Preparation method of high-activity electrode material for all-vanadium redox flow battery
By forming a dense conductive network and a three-dimensional network structure in porous carbon-based materials, the problems of poor electrochemical activity and low mechanical strength of porous carbon-based materials under high electrical density are solved, and the electrochemistry of all-vanadium redox flow battery electrode materials is improved. performance and mechanical strength, extending service life.
Patent Information
- Application Number
- CN202410866180.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-01
AI Technical Summary
As electrode materials for all-vanadium redox flow batteries, porous carbon-based materials have good chemical stability, but have poor electrochemical activity under high electrical density and low mechanical strength. They are prone to structural damage or deformation, affecting battery performance and Stability; Nano-bismuth powder is easily brittle at low temperatures, reducing the electrochemical performance and service life of electrode materials.
Polystyrene is synthesized in situ on the surface of nanoparticles and then mixed with carbon precursors to form a dense conductive network to improve electrochemical performance; pre-oxidation and high-temperature carbonization refine the pore size and enhance mechanical strength; the bismuth source is intercalated into the graphene oxide layer space to avoid accumulation and enlarging the layer spacing, and improve the vanadium ion contact area and charge transfer efficiency; loaded nano-bismuth graphene oxide is mixed with metal oxide to form a three-dimensional network structure to improve adsorption and storage performance.
It improves the electrochemical performance and mechanical strength of the electrode material, extends the service life, enhances the adsorption and storage performance of vanadium ions, avoids the fragility problem of nano-bismuth powder, and improves the overall performance of the battery.
Smart Images

Figure BDA0004920298550000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of liquid flow battery electrode materials, and in particular to a method for preparing a high-activity electrode material for an all-vanadium liquid flow battery. Background Art
[0002] The all-vanadium liquid flow battery consists of two tanks filled with electrolyte solution and a group of electrochemical cell components. The electrolyte solution contains vanadium ions of different valence states. During the charging and discharging process, the vanadium ions in the electrolyte solution are oxidized and reduced, and electrons are exchanged between the positive and negative electrodes of the electrochemical cell to complete the charging and discharging. As one of the key components of the all-vanadium liquid flow energy storage battery, the performance of the electrode has a great influence on the liquid flow energy storage battery. As the electrode material for all-vanadium liquid flow batteries, porous carbon-based materials have a large surface area and excellent corrosion resistance. They are widely used in smart homes, commercial buildings, microgrids and other fields. Therefore, it is urgent to develop a liquid flow battery electrode material with both high mechanical strength and high energy storage capacity.
[0003] As electrode materials for all-vanadium liquid flow batteries, porous carbon-based materials have good chemical stability and a large reaction area during charge and discharge. However, the electrochemical activity of porous carbon-based materials is poor at high current density, which inhibits the operating current of all-vanadium liquid flow batteries and causes a decrease in charge and discharge performance. By depositing nano-bismuth powder on carbon-based materials, sufficient reaction active sites can be provided for vanadium ions, thereby improving the activity of the electrode material. However, nano-bismuth powder is a metal and is easily brittle under external forces at low temperatures, which reduces the electrochemical performance and service life of the electrode material. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a highly active electrode material for an all-vanadium liquid flow battery: after in-situ synthesis of polystyrene on the surface of nanoparticles, the nanoparticles are placed in a culture solution for dilution, and then a carbon precursor is added for mixed culture to prevent the nanoparticles from agglomerating during the culture process, resulting in uneven dispersion of the nanoparticles in the plant carbon precursor, and facilitating the nanoparticles to form a dense conductive network in a porous carbon-based material, thereby improving the electrochemical properties of the electrode material; the enriched core-shell nanoparticle carbon precursor is ground into a powder, pre-oxidized and subjected to high-temperature carbonization treatment, and the polystyrene on the surface of the core-shell nanoparticles is thermally decomposed to release nanoparticles that fill the macropores of the porous carbon-based material, thereby refining the pore size, and As the skeleton of porous carbon-based materials, the mechanical strength of porous carbon-based materials is improved, and the brittleness of porous carbon materials due to pores is avoided; bismuth source is intercalated between graphene oxide layers and then reduced at high temperature to avoid the accumulation of graphene oxide sheets leading to a decrease in charge storage capacity, and nano-bismuth is synthesized between graphene oxide layers to further expand the interlayer spacing, increase the contact area with vanadium ions and the charge transfer efficiency; the nano-bismuth graphene oxide loaded with metal oxide is mixed with metal oxide, and the metal oxide is used as the skeleton of the aerogel to form a three-dimensional network structure, so that the aerogel has higher mechanical properties, and the prepared composite aerogel has excellent adsorption properties, which improves the adsorption and storage properties of vanadium ions.
