invention, the coating treatment method includes but is not limited to coating treatment by impregnation, and the purpose of simultaneously improving the primary efficiency and specific capacity of the material is achieved by the method of nitrogen-doped impregnation carbon coating.

[0058] Firstly, a nitrogen-containing carbon source is dissolved in a solvent to obtain an impregnation solution; then, the biomass precursor is immersed in the impregnation solution for 0.5h to 24h, and then dried, thereby achieving impregnation coating.

[0059] In a preferred embodiment, the concentration of the impregnating solution can be 0.5wt% to 20wt%, and its typical but non-limiting concentration is, for example, 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt%, which is more conducive to improving the effect of impregnation coating, and is more conducive to simultaneously improving the first efficiency and specific capacity of the material.

[0060] In a preferred embodiment, the solvent of the impregnation solution includes but is not limited to at least one of water, ethanol, propanol, butanol, benzyl alcohol, isopropanol, dimethyl ether, tetrahydrofuran, diethylene glycol dimethyl ether and phenyl ethyl ether.

[0061] In a preferred embodiment, the conditions for high temperature carbonization are as follows:

[0062] Raise the temperature to 900°C to 1500°C at a rate of 2°C / min to 10°C / min, and keep the temperature for 2h to 8h;

[0063] The heating rate may be, for example, 2°C / min, 4°C / min, 6°C / min, 8°C / min, 10°C / min, but is not limited thereto; the insulation time may be, for example, 2h, 4h, 6h, 8h, but is not limited thereto.

[0064] In the present invention, the protective atmosphere during the high temperature carbonization process includes but is not limited to at least one of nitrogen, argon and helium.

[0065] In a preferred embodiment, after the high-temperature carbonization, the product is further subjected to ball milling and screening to obtain a finished hard carbon negative electrode material.

[0066] In the present invention, the ball milling speed can be 100r / min to 600r / min, and its typical but non-limiting speed is 100r / min, 200r / min, 300r / min, 400r / min, 500r / min, 600r / min; the ball milling time can be 0.5h to 6h, and its typical but non-limiting time is 0.5h, 1h, 2h, 3h, 4h, 5h, 6h.

[0067] A typical preparation method of a hard carbon negative electrode material comprises the following steps:

[0068] (1) Rough crushing and pre-carbonization: The first carbon source (i.e., biomass carbon source) is roughly crushed, and then placed in a carbonization furnace at 250° C. to 800° C. for low-temperature carbonization (i.e., pre-carbonization) to obtain a first precursor;

[0069] (2) Purification and reduction: The first precursor is immersed in an acid solution, then washed with deionized water until neutral, then an appropriate amount of a reducing agent is added to react at room temperature, and finally washed and dried to obtain a second precursor;

[0070] (3) Impregnation coating: dissolving the second carbon source (i.e., nitrogen-containing carbon source) in a solvent to obtain an impregnation solution, immersing the second precursor in the impregnation solution, and then drying to obtain a third precursor;

[0071] (4) High temperature carbonization, ball milling and screening: The third precursor is placed at 900°C to 1500°C for high temperature carbonization, and then ball milled and screened to obtain a hard carbon negative electrode material.

[0072] According to a second aspect of the present invention, there is provided a hard carbon negative electrode material prepared by any of the preparation methods described above.

[0073] The hard carbon negative electrode material provided by the present invention has a higher gram capacity and a higher first-cycle coulombic efficiency, and is suitable for high-performance sodium ion batteries.

[0074] According to a third aspect of the present invention, a sodium ion battery is provided, wherein the negative electrode of the sodium ion battery comprises the hard carbon negative electrode material described above.

[0075] The sodium ion battery provided by the present invention has excellent electrochemical performance, and the gram capacity and the initial efficiency are significantly improved.

