New energy battery negative electrode material hard carbon precursor processing method
By removing the green and yellow bamboo material from the bamboo knots and carbonizing it in an oxygen-free reactor, combined with washing and drying, the problem of high cost and unstable quality of the bamboo material precursor carbon material is solved, and cost reduction and Quality improvement.
Patent Information
- Application Number
- CN202410941057.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-29
AI Technical Summary
In the existing technology, carbon materials, which are precursors for bamboo wood processing, have high costs, high ash content, large specificity ratios, and quality stability problems, making them unable to effectively replace imported precursor materials.
Fresh bamboo is used to remove the bamboo green and bamboo knots, and is carbonized through an oxygen-free reactor pyrolysis process. It is combined with air cooling, crushing, washing and drying to control the ash content and ratio, reduce costs and improve quality stability.
It effectively reduces costs, controls ash content and specificity, improves the quality of negative hard carbon precursor materials for new energy batteries, and solves the problems of high ash content, small specific volume, and large specificity.
Smart Images

Figure CN118851154A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of negative electrode hard carbon materials, and specifically relates to a method for processing a hard carbon precursor of a negative electrode material for a new energy battery. Background Art
[0002] With the rapid development of the new energy battery industry, the demand for negative electrode hard carbon materials is also increasing. Precursors are a very important part of the hard carbon production process. At present, precursor materials are heavily dependent on imports, and the raw material anthracite is a non-renewable resource. It is a general trend to replace anthracite with bamboo and wood as raw materials. Bamboo materials are not only renewable resources, but also have low costs.
[0003] Now some enterprises are conducting research on processing methods for precursor carbon materials using bamboo and wood materials, but there are still some problems: for example, the carbon materials obtained by aerobic carbonization process cost about twice as much, and the ash content is too high and the specific surface area is too large. The carbon materials obtained by external heating converter anaerobic process cannot solve the sealing problem of the inlet and outlet, which will inevitably lead to higher ash content and larger specific surface area, which is only slightly better than the aerobic carbonization process. In addition, there is the problem of stability of the quality of the precursor materials. For the same batch of materials, the sampling and test results vary greatly, and the quality is still quite different from that of imported precursor materials. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a method for processing a hard carbon precursor of anode materials for new energy batteries.
[0005] The technical solution adopted to solve the above technical problems is: a method for processing a hard carbon precursor of anode material of a new energy battery, comprising the following specific steps:
[0006] S1. Bamboo material processing: fresh bamboo materials are selected and cut and broken, and bamboo green and bamboo nodes of the bamboo materials are removed to reduce non-cellulose components in the bamboo materials and obtain bamboo yellow;
[0007] S2, heating treatment: the bamboo yellow obtained in S1 is filled and sealed in an oxygen-free reactor, and then the oxygen-free reactor is hoisted into the furnace body of the carbonization furnace for heating treatment. After the bamboo yellow is pyrolyzed to 250°C-270°C to produce combustible volatile gas, the heat source of the carbonization furnace is turned off, and the pyrolysis is continued by using the spontaneous combustion of the volatile gas;
[0008] S3, cooling treatment: after the volatile gas is naturally extinguished, the oxygen-free reactor is lifted out of the furnace body and cooled naturally. After the oxygen-free reactor is naturally cooled to less than 100° C., the primary charcoal obtained through the above processing is lifted out of the oxygen-free reactor and cooled by air, so that the temperature of the primary charcoal is cooled to room temperature;
[0009] S4, crushing treatment: crushing the primary charcoal after cooling in S3, so that the primary charcoal is crushed into charcoal blocks;
[0010] S5, soaking treatment: put the broken carbon blocks after S4 into a pure water pool, wash until there is no black water, soak for 2h-8h and then take them out;
[0011] S6, drying treatment: drying the broken carbon blocks after the water washing and soaking in S5 using a drying device, and after the broken carbon blocks are dried, a finished carbon is obtained.
[0012] Furthermore, the species of the fresh bamboo in S1 is Phyllostachys pubescens, and the age of the fresh bamboo is 3 to 6 years.
[0013] Furthermore, the temperature of the carbonization furnace in S2 is controlled between 500°C and 800°C.
[0014] Furthermore, the diameter of the carbon blocks in S4 is controlled between 30 meshes and 60 meshes.
[0015] Furthermore, the temperature of the drying equipment in S6 is controlled between 80°C and 120°C.