[0005] The technical problem to be solved by the present invention is as follows: Porous carbon-based materials as electrode materials for all-vanadium liquid flow batteries have good chemical stability and a large reaction area during charge and discharge, but the electrochemical activity of porous carbon-based materials under high current density is poor, and the porous carbon-based materials have relatively low mechanical strength due to their porous structure, and are prone to structural damage or deformation during battery operation, affecting the performance and stability of the battery; by depositing nano-bismuth powder on the carbon-based material, sufficient reaction active sites can be provided for vanadium ions, thereby improving the activity of the electrode material, but nano-bismuth powder is a metal and is easily brittle under external force at low temperatures, thereby reducing the electrochemical performance and service life of the electrode material.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a highly active electrode material for an all-vanadium liquid flow battery comprises the following steps:
[0008] S1. Grinding the enriched core-shell nanoparticle carbon precursor into powder, pre-oxidizing and carbonizing at high temperature to obtain a modified porous carbon-based material;
[0009] Furthermore, the particle size of the enriched core-shell nanoparticle carbon precursor is 20-60 nm.
[0010] Further preferably, the particle size of the enriched core-shell nanoparticle carbon precursor is 20-50 nm.
[0011] Further preferably, the particle size of the enriched core-shell nanoparticle carbon precursor is 40 nm.
[0012] Furthermore, the pre-oxidation temperature is 250-350° C., and the time is 1-4 h.
[0013] More preferably, the pre-oxidation temperature is 250-330° C. and the time is 1-3 h.
[0014] More preferably, the pre-oxidation temperature is 300° C. and the time is 2 h.
[0015] Furthermore, the high temperature carbonization temperature is 600-900°C and the time is 2-5h.
[0016] More preferably, the high temperature carbonization temperature is 600-800° C. and the time is 2-4 hours.
[0017] More preferably, the high temperature carbonization temperature is 700° C. and the time is 3 h.
[0018] Further, the modified porous carbon-based material is prepared by the following steps:
[0019] The enriched core-shell nanoparticle carbon precursor was placed in a freeze dryer and dried for 12 hours to better maintain the internal structure of the plant. It was taken out, placed in a grinder and ground into powder, placed in a muffle furnace, and pre-oxidized at 300°C for 2 hours to depolymerize part of the cellulose, hemicellulose and lignin into monomers. The temperature was raised to 700°C, carbonized for 3 hours under a nitrogen atmosphere, cooled to room temperature, placed in a potassium hydroxide solution, stirred for 2 hours to fully activate the carbon precursor, filtered, washed with deionized water 3 times, and dried in an oven at 60°C for 10 minutes to obtain a modified porous carbon-based material.
[0020] Among them, the core-shell nanoparticles were enriched and pre-oxidized at 300°C to depolymerize the cellulose, hemicellulose and lignin in the carbon precursor Eichhornia crassipes into monomers. The monomers were dehydrated and decarboxylated to generate bio-oil and syngas, promoting the formation of a bio-carbon network.
[0021] Furthermore, a high-temperature carbonization treatment was carried out at 700°C, so that the polystyrene on the surface of the core-shell nanoparticles was thermally decomposed to produce gas release, thereby forming mesoporous pores inside the biochar. The polystyrene on the surface of the core-shell nanoparticles was thermally decomposed to release nanoparticles that filled the macropores of the porous carbon-based material, refining the pore size, converting the macropores into a mesoporous structure, improving the adsorption performance of vanadium ions, providing a channel for ions to enter the carbon-based material, facilitating the diffusion and transfer of electrolyte ions during the charge and discharge process, and enhancing the electrochemical performance.
[0022] Furthermore, the ratio of the enriched core-shell nanoparticle carbon precursor to the potassium hydroxide solution is (5-6) g: (20-40) mL.
[0023] Furthermore, the enriched core-shell nanoparticle carbon precursor is prepared by in-situ synthesizing polystyrene on the surface of the nanoparticle, diluting it in a culture medium, and then adding the carbon precursor for mixed culture.