[0076] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0077] Example 1

[0078] A method for preparing a hard carbon negative electrode material comprises the following steps:

[0079] (1) Coarse crushing and pre-carbonization: The coconut shell was coarsely crushed to an average particle size of 3 mm, and then pre-carbonized at low temperature in a carbonization furnace at 500° C. to obtain a coconut shell-based precursor 1;

[0080] (2) Purification and reduction: immerse the coconut shell-based precursor 1 in a 1 mol / L hydrochloric acid solution, stir and soak for 2 h, filter and then wash with deionized water until neutral, then add sodium bisulfite (2 wt %) to react for 1 h, and finally wash and dry to obtain the coconut shell-based precursor 2;

[0081] (3) Impregnation coating: dopamine was dissolved in deionized water to obtain a 5 wt% impregnation solution, and the coconut shell-based precursor 2 was immersed in the impregnation solution for 2 h, and then dried to obtain the coconut shell-based precursor 3;

[0082] (4) High temperature carbonization, ball milling and sieving: The coconut shell-based precursor 3 was placed at 1200°C for high temperature carbonization, wherein the heating rate was 2°C / min, the holding time was 5h, the carbonized material was ball milled for 1h, the ball milling speed was 200r / min, and finally passed through a 325 mesh sieve to obtain a hard carbon negative electrode material, the electron microscope image of which is shown in Figure 1 , it can be seen that the hard carbon material has uniform particle size distribution and excellent performance.

[0083] Example 2

[0084] A method for preparing a hard carbon negative electrode material comprises the following steps:

[0085] (1) Coarse crushing and pre-carbonization: The bamboo is coarsely crushed to an average particle size of 2 mm, and then pre-carbonized at low temperature in a carbonization furnace at 400° C. to obtain a bamboo-based precursor 1;

[0086] (2) Purification and reduction: The bamboo-based precursor 1 was immersed in a 4 mol / L hydrochloric acid solution, stirred and immersed for 2 h, filtered, and then washed with deionized water until neutral, and then sodium borohydride (2 wt %) was added to react for 1.5 h, and finally washed and dried to obtain the bamboo-based precursor 2;

[0087] (3) Impregnation coating: polyvinyl pyrrolidone was dissolved in deionized water to obtain a 7 wt % impregnation solution, and the bamboo-based precursor 2 was immersed in the impregnation solution for 2 h, and then dried to obtain the bamboo-based precursor 3;

[0088] (4) High-temperature carbonization, ball milling and screening: The bamboo-based precursor 3 was placed at 1300°C for high-temperature carbonization, with a heating rate of 10°C / min and a holding time of 5 h. The carbonized material was ball milled for 1.5 h at a ball milling speed of 300 r / min, and finally passed through a 325-mesh sieve to obtain a hard carbon negative electrode material.

[0089] Example 3

[0090] A method for preparing a hard carbon negative electrode material comprises the following steps:

[0091] (1) Coarse crushing and pre-carbonization: The bamboo is coarsely crushed to an average particle size of 2 mm, and then pre-carbonized at a low temperature in a carbonization furnace at 600° C. to obtain a bamboo-based precursor 1;

[0092] (2) Purification and reduction: The bamboo-based precursor 1 was immersed in a 4 mol / L nitric acid solution, stirred and immersed for 2 h, filtered, and then washed with deionized water until neutral, then sodium borohydride (3 wt %) was added to react for 2 h, and finally washed and dried to obtain the bamboo-based precursor 2;

[0093] (3) Impregnation coating: polypyrrole is dissolved in ethanol to obtain a 3 wt % impregnation solution, the bamboo-based precursor 2 is immersed in the impregnation solution for 2 h, and then dried to obtain the bamboo-based precursor 3;

[0094] (4) High-temperature carbonization, ball milling and screening: The bamboo-based precursor 3 was placed at 1400°C for high-temperature carbonization, with a heating rate of 5°C / min and a holding time of 5 h. The carbonized material was ball milled for 1.5 h at a ball milling speed of 500 r / min, and finally passed through a 325-mesh sieve to obtain a hard carbon negative electrode material.

