High-capacity hard carbon negative electrode material, preparation method thereof and sodium ion battery

By polymerizing and solidifying and high-temperature carbonizing sugar compounds and pore-forming agents, hard carbon anode materials with high capacity are prepared, which solves the problem of insufficient capacity of hard carbon anode materials and improves the energy density and cycle life of sodium-ion batteries.

CN118851155APending Publication Date: 2024-10-29四川佰思格新材料科技有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411107102.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing hard carbon anode materials have low capacity, which limits the energy density and cycle life of sodium-ion batteries.

Method used

By subjecting a mixture of sugar compounds and pore-forming agents to polymerization and solidification, low-temperature pretreatment, and high-temperature carbonization, a high-capacity hard carbon anode material with a microcrystalline spacing suitable for sodium ion deintercalation is prepared.

Benefits of technology

It significantly increases the capacity of hard carbon anode materials, improves its kinetic properties and Coulomb efficiency, and reduces material consumption and preparation costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851155A_ABST
    Figure CN118851155A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sodium-ion batteries, in particular to a high-capacity hard carbon negative electrode material and a preparation method thereof and a sodium-ion battery. The preparation method comprises the following steps: preparing a mixture of a carbohydrate compound and a pore-forming agent, dispersing the mixture in a solvent, heating to 140-200 DEG C for reaction, washing and drying a cured product to obtain the high-capacity hard carbon negative electrode material. And heating the dried and cured product to 280-400 DEG C in an inert gas atmosphere, carrying out low-temperature pretreatment, cleaning the pretreated product with acid or alkali, heating to 1000-1600 DEG C in the inert gas atmosphere, and carrying out high-temperature carbonization to obtain the high-capacity hard carbon negative electrode material. According to the preparation method, the carbohydrate compound and the pore-forming agent are adopted as raw materials, and then polymerization curing, low-temperature pretreatment, acid and alkali washing and high-temperature carbonization treatment processes are combined, so that the prepared hard carbon negative electrode material has a microstructure suitable for sodion deintercalation, and the capacity of the hard carbon negative electrode material is favorably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a high-capacity hard carbon negative electrode material and a preparation method thereof, and a sodium ion battery. Background Art

[0002] Sodium-ion batteries have attracted much attention due to their low cost and high safety performance, and are expected to replace lithium-ion batteries. As one of the main components of sodium-ion batteries, the negative electrode material has an important impact on the energy density and cycle life of sodium-ion batteries. Sodium and lithium are in the same main group and have similar physical and chemical properties. However, since the ionic radius of sodium ions is larger than that of lithium ions, the graphite negative electrode traditionally used in lithium-ion batteries is not suitable for sodium-ion batteries. Therefore, it is necessary to develop negative electrode materials suitable for sodium-ion batteries.

[0003] Among the many sodium storage negative electrode materials, hard carbon materials have become the most promising sodium ion battery negative electrode materials due to their large interlayer space; however, the existing hard carbon materials are limited by the sodium ion adsorption-embedding-vacancy filling mechanism, and their capacity is often not high; therefore, how to improve the capacity of hard carbon negative electrode materials is a technical problem that needs to be solved urgently. Summary of the invention

[0004] In order to solve the problem of low capacity of hard carbon negative electrode materials in the prior art, the present invention provides a method for preparing a high-capacity hard carbon negative electrode material. The preparation method polymerizes and solidifies a mixture of a sugar compound and a pore-forming agent, and then performs a carbonization treatment, so that the prepared hard carbon negative electrode material has a microcrystalline interlayer spacing suitable for sodium ion deintercalation, thereby helping to improve the capacity of the hard carbon negative electrode material and solving the problem of low capacity of hard carbon negative electrode materials in the prior art.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] A method for preparing a high-capacity hard carbon negative electrode material comprises the following steps:

[0007] S1: preparing a mixture of a carbohydrate compound and a pore-forming agent, and dispersing the mixture in a solvent to obtain a dispersion;

[0008] S2: heating the dispersion to 140-200° C. to react and obtain a solidified product; washing and drying the solidified product to obtain a dry solidified product;

[0009] S3: In an inert gas atmosphere, heating the dried solidified product to 280-400° C. for low-temperature pretreatment to obtain a pretreated product;

[0010] S4: washing the pretreated product with an acid or an alkali until it is neutral, and drying to obtain a dried pretreated product;

[0011] S5: In an inert gas atmosphere, the dried pre-treated product is heated to 1000-1600° C. for high-temperature carbonization to obtain a high-capacity hard carbon negative electrode material.