[0024] Furthermore, the nanoparticles are selected from any one of nanosilver, nanocopper, nanocarbon black, nanotitanium dioxide, and carbon nanotubes.
[0025] Furthermore, the particle size of the nanoparticles is 20-60 nm.
[0026] More preferably, the particle size of the nanoparticles is 20-40 nm.
[0027] More preferably, the particle size of the nanoparticles is 30 nm.
[0028] Furthermore, the carbon precursor is selected from any one of Eichhornia crassipes and Hibiscus scabra.
[0029] Furthermore, the culture solution is prepared by mixing Hoagland's solution, calcium nitrate, and deionized water in a dosage ratio of (0.6-0.66) g: (0.4-0.5) g: (400-600) mL.
[0030] Further, the enriched core-shell nanoparticle carbon precursor is prepared by the following steps:
[0031] A1. Add 3-(methacryloyloxy)propyltrimethoxysilane and nanoparticles to ethanol, stir and react for 24 hours, filter, wash with deionized water three times, and dry in a 90°C oven for 10 minutes to obtain a solid. Add the solid and polyvinyl pyrrolidone to 25 mL of deionized water and 10 mL of ethanol, stir evenly, heat to 45°C, add styrene, potassium persulfate and sodium styrene sulfonate, stir evenly, place in a 80°C water bath, stir and react for 3 hours, add a 36% by mass sodium chloride solution to demulsify, filter to obtain a solid, wash the solid with deionized water three times, and dry in a 60°C oven for 10 minutes to obtain core-shell nanoparticles.
[0032] Among them, 3-(methacryloyloxy)propyltrimethoxysilane reacts with the hydroxyl groups on the surface of the nanoparticles, so that the surface of the nanoparticles carries reactive double bonds. Under the action of the catalyst potassium persulfate and the surfactant polyvinyl pyrrolidone, styrene can be polymerized on the surface of the nanoparticles to form polystyrene-coated nanoparticle microspheres, avoiding the agglomeration of the conductive nanoparticles, allowing the nanoparticles to be evenly dispersed in the carbon precursor water hyacinth plant system, which is beneficial for the nanoparticles to form a dense conductive network in the porous carbon-based material, thereby improving the electrochemical properties of the electrode material.
[0033] Furthermore, the dosage ratio of solid, polyvinyl pyrrolidone, styrene, potassium persulfate and sodium styrene sulfonate is (2-3) g: (0.01-0.03) g: (0.1-0.3) g: (0.001-0.004) g: (0.3-0.7) g.
[0034] A2. Add core-shell nanoparticles to the culture medium, and perform ultrasonic treatment to disperse the core-shell nanoparticles in the culture medium to obtain a dispersion. Place the carbon precursor in the culture medium for 7 days. After culturing in the dispersion for 14 days, take it out and wash the root of the carbon precursor with deionized water to remove the core-shell nanoparticles adhering to the surface, thereby obtaining an enriched core-shell nanoparticle carbon precursor.
[0035] Among them, the plant carbon precursor water hyacinth and core-shell nanoparticles are cultured in culture solution. The root system of the carbon precursor water hyacinth contains a porous structure. When absorbing nutrients from the culture solution, the core-shell nanoparticles enter the roots of the plant carbon precursor water hyacinth through the culture solution flow. Under the action of transpiration tension and root pressure, the nanoparticles are transported to the branches of the water hyacinth, so that the core-shell nanoparticles are evenly dispersed in the carbon precursor system.
[0036] Furthermore, the ratio of the core-shell nanoparticles, culture solution, and carbon precursor is (0.5-1.5) g: (8-12) mL: (8-12) g.
[0037] S2. Mixing the nano-bismuth loaded graphene oxide with metal oxide to prepare a composite aerogel;
[0038] Furthermore, the composite aerogel has a pore size of 30-50 nm and a particle size of 8-15 μm;
[0039] More preferably, the composite aerogel has a pore size of 30-40 nm and a particle size of 8-13 μm.
[0040] More preferably, the composite aerogel has a pore size of 35 nm and a particle size of 11 μm.
[0041] Furthermore, the metal oxide is selected from one or more of nickel oxide, zinc oxide and manganese oxide.
[0042] Furthermore, the particle size of the metal oxide is 0.2-1.5 μm.
[0043] More preferably, the particle size of the metal oxide is 0.2-1 μm.