[0095] Example 4

[0096] A method for preparing a hard carbon negative electrode material comprises the following steps:

[0097] (1) Coarse crushing and pre-carbonization: The walnut shells were coarsely crushed to an average particle size of 4 mm, and then pre-carbonized at a low temperature in a carbonization furnace at 800° C. to obtain a walnut shell-based precursor 1;

[0098] (2) Purification and reduction: immerse the walnut shell-based precursor 1 in a 4 mol / L sulfuric acid solution, stir and soak for 2 h, filter and then wash with deionized water until neutral, then add sodium sulfite (5 wt %) to react for 0.5 h, and finally wash and dry to obtain a walnut shell-based precursor 2;

[0099] (3) Impregnation coating: polyacrylamide and polyvinyl pyrrolidone are dissolved in deionized water to obtain a 5 wt % impregnation solution, and the walnut shell-based precursor 2 is immersed in the impregnation solution for 2 h, and then dried to obtain a walnut shell-based precursor 3;

[0100] (4) High-temperature carbonization, ball milling and screening: The walnut shell-based precursor 3 was placed at 1400°C for high-temperature carbonization, with a heating rate of 5°C / min and a holding time of 5 h. The carbonized material was ball milled for 2 h at a ball milling speed of 500 r / min, and finally passed through a 325-mesh sieve to obtain a hard carbon negative electrode material.

[0101] Example 5

[0102] A method for preparing a hard carbon negative electrode material comprises the following steps:

[0103] (1) Coarse crushing and pre-carbonization: The walnut shells were coarsely crushed to an average particle size of 4 mm, and then pre-carbonized at low temperature in a carbonization furnace at 300° C. to obtain a walnut shell-based precursor 1;

[0104] (2) Purification and reduction: walnut shell-based precursor 1 was immersed in a 3 mol / L nitric acid solution, stirred and immersed for 2 h, filtered, and then washed with deionized water until neutral, then sodium borohydride (3 wt %) was added to react for 1.5 h, and finally washed and dried to obtain walnut shell-based precursor 2;

[0105] (3) Impregnation coating: polyphenylpyrrole and polyvinylpyrrolidone are dissolved in tetrahydrofuran to obtain an 11 wt % impregnation solution, and the walnut shell-based precursor 2 is immersed in the impregnation solution for 2 h, and then dried to obtain a walnut shell-based precursor 3;

[0106] (4) High-temperature carbonization, ball milling and screening: The walnut shell-based precursor 3 was placed at 1400°C for high-temperature carbonization, wherein the heating rate was 8°C / min and the holding time was 5h. The carbonized material was ball milled for 1h at a ball milling speed of 200r / min and finally passed through a 325-mesh sieve to obtain a hard carbon negative electrode material.

[0107] Example 6

[0108] A method for preparing a hard carbon negative electrode material comprises the following steps:

[0109] (1) Coarse crushing and pre-carbonization: The bamboo is coarsely crushed to an average particle size of 5 mm, and then pre-carbonized at a low temperature in a carbonization furnace at 600° C. to obtain a bamboo-based precursor 1;

[0110] (2) Purification and reduction: The bamboo-based precursor 1 was immersed in a 2 mol / L sulfuric acid solution, stirred and immersed for 2 h, filtered, and then washed with deionized water until neutral, then sodium bisulfite (3 wt %) was added to react for 2 h, and finally washed and dried to obtain the bamboo-based precursor 2;

[0111] (3) Impregnation coating: polyacrylamide and polyvinyl pyrrolidone are dissolved in deionized water to obtain a 5 wt % impregnation solution, and the bamboo-based precursor 2 is immersed in the impregnation solution for 2 h, and then dried to obtain the bamboo-based precursor 3;

[0112] (4) High-temperature carbonization, ball milling and screening: The bamboo-based precursor 3 was placed at 1300°C for high-temperature carbonization, with a heating rate of 10°C / min and a holding time of 5 h. The carbonized material was ball milled for 3 h at a ball milling speed of 200 r / min, and finally passed through a 325-mesh sieve to obtain a hard carbon negative electrode material.

[0113] Comparative Example 1

[0114] A method for preparing a hard carbon negative electrode material comprises the following steps:

[0115] (1) Coarse crushing and pre-carbonization: The coconut shell was coarsely crushed to an average particle size of 3 mm, and then pre-carbonized at low temperature in a carbonization furnace at 500° C. to obtain a coconut shell-based precursor 1;

[0116] (2) Purification: immerse the coconut shell-based precursor 1 in a 1 mol / L hydrochloric acid solution, stir and soak for 2 h, filter, wash with deionized water until neutral, and dry to obtain the coconut shell-based precursor 2;

[0117] (3) High-temperature carbonization, ball milling and screening: The coconut shell-based precursor 2 was placed at 1200°C for high-temperature carbonization, with a heating rate of 2°C / min and a holding time of 5h. The carbonized material was ball milled for 1h at a ball milling speed of 200r / min, and finally passed through a 325-mesh sieve to obtain a hard carbon negative electrode material.