[0012] Optionally, the carbohydrate compound is selected from at least one of glucose polymers and fructo-oligosaccharides.

[0013] Optionally, the preparation method of the glucose polymer is as follows: glucose is mixed with sorbitol and citric acid, and a polycondensation reaction is carried out at 120-180°C.

[0014] Optionally, the mass ratio of the glucose, the sorbitol and the citric acid is (80-95):(5-15):(0.5-5).

[0015] Optionally, the oligofructose is prepared by hydrolyzing sucrose.

[0016] Optionally, the pore-forming agent is selected from at least one of sodium chloride, ammonium chloride, calcium chloride, magnesium chloride, potassium chloride and sodium carbonate.

[0017] Optionally, in step S1, the mass ratio of the carbohydrate compound to the pore-forming agent is (90-99): (10-1).

[0018] Optionally, the solvent in step S1 includes water and ethanol.

[0019] Another object of the present invention is to provide a high-capacity hard carbon negative electrode material, which is prepared by the preparation method of the high-capacity hard carbon negative electrode material as described above.

[0020] Another object of the present invention is to provide a sodium ion battery comprising the high-capacity hard carbon negative electrode material as described above.

[0021] The beneficial effects of the present invention are:

[0022] The method for preparing a high-capacity hard carbon negative electrode material provided by the present invention adopts sugar compounds and pore-forming agents as raw materials, and then combines polymerization curing, low-temperature pretreatment, acid washing and alkali washing, and high-temperature carbonization treatment processes, so that the prepared hard carbon negative electrode material has a microstructure suitable for sodium ion deintercalation, thereby helping to improve the capacity of the hard carbon negative electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0024] Figure 1 is a SEM image of the hard carbon negative electrode material prepared in Example 1 of the present invention;

[0025] Figure 2 This is a graph showing the electrochemical performance test results of the hard carbon negative electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] The present invention is now further described in detail. The embodiments described below are exemplary and intended to be used to explain the present invention, but cannot be understood as limiting the present invention. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0027] In order to solve the problem of low capacity of hard carbon negative electrode materials in the prior art, the present invention provides a method for preparing a high-capacity hard carbon negative electrode material, the preparation method comprising the following steps:

[0028] S1: preparing a mixture of a carbohydrate compound and a pore-forming agent, and dispersing the mixture in a solvent to obtain a dispersion;

[0029] S2: heating the dispersion to 140-200°C for reaction, preferably placing the dispersion in a water bath at 140-200°C for 12-18h at normal pressure or in a closed pressure vessel, so that the sugar compound is polymerized and solidified to obtain a solidified product, and the material is taken out; washing and drying the solidified product to obtain a dry solidified product; preferably, the material is washed with deionized water and ethanol for multiple times, and the material is dried by drying / filter pressing-drying / centrifugation-drying and the like, and the drying atmosphere can be vacuum, nitrogen or argon;

[0030] S3: In an inert gas atmosphere, the dried solidified product is heated to 280-400° C. for low-temperature pretreatment, preferably for 5-10 hours, to obtain a pretreated product;

[0031] S4: washing the pretreated product with an acid or an alkali, washing it to neutrality, and drying it to obtain a dried pretreated product;

[0032] S5: In an inert gas atmosphere, the dried pre-treated product is heated to 1000-1600° C., preferably 1200-1600° C. for high-temperature carbonization, preferably for 1-6 hours, to obtain a high-capacity hard carbon negative electrode material.