[0044] More preferably, the particle size of the metal oxide is 0.5 μm.
[0045] Furthermore, the particle size of the nano-bismuth is 50-100 nm.
[0046] More preferably, the particle size of the nano-bismuth is 50-80 nm.
[0047] More preferably, the particle size of the nano-bismuth is 60 nm.
[0048] Further, the composite aerogel is prepared by the following steps:
[0049] The nano-bismuth-loaded graphene oxide and metal oxide were added to deionized water, ultrasonically treated for 30 minutes, 2% by mass of glutaraldehyde was added, stirred for 40 minutes and then cross-linked, heated to 200°C, stirred for 30 minutes to remove unreacted glutaraldehyde, cooled to room temperature, filtered to obtain a gel-like substance, and the gel-like substance was placed in a freeze dryer and freeze-dried at -12°C to obtain a composite aerogel;
[0050] Among them, the oxygen-containing functional groups contained on the surface and sides of the nano-bismuth graphene oxide can react with the hydroxyl groups on the surface of the nano-metal oxide with glutaraldehyde to form a cross-linked gel-like substance in which the nano-bismuth graphene oxide is loaded and coated with the nano-metal oxide. After freeze-drying to remove moisture, a composite aerogel with metal oxide as the skeleton is formed, which has high mechanical strength. The metal oxide acts as a conductive material to form a conductive path inside the aerogel, thereby improving the conductivity of the composite aerogel.
[0051] Furthermore, the amount ratio of loaded nano-bismuth graphene oxide, metal oxide, and glutaraldehyde is (1.6-2) g: (1.4-1.8) g: (0.3-0.7) mL.
[0052] Furthermore, the nano-bismuth loaded graphene oxide is prepared by intercalating a bismuth source into the interlayer of graphene oxide and then reducing it at high temperature;
[0053] Further, the bismuth source is selected from one or more of bismuth nitrate, bismuth citrate and bismuth chloride.
[0054] Furthermore, the particle size of graphene oxide is 0.5-2.5 μm.
[0055] More preferably, the graphene oxide has a particle size of 0.5-2 μm.
[0056] More preferably, the graphene oxide has a particle size of 1.5 μm.
[0057] Furthermore, the high temperature reduction temperature is 600-900°C.
[0058] More preferably, the high temperature reduction temperature is 600-800°C.
[0059] More preferably, the high temperature reduction temperature is 650°C.
[0060] Further, the composite aerogel is prepared by the following steps:
[0061] B1. Add graphene oxide to deionized water, stir evenly, add bismuth source, heat to 40°C, stir at 600 rpm for 40 min, add 36% sodium hydroxide solution to adjust the pH to 7.5, continue stirring for 1 h, filter, wash with deionized water 3 times, and dry in an oven at 80°C for 10 min to obtain modified graphene oxide.
[0062] Among them, under the action of mechanical stirring, the bismuth ions in the bismuth source can combine with the carboxyl and hydroxyl groups between the graphene oxide layers through chemical bonds, so that the bismuth ions are intercalated into the graphene oxide layers, avoiding the accumulation of graphene oxide sheets and causing the charge storage capacity to decrease. The bismuth element has excellent conductive properties and is intercalated into the graphene oxide layers, thereby improving the charge transfer efficiency of the all-vanadium liquid flow battery.
[0063] Furthermore, the usage ratio of graphene oxide, bismuth source and sodium hydroxide solution is (0.05-0.15) g:(0.1-0.2) g:(1-3) mL.
[0064] B2. Place the modified graphene oxide in an atmosphere furnace, introduce inert gas nitrogen, heat to 650°C, treat for 2 hours, cool to room temperature, wash with deionized water for 3 minutes, and dry in an oven at 70°C for 10 minutes to obtain nano-bismuth-loaded graphene oxide.
[0065] Among them, inert gas nitrogen is used as a reducing gas. At 650°C, the bismuth ions between the modified graphene oxide layers are reduced to bismuth atoms. The reduced bismuth atoms aggregate into nuclei to form nano-bismuth particles, thereby forming nano-bismuth particles between the graphene oxide layers, further expanding the interlayer spacing, increasing the contact area with vanadium ions and the charge transfer efficiency. The sheet-arranged graphene oxide can absorb external stress, improve the impact resistance of nano-bismuth, and avoid the fragility of nano-bismuth powder, which leads to a decrease in the electrochemical properties and service life of the electrode material.