[0118] Comparative Example 2

[0119] A method for preparing a hard carbon negative electrode material comprises the following steps:

[0120] (1) Coarse crushing and pre-carbonization: The coconut shell was coarsely crushed to an average particle size of 3 mm, and then low-temperature carbonized in a carbonization furnace at 500° C. to obtain a coconut shell-based precursor 1;

[0121] (2) Purification and reduction: immerse the coconut shell-based precursor 1 in a 1 mol / L hydrochloric acid solution, stir and soak for 2 h, filter and then wash with deionized water until neutral, then add sodium bisulfite (0.5 wt %) and react for 0.5 h, finally wash and dry to obtain the coconut shell-based precursor 2;

[0122] (3) High-temperature carbonization, ball milling and screening: The coconut shell-based precursor 2 was placed at 1200°C for high-temperature carbonization, with a heating rate of 2°C / min and a holding time of 5h. The carbonized material was ball milled for 1h at a ball milling speed of 200r / min, and finally passed through a 325-mesh sieve to obtain a hard carbon negative electrode material.

[0123] Comparative Example 3

[0124] A method for preparing a hard carbon negative electrode material comprises the following steps:

[0125] (1) Coarse crushing and pre-carbonization: The coconut shell was coarsely crushed to an average particle size of 3 mm, and then low-temperature carbonized in a carbonization furnace at 500° C. to obtain a coconut shell-based precursor 1;

[0126] (2) Purification and reduction: immerse the coconut shell-based precursor 1 in a 1 mol / L hydrochloric acid solution, stir and soak for 2 h, filter and then wash with deionized water until neutral, then add sodium bisulfite (0.5 wt %) and react for 0.5 h, finally wash and dry to obtain the coconut shell-based precursor 2;

[0127] (3) Impregnation coating: Glucose was dissolved in deionized water to obtain a 5 wt% impregnation solution, and the coconut shell-based precursor 2 was immersed in the impregnation solution for 2 h, and then dried to obtain the coconut shell-based precursor 3;

[0128] (4) High-temperature carbonization, ball milling and screening: The coconut shell-based precursor 3 was placed at 1200°C for high-temperature carbonization, with a heating rate of 2°C / min and a holding time of 5 h. The carbonized material was ball milled for 1 h at a ball milling speed of 200 r / min, and finally passed through a 325-mesh sieve to obtain a hard carbon negative electrode material.

[0129] Comparative Example 4

[0130] A method for preparing a hard carbon negative electrode material comprises the following steps:

[0131] (1) Coarse crushing and pre-carbonization: The bamboo is coarsely crushed to an average particle size of 2 mm, and then pre-carbonized at low temperature in a carbonization furnace at 400° C. to obtain a bamboo-based precursor 1;

[0132] (2) Purification: The bamboo-based precursor 1 was immersed in a 4 mol / L hydrochloric acid solution, stirred and immersed for 2 h, filtered, washed with deionized water until neutral, and dried to obtain the bamboo-based precursor 2;

[0133] (3) High-temperature carbonization, ball milling and screening: The bamboo-based precursor 2 was placed at 1300°C for high-temperature carbonization, with a heating rate of 10°C / min and a holding time of 5 h. The carbonized material was ball milled for 1.5 h at a ball milling speed of 300 r / min, and finally passed through a 325-mesh sieve to obtain a hard carbon negative electrode material.

[0134] Test example

[0135] The electrochemical performance of the hard carbon negative electrode materials obtained in the examples and comparative examples was tested, and the results are shown in Table 1.

[0136] Specifically, the hard carbon negative electrode material obtained in the embodiment or comparative example is used as an active ingredient, mixed with CMC, SBR and conductive agent Super P in a mass ratio of 95.5:1.5:2:1, and solvent water is added to prepare a negative electrode slurry. The negative electrode slurry is evenly coated on the copper foil current collector with a scraper, and the coating thickness is 250±1μm. After vacuum drying, a 12mm diameter circular electrode sheet is prepared; a sodium sheet is used as a counter electrode, glass fiber is used as a diaphragm, and the electrolyte is 1M NaPF6 in DIGLYME=100Vol%; the half-cell is assembled in a glove box, and after the assembly is completed, it is tested at a current density of 0.1C, and the test range is 0.001V~2.0V.