[0016] The beneficial effects of the present invention are as follows:
[0017] The present invention adopts bamboo green and bamboo yellow with high ash content removed from bamboo nodes as raw materials, and uses an anaerobic reactor pyrolysis process for carbonization, which can not only effectively reduce costs, but also further ensure the control of ash content because of the small carbon loss in this process. At the same time, this process can also control the specific surface area not to be too large while ensuring a high specific volume. In the anaerobic carbonization stage, this process first treats the specific volume, specific surface area and ash content to meet the standards, and then soaks in pure water to reduce the volatile matter, thereby solving the technical problems of high ash content, small specific volume, large specific surface area and high volatile matter in the negative electrode hard carbon precursor material of new energy batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0020] Embodiment 1
[0021] like Figure 1 As shown, a method for processing a hard carbon precursor of a new energy battery negative electrode material in this embodiment includes the following specific steps:
[0022] S1. Bamboo material processing: Select fresh bamboo materials of 3-6 years old and species of Phyllostachys pubescens, cut and break them, and remove the green bamboo and bamboo nodes of the bamboo materials to reduce the non-cellulose components in the bamboo materials, and obtain bamboo yellow;
[0023] S2, heating treatment: the bamboo yellow obtained in S1 is filled and sealed in an oxygen-free reactor, and then the oxygen-free reactor is hoisted into the furnace body of the carbonization furnace for heating treatment, and the temperature of the carbonization furnace is controlled between 500°C and 800°C. After the bamboo yellow is pyrolyzed to 250°C-270°C to produce combustible volatile gas, the heat source of the carbonization furnace is turned off, and the pyrolysis is continued by using the spontaneous combustion of the volatile gas;
[0024] S3, cooling treatment: after the volatile gas is naturally extinguished, the oxygen-free reactor is lifted out of the furnace body and cooled naturally. After the oxygen-free reactor is naturally cooled to less than 100° C., the primary charcoal obtained through the above processing is lifted out of the oxygen-free reactor and cooled by air, so that the temperature of the primary charcoal is cooled to room temperature;
[0025] S4, crushing treatment: crushing the primary charcoal after cooling in S3, so that the primary charcoal is crushed into charcoal blocks with a diameter between 30 meshes and 60 meshes;
[0026] S5, soaking treatment: put the broken carbon blocks after S4 into a pure water pool, wash until there is no black water, soak for 8 hours and then take them out;
[0027] S6, drying treatment: drying the broken carbon blocks after water washing and soaking in S5 using a drying device, and controlling the temperature of the drying device at 80°C-120°C. After the broken carbon blocks are dried, finished carbon is obtained.
[0028] Embodiment 2
[0029] The difference between this embodiment and the first embodiment is that a method for processing a hard carbon precursor of a negative electrode material for a new energy battery comprises the following specific steps:
[0030] S1. Bamboo material processing: Select fresh bamboo materials of 3-6 years old and species of Phyllostachys pubescens, cut and break them, and remove the green bamboo and bamboo nodes of the bamboo materials to reduce the non-cellulose components in the bamboo materials, and obtain bamboo yellow;
[0031] S2, heating treatment: the bamboo yellow obtained in S1 is filled and sealed in an oxygen-free reactor, and then the oxygen-free reactor is hoisted into the furnace body of the carbonization furnace for heating treatment, and the temperature of the carbonization furnace is controlled between 500°C and 800°C. After the bamboo yellow is pyrolyzed to 250°C-270°C to produce combustible volatile gas, the heat source of the carbonization furnace is turned off, and the pyrolysis is continued by using the spontaneous combustion of the volatile gas;
[0032] S3, cooling treatment: after the volatile gas is naturally extinguished, the oxygen-free reactor is lifted out of the furnace body and cooled naturally. After the oxygen-free reactor is naturally cooled to less than 100° C., the primary charcoal obtained through the above processing is lifted out of the oxygen-free reactor and cooled by air, so that the temperature of the primary charcoal is cooled to room temperature;
[0033] S4, crushing treatment: crushing the primary charcoal after cooling in S3, so that the primary charcoal is crushed into charcoal blocks with a diameter between 30 meshes and 60 meshes;
[0034] S5, soaking treatment: put the broken carbon blocks after S4 into a pure water pool, wash until there is no black water, soak for 2 hours and then take them out;
[0035] S6, drying treatment: drying the broken carbon blocks after water washing and soaking in S5 using a drying device, and controlling the temperature of the drying device at 80°C-120°C. After the broken carbon blocks are dried, finished carbon is obtained.
[0036] Embodiment 3
[0037] The difference between this embodiment and the first embodiment is that a method for processing a hard carbon precursor of a negative electrode material for a new energy battery comprises the following specific steps:
[0038] S1. Bamboo material processing: Select fresh bamboo materials of 3-6 years old and species of Phyllostachys pubescens, cut and break them, and remove the green bamboo and bamboo nodes of the bamboo materials to reduce the non-cellulose components in the bamboo materials, and obtain bamboo yellow;
[0039] S2, heating treatment: the bamboo yellow obtained in S1 is filled and sealed in an oxygen-free reactor, and then the oxygen-free reactor is hoisted into the furnace body of the carbonization furnace for heating treatment, and the temperature of the carbonization furnace is controlled between 500°C and 800°C. After the bamboo yellow is pyrolyzed to 250°C-270°C to produce combustible volatile gas, the heat source of the carbonization furnace is turned off, and the pyrolysis is continued by using the spontaneous combustion of the volatile gas;
[0040] S3, cooling treatment: after the volatile gas is naturally extinguished, the oxygen-free reactor is lifted out of the furnace body and cooled naturally. After the oxygen-free reactor is naturally cooled to less than 100° C., the primary charcoal obtained through the above processing is lifted out of the oxygen-free reactor and cooled by air, so that the temperature of the primary charcoal is cooled to room temperature;
[0041] S4, crushing treatment: crushing the primary charcoal after cooling in S3, so that the primary charcoal is crushed into charcoal blocks with a diameter between 30 meshes and 60 meshes, and the finished charcoal is obtained.