[0066] S3. The composite aerogel is mixed with a binder to form a slurry, and the slurry is coated on the surface of the modified porous base material. After drying, roll-forming, and cutting, a highly active electrode material is obtained.
[0067] Furthermore, the binder is selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, carboxylated styrene butadiene latex, and sodium carboxymethyl cellulose.
[0068] Furthermore, the drying temperature is 60-90°C.
[0069] Furthermore, compared with the prior art, the present invention has the following beneficial effects:
[0070] (1) In the technical scheme of the present invention, core-shell nanoparticles formed by in-situ synthesis of polystyrene on the surface of nanoparticles are cultured in a culture medium with a plant carbon precursor, water hyacinthus, and then the core-shell nanoparticles are transported to the branch part of the water hyacinthus, and then the nanoparticles are filled into the carbon precursor system, which is beneficial for the nanoparticles to form a dense conductive network in the porous carbon-based material, thereby improving the electrochemical performance of the electrode material; after pre-oxidation treatment, the cellulose, hemicellulose and lignin in the carbon precursor water hyacinthus are depolymerized into monomers, and the formed monomers are dehydrated and decarboxylated to generate bio-oil and synthesis gas, thereby promoting the formation of a conductive bio-carbon network; after high-temperature carbonization treatment, the polystyrene on the surface of the core-shell nanoparticles is thermally decomposed to generate gas release, thereby forming mesoporous pores inside the biochar, and the polystyrene on the surface of the core-shell nanoparticles is thermally decomposed to release nanoparticles to fill the macroporous pores of the porous carbon-based material, thereby refining the pore size, converting the macropores into mesoporous structures, improving the adsorption performance of vanadium ions, and providing channels for ions to enter the carbon-based material, thereby facilitating the diffusion and transfer of electrolyte ions during the charge and discharge process, thereby enhancing the electrochemical performance.
[0071] (2) In the technical solution of the present invention, the nanoparticles serve as the skeleton of the porous carbon-based material, which improves the mechanical strength of the porous carbon-based material and avoids the brittleness of the porous carbon-based material due to the pores. The nanoparticles dispersed in the porous carbon-based material can connect the pores of the porous carbon-based material to form a conductive network, thereby improving the charge transfer rate of the porous carbon-based material and further improving the electrochemical performance of the carbon-based material.
[0072] (3) In the technical solution of the present invention, the bismuth source is intercalated between the graphene oxide layers and then subjected to high-temperature reduction treatment, so that the metal bismuth ions between the graphene oxide layers are reduced to nano-bismuth particles, thereby avoiding the accumulation of graphene oxide sheets leading to a decrease in charge storage capacity, and further expanding the interlayer spacing, thereby increasing the contact area with vanadium ions and the charge transfer efficiency; the graphene oxide sheets arranged in layers can absorb external stress, improve the impact resistance of nano-bismuth, and avoid the fragility of nano-bismuth powder leading to a decrease in the electrochemical performance and service life of the electrode material. In addition, nano-bismuth powder is synthesized between the graphene oxide layers, so that the nano-bismuth powder can Better adhesion on graphene oxide to avoid the shedding of nano-bismuth powder; aerogel is prepared by loading nano-bismuth graphene oxide and metal oxide, and the metal oxide serves as the skeleton of the aerogel to form a three-dimensional network structure, so that the aerogel has higher mechanical properties, and the formed three-dimensional network structure has better conductivity, provides channels for vanadium ions, and improves electrochemical properties. In addition, the formed aerogel has a porous structure and better adsorption performance, which improves the adsorption and storage performance of vanadium ions, and can adsorb nano-bismuth powder to avoid the shedding of nano-bismuth powder, further enhancing the fixation of nano-bismuth powder.