[0033] In the preparation method, after the sugar compound and the pore-forming agent are mixed, the sugar compound is polymerized again through a polymerization curing reaction, and the pore-forming agent is coated during the polymerization to obtain a cured product with the pore-forming agent coated inside; the cured product is subjected to a low-temperature pretreatment process, and then the pore-forming agent is removed by acid washing or alkali washing and water washing, so that certain micropores and ultramicropores can be formed on the pretreated product; and then the prepared hard carbon negative electrode material is subjected to a subsequent high-temperature carbonization treatment process, so that the prepared hard carbon negative electrode material has a microcrystalline layer spacing suitable for sodium ion deintercalation, and the micropores and ultramicropores are closed to form closed pores, thereby being able to improve the capacity of the hard carbon negative electrode material.

[0034] The method for preparing a high-capacity hard carbon negative electrode material provided by the present invention adopts sugar compounds and pore-forming agents as raw materials, and then combines polymerization curing, low-temperature pretreatment, acid washing and alkali washing, and high-temperature carbonization treatment processes, so that the prepared hard carbon negative electrode material has a microstructure suitable for sodium ion deintercalation, thereby helping to improve the capacity of the hard carbon negative electrode material.

[0035] The sugar compound in the present invention can be a commonly used biomass carbon source such as glucose, fructose, sucrose, etc.; the sugar compound in the present invention is preferably selected from at least one of glucose polymers and oligofructose; compared with directly using glucose, sucrose, etc. as a carbon source, using glucose polymers or oligofructose as a carbon source can help promote the aggregation and growth of hard carbon particles, reduce the specific surface area of ​​the material, improve the kinetic properties of the hard carbon material, and make the prepared hard carbon negative electrode material have higher coulombic efficiency and rate performance; in addition, it also helps to improve the hard carbon yield. Compared with directly using glucose, sucrose, etc. as a carbon source, the hard carbon yield is increased from 12-22% to 50-60%, which greatly reduces material consumption, thereby reducing the cost of hard carbon preparation.

[0036] The glucose polymer of the present invention can be prepared by a method known in the prior art; specifically, the preferred preparation method of the glucose polymer of the present invention is as follows: glucose is mixed with sorbitol and citric acid, and a polycondensation reaction is carried out at 120-180°C.

[0037] In order to take into account both the electrochemical performance and the economy of the hard carbon negative electrode material, the present invention preferably has a mass ratio of glucose, sorbitol, and citric acid of (80-95): (5-15): (0.5-5).

[0038] Similarly, the oligofructose in the present invention can be prepared by methods known in the prior art. Specifically, the present invention preferably prepares the oligofructose from sucrose by hydrolysis, and further preferably prepares the oligofructose as follows: dissolving sucrose in hydrochloric acid or sodium hydroxide solution, hydrolyzing in a water bath at 60-90° C. or under heating conditions, and neutralizing the liquid with sodium carbonate or hydrochloric acid as a neutralizer to prepare an intermediate - a mixed liquid of oligofructose and sodium chloride; in the mixed liquid prepared by the preparation method, sodium chloride can be used as a pore-forming agent in subsequent reactions, and therefore, the oligofructose in the product does not need to be purified, which helps to reduce the number of operating steps.

[0039] In order to ensure the capacity of the hard carbon negative electrode material, the preferred pore-forming agent of the present invention is selected from at least one of sodium chloride, ammonium chloride, calcium chloride, magnesium chloride, potassium chloride and sodium carbonate.

[0040] In order to take into account both the electrochemical performance and the economy of the hard carbon negative electrode material, the mass ratio of the sugar compound to the pore-forming agent in step S1 of the present invention is preferably (90-99): (10-1).

[0041] In the present invention, the solvent in step S1 preferably includes water and ethanol, and further preferably, the mass ratio of the mixture to water and ethanol in step S1 is (35-45): (35-65): (1-10).