[0137] Table 1

[0138]

[0139] It can be seen that the hard carbon negative electrode material prepared by the preparation method of the present invention, as a sodium ion battery made of negative electrode active material, has excellent comprehensive electrochemical properties, and the specific capacity and first efficiency are significantly improved.

[0140] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a hard carbon negative electrode material, It is characterized in that The following steps are involved: The biomass carbon source is sequentially subjected to pre-carbonization and room temperature reduction treatment to obtain a biomass precursor, the biomass precursor is coated with a nitrogen-containing carbon source, and then subjected to high temperature carbonization to obtain the hard carbon negative electrode material; The temperature of the pre-carbonization is 250°C to 800°C, and the temperature of the high-temperature carbonization is 900°C to 1500°C.

2. The preparation method according to claim 1, It is characterized in that The biomass carbon source includes at least one of coconut shells, straws, bamboo, rice husks, corn cobs and walnut shells.

3. The preparation method according to claim 1, It is characterized in that The pre-carbonization step also includes a step of roughly breaking the biomass carbon source; Preferably, the average particle size after coarse crushing is 2 mm to 8 mm.

4. The preparation method according to any one of claims 1 to 3, It is characterized in that The pre-carbonization time is 1h to 4h; Preferably, the protective atmosphere for pre-carbonization includes at least one of nitrogen, argon and helium.

5. The preparation method according to any one of claims 1 to 3, It is characterized in that The reduction treatment also includes a step of purifying the pre-carbonized product; Preferably, the purification method includes purification by acid washing; Preferably, the acid used in the acid solution includes at least one of hydrofluoric acid, sulfuric acid, nitric acid, hydrochloric acid and phosphoric acid; Preferably, the concentration of the acid solution is 0.5 mol / L to 6 mol / L; Preferably, the purification time is 1 h to 8 h.

6. The preparation method according to claim 5, It is characterized in that The reducing agent used in the reduction treatment includes at least one of sodium bisulfite, sodium sulfite and sodium borohydride; Preferably, the reduction treatment time is 0.5h to 4h.

7. The preparation method according to any one of claims 1 to 3, It is characterized in that The nitrogen-containing carbon source includes at least one of dopamine, polyvinyl pyrrolidone, polypyrrole, polyphenylpyrrole, polyacrylamide and polyaniline; Preferably, the coating treatment comprises coating treatment by dipping; Preferably, the concentration of the impregnation solution is 0.5wt% to 20wt%; Preferably, the solvent of the impregnation solution includes at least one of water, ethanol, propanol, butanol, benzyl alcohol, isopropanol, dimethyl ether, tetrahydrofuran, diethylene glycol dimethyl ether and phenyl ethyl ether; Preferably, the immersion time is 0.5 h to 24 h.

8. The preparation method according to claim 1, It is characterized in that The heating rate of the high temperature carbonization is 2°C / min to 10°C / min; Preferably, the high temperature carbonization time is 2h to 8h; Preferably, the protective atmosphere for high-temperature carbonization includes at least one of nitrogen, argon and helium.

9. A hard carbon negative electrode material prepared by the preparation method according to any one of claims 1 to 8.

10. A sodium ion battery, It is characterized in that The negative electrode of the sodium ion battery comprises the hard carbon negative electrode material according to claim 9.

Citation Information

Patent Citations

  • Battery hard carbon negative electrode material and preparation method thereof

    CN116281939A

  • Preparation method of hard carbon negative electrode material for sodium ion battery

    CN117602609A

  • Preparation method and application of soft and hard carbon composite negative electrode material

    CN117865124A

  • Composite hard carbon material, preparation method therefor, and use thereof

    WO2024109849A1

Cited By

  • Hard carbon material and preparation method thereof, negative electrode, battery and electric equipment

    CN120149404A

  • Negative electrode material and preparation method thereof, negative electrode plate and battery

    CN120717446A