[0073] (4) In the technical solution of the present invention, the composite aerogel is composited with the modified porous base material to form a composite electrode having high electrochemical activity; the porous aerogel coated on the surface of the modified porous carbon-based material has excellent adsorption properties, which improves the adsorption and storage properties of vanadium ions, thereby increasing the service life of the electrode material. DETAILED DESCRIPTION
[0074] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0075] Example 1
[0076] The modified porous carbon-based material is prepared by the following steps:
[0077] A1. 0.15 g of 3-(methacryloyloxy)propyltrimethoxysilane, 0.5 g of nanosilver, 0.3 g of nanocopper and 0.7 g of nanocarbon black were added to 30 mL of ethanol, stirred for 24 h, filtered, washed and dried to obtain a solid, 2.5 g of the solid and 0.02 g of polyvinyl pyrrolidone were added to 25 mL of deionized water and 10 mL of ethanol, stirred evenly, heated to 45 ° C, 0.2 g of styrene, 0.003 g of potassium persulfate and 0.5 g of sodium styrene sulfonate were added, stirred evenly, placed in a water bath at 80 ° C, stirred for 3 h, and then a 36% mass fraction of sodium chloride solution was added, filtered, washed 3 times and dried to obtain core-shell nanoparticles;
[0078] A2. 1 g of core-shell nanoparticles was added to 10 mL of culture medium, and ultrasonic treatment was performed to obtain a dispersion. 7 g of water hyacinth and 3 g of water hibiscus were placed in the culture medium and cultured for 7 days. After being placed in the dispersion and cultured for 14 days, the roots of the carbon precursors were taken out and washed with deionized water, and dried at 80 ° C to obtain enriched core-shell nanoparticle carbon precursors;
[0079] A3. Place 5.6 g of enriched core-shell nanoparticle carbon precursor in a freeze dryer and dry it for 12 hours. Take it out, grind it in a grinder to powder, place it in a muffle furnace, pre-oxidize it at 300°C for 2 hours, heat it to 700°C, carbonize it in a nitrogen atmosphere for 3 hours, cool it to room temperature, place it in 30 mL of potassium hydroxide solution, stir it for 2 hours, filter it, wash it with deionized water 3 times, and dry it in an oven at 60°C for 10 minutes to obtain a modified porous carbon-based material.
[0080] Comparative Example 1
[0081] The difference between this comparative example and Example 1 is that the nanoparticles are not modified by coating with polystyrene.
[0082] Comparative Example 2
[0083] The difference between this comparative example and Example 1 is that no core-shell nanoparticles are added.
[0084] Example 2
[0085] The composite aerogel is prepared by the following steps:
[0086] B1. Add 0.1 g of graphene oxide to 160 mL of deionized water, stir evenly, add 0.06 g of bismuth nitrate, 0.04 g of bismuth citrate and 0.06 g of bismuth chloride, heat to 40°C, stir at 600 rpm for 40 min, add 2 mL of 36% sodium hydroxide solution to adjust the pH to 7.5, continue stirring for 1 h, filter, wash with deionized water 3 times, and dry in an oven at 80°C for 10 min to obtain modified graphene oxide; place the modified graphene oxide in an atmosphere furnace, introduce inert gas nitrogen, heat to 650°C, treat for 2 h, cool to room temperature, wash with deionized water 3 times, and dry at 70°C for 10 min to obtain nano-bismuth-loaded graphene oxide.
[0087] B2. 1.8 g of nano-bismuth-loaded graphene oxide and 0.7 g of nickel oxide, 0.5 g of zinc oxide, and 0.4 g of manganese oxide were added to 70 mL of deionized water, ultrasonically treated for 30 min, 0.5 mL of 2% glutaraldehyde was added, stirred for 40 min and then cross-linked, the temperature was raised to 200 ° C, stirred for 30 min, cooled to room temperature, and a gel-like substance was obtained by filtration. The gel-like substance was placed in a freeze dryer and freeze-dried at -12 ° C to obtain a composite aerogel.
[0088] Comparative Example 3
[0089] The difference between this comparative example and Example 2 is that the nano-bismuth-loaded graphene oxide is replaced by commercially available graphene oxide.
[0090] Comparative Example 4
[0091] The difference between this comparative example and Example 2 is that nickel oxide, zinc oxide and manganese oxide are not added.
[0092] Example 3
[0093] A method for preparing a highly active electrode material for an all-vanadium liquid flow battery comprises the following steps:
[0094] 12g of composite aerogel, 2.5g of binder and 1.2g of N-methylpyrrolidone solution were mixed and stirred evenly to form a slurry, which was coated on the surface of the modified porous base material and dried in an oven at 80°C. After roller pressing and cutting, a highly active electrode material was obtained.