[0042] Another object of the present invention is to provide a high-capacity hard carbon negative electrode material, which is prepared by the preparation method of the high-capacity hard carbon negative electrode material as described above.

[0043] The high-capacity hard carbon negative electrode material provided by the present invention adopts sugar compounds and pore-forming agents as raw materials, and then combines polymerization curing, low-temperature pretreatment, acid washing and alkali washing, and high-temperature carbonization treatment processes, so that the prepared hard carbon negative electrode material has a microstructure suitable for sodium ion deintercalation, thereby helping to improve the capacity of the hard carbon negative electrode material.

[0044] Another object of the present invention is to provide a sodium ion battery, which comprises the high-capacity hard carbon negative electrode material as described above.

[0045] The sodium ion battery provided by the present invention adopts a high-capacity hard carbon negative electrode material. By using sugar compounds and pore-forming agents as raw materials, and combining polymerization curing, low-temperature pretreatment, acid washing and alkali washing, and high-temperature carbonization treatment processes, the prepared hard carbon negative electrode material has a microstructure suitable for sodium ion deintercalation, thereby helping to improve the capacity of the sodium ion battery.

[0046] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below.

[0047] Example 1

[0048] This embodiment provides a method for preparing a high-capacity hard carbon negative electrode material, comprising the following steps:

[0049] S1: Mix glucose, sorbitol and citric acid in a mass ratio 85:12.5:2.5 Mix and react at 130° C. for 0.5 h to obtain a glucose polymer; mix the glucose polymer with sodium chloride in a mass ratio of 98.5:1.5 to obtain a mixture; disperse the mixture in a mixed solution of water and ethanol by stirring, wherein the mass ratio of the mixture to water and ethanol is 40:50:5 to obtain a dispersion;

[0050] S2: placing the dispersion in a sealed pressure vessel, heating it in a water bath at 170° C. for 15 h to obtain a solidified product, taking out the material, washing the material with deionized water and ethanol for multiple times, and drying the material by drying / filter pressing-drying / centrifugation-drying process, with nitrogen as the drying atmosphere, to obtain a dry solidified product;

[0051] S3: In a nitrogen atmosphere, the dried solidified product is heated to 340° C. for low-temperature pretreatment for 7 h to obtain a pretreated product;

[0052] S4: The pre-treated product is washed with NaOH and deionized water until the pH of the filtrate is 7-10, and the sample is placed in an oven at 80° C. to dry overnight to obtain a dry pre-treated product;

[0053] S5: In a nitrogen atmosphere, the dried pretreated product was heated to 1250°C for high temperature carbonization for 3 h to obtain a high capacity hard carbon negative electrode material.

[0054] The SEM image of the high capacity hard carbon negative electrode material is shown in Figure 1 The electrochemical performance test results are shown in Figure 2 shown.

[0055] Example 2

[0056] This embodiment provides a method for preparing a high-capacity hard carbon negative electrode material, comprising the following steps:

[0057] S1: Glucose, sorbitol and citric acid are mixed in a mass ratio of 90:5:5, and reacted at 145°C for 1 hour to obtain a glucose polymer; glucose polymer is mixed with ammonium chloride in a mass ratio of 99:1 to obtain a mixture; the mixture is dispersed in a mixed solution of water and ethanol by stirring, and the mass ratio of the mixture to water and ethanol is 45:35:10 to obtain a dispersion;

[0058] S2: placing the dispersion in a sealed pressure vessel, heating it in a water bath at 140° C. for 18 h to obtain a solidified product, taking out the material, washing the material with deionized water and ethanol for multiple times, and drying the material by drying / filter pressing-drying / centrifugation-drying process, with nitrogen as the drying atmosphere, to obtain a dry solidified product;

[0059] S3: In a nitrogen atmosphere, the dried solidified product is heated to 280° C. for low-temperature pretreatment for 10 h to obtain a pretreated product;

[0060] S4: The pre-treated product was washed with NaOH and deionized water until the pH of the filtrate was 7-10, and the sample was placed in a 65°C oven to dry overnight to obtain a dry pre-treated product;

[0061] S5: In a nitrogen atmosphere, the dried pretreated product is heated to 1200° C. and carbonized for 6 h to obtain a high-capacity hard carbon negative electrode material.