[0042] The ash content and volatile content of the finished carbon obtained by the above-mentioned Example 1, Example 2 and Example 3 were tested, and the results are shown in the following table:
[0043] Example Ash content (%) Volatile matter (%) Embodiment 1 0.95% 13% Embodiment 2 1.1% 16% Embodiment 3 1.9% 20%
[0044] In summary, by washing the crushed carbon blocks with pure water and soaking them for several hours, the ash content and volatile matter of the finished carbon can be effectively reduced.
[0045] The ash and volatile content of the finished charcoal obtained in the first embodiment and the common bamboo yellow charcoal and bamboo chip charcoal in the prior art were tested, and the results are shown in the following table:
[0046] sample Ash content (%) Volatile matter (%) Embodiment 1 0.95% 13% Bamboo charcoal 0.85% 16% Bamboo charcoal 1.71% 18%
[0047] In summary, the present invention uses bamboo green and bamboo yellow with high ash content removed from bamboo nodes as raw materials, and uses an anaerobic reactor pyrolysis process for carbonization, which can ensure the control of ash content. At the same time, in the anaerobic carbonization stage, the specific volume, specific surface area and ash content are first treated to meet the standards, and then immersed in pure water to reduce the volatile matter, so that the volatile matter of the hard carbon precursor material of the negative electrode of the new energy battery can be effectively reduced. The present invention can ensure the control of ash content on the basis of low process cost.
[0048] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention.
Claims
1. A method for processing a hard carbon precursor of a new energy battery negative electrode material, characterized in that: The specific steps include: S1. Bamboo material processing: fresh bamboo materials are selected and cut and broken, and bamboo green and bamboo nodes of the bamboo materials are removed to reduce non-cellulose components in the bamboo materials and obtain bamboo yellow; S2, heating treatment: the bamboo yellow obtained in S1 is filled and sealed in an oxygen-free reactor, and then the oxygen-free reactor is hoisted into the furnace body of the carbonization furnace for heating treatment. After the bamboo yellow is pyrolyzed to 250°C-270°C to produce combustible volatile gas, the heat source of the carbonization furnace is turned off, and the pyrolysis is continued by using the spontaneous combustion of the volatile gas; S3, cooling treatment: after the volatile gas is naturally extinguished, the oxygen-free reactor is lifted out of the furnace body and cooled naturally. After the oxygen-free reactor is naturally cooled to less than 100° C., the primary charcoal obtained through the above processing is lifted out of the oxygen-free reactor and cooled by air, so that the temperature of the primary charcoal is cooled to room temperature; S4, crushing treatment: crushing the primary charcoal after cooling in S3, so that the primary charcoal is crushed into charcoal blocks; S5, soaking treatment: put the broken carbon blocks after S4 into a pure water pool, wash until there is no black water, soak for 2h-8h and then take them out; S6, drying treatment: drying the broken carbon blocks after the water washing and soaking in S5 using a drying device, and after the broken carbon blocks are dried, a finished carbon is obtained.
2. The method for processing a hard carbon precursor of a new energy battery negative electrode material according to claim 1, characterized in that: The species of the fresh bamboo in S1 is Phyllostachys pubescens, and the age of the fresh bamboo is 3 to 6 years.
3. The method for processing a hard carbon precursor of a new energy battery negative electrode material according to claim 1, characterized in that: The temperature of the carbonization furnace in S2 is controlled between 500°C and 800°C.
4. The method for processing a hard carbon precursor of a new energy battery negative electrode material according to claim 1, characterized in that: The diameter of the carbon blocks in S4 is controlled between 30 meshes and 60 meshes.
5. The method for processing a hard carbon precursor of a new energy battery negative electrode material according to claim 1, characterized in that: The temperature of the drying equipment in S6 is controlled between 80°C and 120°C.
Citation Information
Patent Citations
Production method of carbon carving product based on waste bamboo material
CN104401163A
Preparation method of bamboo hard charcoal material and bamboo hard charcoal material
CN117602610A
Preparation and modification method of sodium ion battery negative electrode material for bamboo wood
CN117819527A
Method of making bamboo charcoal adsorbents
US20060281633A1