[0095] Example 4
[0096] A method for preparing a highly active electrode material for an all-vanadium liquid flow battery comprises the following steps:
[0097] 12g of composite aerogel, 2.5g of binder and 1.2g of N-methylpyrrolidone solution were mixed and stirred evenly to form a slurry, which was coated on the surface of the modified porous base material and dried in an oven at 80°C. After roller pressing and cutting, a highly active electrode material was obtained.
[0098] Example 5
[0099] A method for preparing a highly active electrode material for an all-vanadium liquid flow battery comprises the following steps:
[0100] 12g of composite aerogel, 2.5g of binder and 1.2g of N-methylpyrrolidone solution were mixed and stirred evenly to form a slurry, which was coated on the surface of the modified porous base material and dried in an oven at 80°C. After roller pressing and cutting, a highly active electrode material was obtained.
[0101] Comparative Example 5
[0102] The difference between this comparative example and Example 4 is that the modified porous base material is replaced by the material prepared in Comparative Example 1.
[0103] Comparative Example 6
[0104] The difference between this comparative example and Example 4 is that the modified porous base material is replaced by the material prepared in Comparative Example 2.
[0105] Comparative Example 7
[0106] The difference between this comparative example and Example 4 is that the composite aerogel is replaced by the material prepared in Comparative Example 3.
[0107] Comparative Example 8
[0108] The difference between this comparative example and Example 4 is that the composite aerogel is replaced by the material prepared in Comparative Example 4.
[0109] The performance of the highly active electrode materials prepared in Examples 3-5 and Comparative Examples 5-8 was tested.
[0110] The highly active electrode material prepared above was cut into blocks of 8 cm × 6 cm × 0.6 cm as electrodes, and the positive electrode electrolyte was 60 mL VO 2+ The concentration of H2SO4 is 1.5M and the concentration of H2SO4 is 3M. The negative electrode electrolyte is 60mL V 3+ The solution with a concentration of 1.5M and a concentration of 3M H2SO4 was assembled into a single cell and the current density was 80mA / cm 2, the charge voltage is 1.65V, the discharge cut-off voltage is 0.8V, and the electrolyte flow rate is 30mL / min. The conductivity test is performed; the test results are shown in Table 1 below:
[0111] Table 1
[0112]
[0113] It can be seen from the data in Table 1 that Comparative Example 5 is a modified porous carbon-based material prepared without polystyrene coating modification, which is used as a high-activity electrode material for all-vanadium liquid flow batteries. Its electrochemical performance and mechanical breakage are reduced. This may be because styrene can be polymerized on the surface of nanoparticles to form polystyrene-coated nanoparticle microspheres, avoiding the agglomeration of conductive nanoparticles, so that the nanoparticles can be evenly dispersed in the carbon precursor water hyacinth plant system; Comparative Example 6 is a modified porous carbon-based material prepared without adding core-shell nanoparticles, which is used as a high-activity electrode material for all-vanadium liquid flow batteries. Its electrochemical performance and mechanical breakage are reduced. This may be because the nanoparticles serve as the skeleton of the porous carbon-based material, which improves the mechanical strength of the porous carbon-based material and avoids the porous carbon material from being brittle due to the pores. The particles can connect the pores of the porous carbon-based material to form a conductive network, thereby improving the charge transfer rate of the porous carbon-based material; in comparative example 7, the nano-bismuth-loaded graphene oxide is replaced with commercially available graphene oxide, and the prepared composite aerogel is coated on the surface of the porous carbon-based material, and its electrochemical performance is reduced. This may be because nano-bismuth is synthesized between the graphene oxide layers, the interlayer spacing is expanded, the accumulation of graphene oxide sheets is avoided, resulting in a decrease in charge storage capacity, and the shedding of nano-bismuth powder is avoided; in comparative example 8, no metal oxide is added, and the prepared composite aerogel is coated on the surface of the porous carbon-based material, and its strength and electrochemical performance are reduced. This may be because the nano-bismuth-loaded graphene oxide and the metal oxide are used to prepare the aerogel, and the metal oxide serves as the skeleton of the aerogel to form a three-dimensional network structure, so that the aerogel has higher mechanical properties.