[0062] Example 3

[0063] This embodiment provides a method for preparing a high-capacity hard carbon negative electrode material, comprising the following steps:

[0064] S1: Glucose, sorbitol and citric acid were mixed in a mass ratio of 84.5:15:0.5, and reacted at 160° C. for 2 hours to obtain a glucose polymer; glucose polymer was mixed with potassium chloride in a mass ratio of 98:2 to obtain a mixture; the mixture was dispersed in a mixed solution of water and ethanol by stirring, and the mass ratio of the mixture to water and ethanol was 35:65:1 to obtain a dispersion;

[0065] S2: placing the dispersion in a sealed pressure vessel, heating it in a water bath at 200° C. for 12 h to obtain a solidified product, taking out the material, washing the material with deionized water and ethanol for multiple times, and drying the material by drying / filter pressing-drying / centrifugation-drying process, with nitrogen as the drying atmosphere, to obtain a dry solidified product;

[0066] S3: In a nitrogen atmosphere, the dried solidified product is heated to 400° C. for low-temperature pretreatment for 5 h to obtain a pretreated product;

[0067] S4: The pre-treated product was washed with NaOH and deionized water until the pH of the filtrate was 7-10, and the sample was placed in an oven at 105° C. for overnight drying to obtain a dry pre-treated product;

[0068] S5: In a nitrogen atmosphere, the dried pretreated product is heated to 1600° C. for high-temperature carbonization for 1 h to obtain a high-capacity hard carbon negative electrode material.

[0069] Example 4

[0070] This embodiment provides a method for preparing a high-capacity hard carbon negative electrode material, comprising the following steps:

[0071] S1: dissolving sucrose in a sodium hydroxide solution with a concentration of 0.01 mol / L, the mass ratio of sucrose to sodium hydroxide solution being 1:9, hydrolyzing in a water bath at 80°C for 2 hours, neutralizing the liquid with hydrochloric acid as a neutralizer, and preparing a mixed liquid of oligofructose and sodium chloride; dispersing the mixed liquid in ethanol by stirring, the mass ratio of the mixed liquid to ethanol being 90:5, and obtaining a dispersion;

[0072] S2: placing the dispersion in a sealed pressure vessel, heating it in a water bath at 180° C. for 14 h to obtain a solidified product, taking out the material, washing the material with deionized water and ethanol for multiple times, and drying the material by drying / filter pressing-drying / centrifugation-drying process, with nitrogen as the drying atmosphere, to obtain a dry solidified product;

[0073] S3: In a nitrogen atmosphere, the dried solidified product is heated to 350° C. for low-temperature pretreatment for 6 hours to obtain a pretreated product;

[0074] S4: The pre-treated product is washed with NaOH and deionized water until the pH of the filtrate is 7-10, and the sample is placed in an oven at 80° C. to dry overnight to obtain a dry pre-treated product;

[0075] S5: In a nitrogen atmosphere, the dried pretreated product is heated to 1500° C. and carbonized for 2 h to obtain a high-capacity hard carbon negative electrode material.

[0076] Comparative Example 1

[0077] This comparative example provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0078] S1: mixing glucose and sodium chloride in a mass ratio of 98.5:1.5 to obtain a mixture;

[0079] S2: Under a nitrogen atmosphere, the mixture was heated to 340°C for low temperature pretreatment for 7 hours to obtain a pretreated product;

[0080] S3: The pre-treated product was washed with NaOH and deionized water until the pH of the filtrate was 7-10, and the sample was placed in an oven at 80°C for overnight drying to obtain a dry pre-treated product;

[0081] S4: In a nitrogen atmosphere, the dried pretreated product was heated to 1250° C. for high-temperature carbonization for 3 h to obtain a hard carbon negative electrode material.

[0082] Comparative Example 2

[0083] This comparative example provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0084] S1: Glucose and sodium chloride are mixed in a mass ratio of 98.5:1.5 to obtain a mixture; the mixture is dispersed in a mixed solution of water and ethanol by stirring, and the mass ratio of the mixture to water and ethanol is 40:50:5 to obtain a dispersion;

[0085] S2: placing the dispersion in a sealed pressure vessel, heating it in a water bath at 170° C. for 15 h to obtain a solidified product, taking out the material, washing the material with deionized water and ethanol for multiple times, and drying the material by drying / filter pressing-drying / centrifugation-drying process, with nitrogen as the drying atmosphere, to obtain a dry solidified product;

[0086] S3: In a nitrogen atmosphere, the dried solidified product is heated to 340° C. for low-temperature pretreatment for 7 h to obtain a pretreated product;

[0087] S4: The pre-treated product is washed with NaOH and deionized water until the pH of the filtrate is 7-10, and the sample is placed in an oven at 80° C. to dry overnight to obtain a dry pre-treated product;

[0088] S5: In a nitrogen atmosphere, the dried pretreated product was heated to 1250° C. for high temperature carbonization for 3 h to obtain a hard carbon negative electrode material.

[0089] Comparative Example 3

[0090] This comparative example provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0091] S1: Glucose, sorbitol and citric acid were mixed in a mass ratio of 85:12.5:2.5, and reacted at 130°C for 0.5h to obtain glucose polymer;

[0092] S2: placing the glucose polymer in a sealed pressure vessel, heating it in a water bath at 170° C. for 15 h to obtain a solidified product, taking out the material, washing the material with deionized water and ethanol for multiple times, drying the material by a drying / filter pressing-drying / centrifugation-drying process, with nitrogen as the drying atmosphere, to obtain a dry solidified product; mixing the dry solidified product with sodium chloride in a mass ratio of 98.5:1.5 to obtain a mixture; dispersing the mixture in a mixed solution of water and ethanol by stirring, with the mass ratio of the mixture to water and ethanol being 40:50:5, to obtain a dispersion;

[0093] S2: placing the dispersion in a sealed pressure vessel, heating it in a water bath at 170° C. for 15 h to obtain a solidified product, taking out the material, washing the material with deionized water and ethanol for multiple times, and drying the material by drying / filter pressing-drying / centrifugation-drying process, with nitrogen as the drying atmosphere, to obtain a dry solidified product;

[0094] S3: In a nitrogen atmosphere, the dried solidified product is heated to 340° C. for low-temperature pretreatment for 7 h to obtain a pretreated product;

[0095] S4: The pre-treated product was washed with NaOH and deionized water until the pH of the filtrate was 7, and the sample was placed in an oven at 80° C. for overnight drying to obtain a dry pre-treated product;

[0096] S5: In a nitrogen atmosphere, the dried pretreated product was heated to 1250° C. for high temperature carbonization for 3 h to obtain a hard carbon negative electrode material.

[0097] Comparative Example 4

[0098] This comparative example provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0099] S1: Glucose, sorbitol and citric acid are mixed in a mass ratio of 85:12.5:2.5, and reacted at 130° C. for 0.5 h to obtain a glucose polymer; glucose polymer is mixed with sodium chloride in a mass ratio of 98.5:1.5 to obtain a mixture; the mixture is dispersed in a mixed solution of water and ethanol by stirring, and the mass ratio of the mixture to water and ethanol is 40:50:5 to obtain a dispersion;

[0100] S2: placing the dispersion in a sealed pressure vessel, heating it in a water bath at 170° C. for 15 h to obtain a solidified product, taking out the material, washing the material with deionized water and ethanol for multiple times, and drying the material by drying / filter pressing-drying / centrifugation-drying process, with nitrogen as the drying atmosphere, to obtain a dry solidified product;

[0101] S3: The dried solidified product was washed with NaOH and deionized water until the pH of the filtrate was 7, and the sample was placed in an oven at 80°C for overnight drying to obtain a dried pretreated product;

[0102] S4: In a nitrogen atmosphere, the dried pretreated product was heated to 1250° C. for high-temperature carbonization for 3 h to obtain a hard carbon negative electrode material.