[0114] The data in Table 1 show that the highly active electrode materials prepared in Examples 3-5 not only have high telephone performance and mechanical strength, but also have a better service life and higher activity. The enriched core-shell nanoparticle carbon precursor is ground into powder, subjected to pre-oxidation and high-temperature carbonization treatment, and cooled to room temperature to obtain a modified porous carbon-based material; the loaded nano-bismuth graphene oxide is mixed with a metal oxide to prepare a composite aerogel; the composite aerogel is mixed with a binder to form a slurry, and the slurry is coated on the surface of the modified porous base material. After drying, roll forming, and cutting, the prepared highly active electrode materials meet the test performance requirements, while the highly active electrode materials prepared in Comparative Examples 5-8 do not meet the performance requirements, indicating that the highly active electrode materials prepared in the present invention only have high telephone performance and mechanical strength, and the electrode materials have a better service life and higher activity.
[0115] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0116] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a highly active electrode material for an all-vanadium redox flow battery, characterized in that: The preparation method comprises the following steps: S1. Grinding the enriched core-shell nanoparticle carbon precursor into powder, pre-oxidizing and carbonizing at high temperature to obtain a modified porous carbon-based material; The enriched core-shell nanoparticle carbon precursor is prepared by in-situ synthesizing polystyrene on the surface of the nanoparticle, diluting it in a culture solution, and then adding the carbon precursor for mixed culture; The nanoparticles are selected from any one of nanosilver, nanocopper, nanocarbon black, nanotitanium dioxide, and carbon nanotubes; The particle size of the nanoparticles is 20-60 nm; The carbon precursor is selected from any one of Eichhornia crassipes and Hibiscus scabra; S2. Mixing the loaded nano-bismuth graphene oxide with metal oxide to prepare a composite aerogel; The nano-bismuth loaded graphene oxide is prepared by intercalating a bismuth source between graphene oxide layers and then reducing the interlayer at high temperature; The bismuth source is selected from one or more of bismuth nitrate, bismuth citrate and bismuth chloride; The graphene oxide particle size is 0.5-2.5 μm; The high temperature reduction temperature is 600-900°C; S3. The composite aerogel is mixed with a binder to form a slurry, and the slurry is coated on the surface of the modified porous base material. After drying, roll-forming, and cutting, a highly active electrode material is obtained.
2. The method for preparing a highly active electrode material for an all-vanadium redox flow battery according to claim 1, characterized in that: The pre-oxidation temperature is 250-350° C. and the time is 1-4 hours.
3. The method for preparing a highly active electrode material for an all-vanadium redox flow battery according to claim 1, characterized in that: The high temperature carbonization temperature is 600-900°C and the time is 2-5h.
4. The method for preparing a highly active electrode material for an all-vanadium redox flow battery according to claim 1, characterized in that: The culture solution is prepared by mixing Hoagland's solution, calcium nitrate and deionized water in a dosage ratio of (0.6-0.66) g: (0.4-0.5) g: (400-600) mL.
5. The method for preparing a highly active electrode material for an all-vanadium redox flow battery according to claim 1, characterized in that: The particle size of the enriched core-shell nanoparticle carbon precursor is 20-60 nm.
6. The method for preparing a highly active electrode material for an all-vanadium redox flow battery according to claim 1, characterized in that: The high temperature reduction temperature is 600-800°C.
7. The method for preparing a highly active electrode material for an all-vanadium redox flow battery according to claim 1, characterized in that: The metal oxide is selected from one or more of nickel oxide, zinc oxide and manganese oxide; the particle size of the metal oxide is 0.2-0.5 μm.
8. The method for preparing a highly active electrode material for an all-vanadium redox flow battery according to claim 1, characterized in that: The composite aerogel has a pore size of 30-50 nm and a particle size of 8-15 μm.
9. The method for preparing a highly active electrode material for an all-vanadium redox flow battery according to claim 1, characterized in that: The particle size of the nano bismuth is 50-100 nm.
10. The method for preparing a highly active electrode material for an all-vanadium redox flow battery according to claim 1, characterized in that: The binder is selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, carboxylated styrene butadiene latex, and sodium carboxymethyl cellulose.
Citation Information
Patent Citations
Composite electrode material and preparation method thereof, and applications of composite electrode material in all-vanadium flow battery
CN106549162A
Bi-NPs@GO / Al composite hydrolysis hydrogen production material and preparation method thereof
CN110065928A
Metal bismuth nanoparticle composite material and preparation method and application thereof
CN113089017A
Molybdenum dioxide, titanium dioxide and nitrogen-doped carbon nano composite material and preparation method of negative electrode of lithium ion battery
CN115849447A
Bismuth-based composite negative electrode material for sodium-ion battery