[0103] Comparative Example 5

[0104] This comparative example provides a method for preparing a hard carbon negative electrode material, comprising the following steps:

[0105] S1: Glucose, sorbitol and citric acid are mixed in a mass ratio of 85:12.5:2.5, and reacted at 130° C. for 0.5 h to obtain a glucose polymer; glucose polymer is mixed with sodium chloride in a mass ratio of 98.5:1.5 to obtain a mixture; the mixture is dispersed in a mixed solution of water and ethanol by stirring, and the mass ratio of the mixture to water and ethanol is 40:50:5 to obtain a dispersion;

[0106] S2: placing the dispersion in a sealed pressure vessel, heating it in a water bath at 170° C. for 15 h to obtain a solidified product, taking out the material, washing the material with deionized water and ethanol for multiple times, and drying the material by drying / filter pressing-drying / centrifugation-drying process, with nitrogen as the drying atmosphere, to obtain a dry solidified product;

[0107] S3: In a nitrogen atmosphere, the dried solidified product is heated to 340° C. for low-temperature pretreatment for 7 h to obtain a pretreated product;

[0108] S4: In a nitrogen atmosphere, the pretreated product was heated to 1250° C. for high-temperature carbonization for 3 h to obtain a hard carbon negative electrode material.

[0109] The negative electrode materials prepared in the above embodiments and comparative examples are used to prepare sodium ion batteries, and the preparation method is as follows:

[0110] The performance of the negative electrode materials prepared in the above embodiments and comparative examples was evaluated by button cells. The modulation ratio of the electrode slurry was active material: conductive agent SP: binder CMC: dispersant SBR = 92:3.0:1.5:3.5. Appropriate amounts of ethanol and water were added to prepare the slurry. The coating thickness was 200 μm. After drying and tableting, the electrode sheets were made. Metal sodium was used as the counter electrode, 1 mol / L NaPF6 DEC / EC (1:1) solution was used as the electrolyte, and glass fiber filter paper membrane GF / C was used as the diaphragm to assemble into 2032 button cells.

[0111] The electrochemical performance of the sodium ion batteries prepared in the above embodiments and comparative examples was tested, and the test method was as follows:

[0112] The half-battery was left at rest for 120 min; discharged at a constant current of 0.1C to 0.005V; left at rest for 20 min; discharged at a constant current of 0.05C to 0.005V; left at rest for 20 min; discharged at a constant current of 0.02C to 0.005V; left at rest for 20 min; charged at a constant current of 0.1C to 2.0V; the discharge specific capacity and charge specific capacity data were counted, and the first coulombic efficiency was calculated.

[0113] The test results are shown in Table 1:

[0114] Table 1

[0115]

[0116]

[0117] The difference between Comparative Example 1 and Example 1 is that glucose is directly used as the carbon source to prepare the hard carbon negative electrode material, and polymerization curing is not performed during the preparation process. Because the pore-forming agent particles are relatively large, dry-mixing the pore-forming agent will lead to insufficient mixing of the pores and the materials, which is not conducive to subsequent pore formation, resulting in a lower capacity of the prepared hard carbon negative electrode material than that of Example 1.

[0118] The difference between Comparative Example 2 and Example 1 is that glucose is directly used as the carbon source to prepare the hard carbon negative electrode material without condensation. The raw material does not cover the pore-forming agent sufficiently, which is not conducive to subsequent pore formation. Although the capacity of the prepared hard carbon negative electrode material is improved compared with Comparative Example 1, it is still significantly lower than that of Example 1.

[0119] The difference between Comparative Example 3 and Example 1 is that during the preparation process, the glucose polymer is first polymerized and solidified, and then the polymerization and solidification product is mixed with the pore-forming agent. Because the pore-forming agent cannot be coated, the pore-forming agent and the solidified material cannot be evenly mixed, and pores cannot be effectively formed, resulting in a lower capacity of the prepared hard carbon negative electrode material than that of Example 1.

[0120] The difference between Comparative Example 4 and Example 1 is that the dried solidified product is not subjected to low-temperature pretreatment during the preparation process. Since the volatile components in the material are not fully volatilized in the low-temperature section, the residual material affects the microstructure of the material, resulting in a decrease in the capacity of the prepared hard carbon negative electrode material compared to Example 1.

[0121] The difference between Comparative Example 5 and Example 1 is that the low-temperature pretreatment product is not alkaline washed during the preparation process. Since the residual pore-forming agent in the material affects the hard carbon capacity and the first effect, the capacity of the prepared hard carbon negative electrode material is lower than that of Example 1.

[0122] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a high-capacity hard carbon negative electrode material, It is characterized in that The steps include: S1: preparing a mixture of a carbohydrate compound and a pore-forming agent, and dispersing the mixture in a solvent to obtain a dispersion; S2: heating the dispersion to 140-200° C. to react and obtain a solidified product; After washing and drying the solidified product, a dry solidified product is obtained; S3: In an inert gas atmosphere, heating the dried solidified product to 280-400° C. for low-temperature pretreatment to obtain a pretreated product; S4: washing the pretreated product with an acid or an alkali until it is neutral, and drying to obtain a dried pretreated product; S5: In an inert gas atmosphere, the dried pre-treated product is heated to 1000-1600° C. for high-temperature carbonization to obtain a high-capacity hard carbon negative electrode material.

2. The method for preparing the high-capacity hard carbon negative electrode material according to claim 1, It is characterized in that The carbohydrate compound is selected from at least one of glucose polymers and oligofructose.

3. The method for preparing the high-capacity hard carbon negative electrode material according to claim 2, It is characterized in that The preparation method of the glucose polymer is as follows: glucose is mixed with sorbitol and citric acid, and a polycondensation reaction is carried out at 120-180°C.

4. The method for preparing the high-capacity hard carbon negative electrode material according to claim 3, It is characterized in that The mass ratio of the glucose, the sorbitol and the citric acid is (80-95):(5-15):(0.5-5).

5. The method for preparing the high-capacity hard carbon negative electrode material according to claim 2, It is characterized in that The oligofructose is prepared by hydrolyzing sucrose.

6. A method for preparing a high-capacity hard carbon negative electrode material according to any one of claims 1 to 5, It is characterized in that The pore-forming agent is selected from at least one of sodium chloride, ammonium chloride, calcium chloride, magnesium chloride, potassium chloride and sodium carbonate.

7. A method for preparing a high-capacity hard carbon negative electrode material according to any one of claims 1 to 5, It is characterized in that The mass ratio of the sugar compound to the pore-forming agent in step S1 is (90-99): (10-1).

8. A method for preparing a high-capacity hard carbon negative electrode material according to any one of claims 1 to 5, It is characterized in that The solvent in step S1 includes water and ethanol.

9. A high capacity hard carbon negative electrode material, It is characterized in that The method is used to prepare the high-capacity hard carbon negative electrode material according to any one of claims 1 to 8.

10. A sodium ion battery, It is characterized in that Comprising the high capacity hard carbon negative electrode material as claimed in claim 9.

Citation Information

Patent Citations

  • Hard carbon negative electrode material and preparation method and application thereof

    CN115571867A

  • Preparation method of pore-structure-adjustable polycyclic aromatic hydrocarbon hard carbon and application of pore-structure-adjustable polycyclic aromatic hydrocarbon hard carbon to negative electrode of sodium-ion battery

    CN117361490A

  • Phosphorus-carbon negative electrode plate, preparation method thereof and lithium ion battery

    CN117810372A

  • Hard carbon material and preparation method and application thereof

    CN118016847A

  • Preparation method of sodium ion battery hard carbon negative electrode material and hard carbon negative electrode material

    CN118343740A