Graphitized carbon carrier as well as low-temperature preparation method and application thereof

The graphitized carbon carrier is prepared at low temperature by microwave, which solves the temperature gradient and energy consumption problems in high-temperature preparation methods, improves the durability of the graphitized carbon carrier and the electrocatalytic performance of the platinum carbon catalyst, and achieves efficient and environmentally friendly catalyst synthesis.

CN118851166APending Publication Date: 2024-10-29WUXI WEIFU HIGH TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411028936.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In the existing technology, the high-temperature preparation method of graphitized carbon carrier has problems of temperature gradient and uneven heating, which leads to high energy consumption and difficulty in large-scale application. Moreover, the catalyst is prone to failure under operating conditions such as start-up and stop, rapid load change, and cold start. Corrosion causes Pt particles to fall off and reduces the electrochemical active area.

Method used

The method of preparing graphitized carbon carrier at low temperature using microwave is to graphitize carbon powder and inorganic metal salts or metal elements in a microwave reactor, use microwave energy to heat evenly, lower the graphitization temperature, reduce energy consumption, and pass through the acid After liquid cleaning and deionized water rinsing, the graphitized carbon carrier was obtained, which was used to synthesize platinum carbon catalyst.

Benefits of technology

The uniformity and durability of the graphitized carbon carrier are improved. The platinum carbon catalyst formed after loading platinum has good electrocatalytic performance, reduces energy consumption, avoids burning loss of the sample surface, and simplifies the process flow to facilitate automation and Continuous production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851166A_ABST
    Figure CN118851166A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of new energy materials and application, and particularly relates to a graphitized carbon carrier and a low-temperature preparation method and application thereof. The low-temperature preparation method of the graphitized carbon carrier comprises the following steps: (1) uniformly dispersing carbon powder into water, adding an inorganic metal salt or a metal simple substance into a dispersion liquid, magnetically stirring for 1-5 hours, and stirring and evaporating to dryness in a water bath to obtain a solid mixture; and (2) transferring the solid mixture into a microwave reaction furnace for graphitization treatment, introducing argon, controlling the microwave power to be 2000-6000 W, the microwave time to be 10-90 min and the reaction temperature to be 600-1300 DEG C, cleaning the graphitized solid with an acid solution, then washing the solid with deionized water until the solid is neutral, and filtering and drying the solid to obtain the graphitized carbon carrier. The preparation process is simple, the obtained graphitized carbon carrier has excellent durability, and the formed platinum-carbon catalyst has good electro-catalytic performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of new energy materials and applications, and specifically relates to a graphitized carbon carrier and a low-temperature preparation method and application thereof. Background Art

[0002] Proton exchange membrane fuel cells use hydrogen and oxygen to produce electricity through electrochemical reactions, which in turn drive the motor. The cathode / anode catalyst layer is the site of the fuel cell reaction, and Pt / C catalyst is still the best choice for fuel cell catalysts at this stage. However, in actual operating conditions, there will be phenomena such as start-stop, rapid load change, cold start and insufficient gas supply. The appearance of these phenomena will cause the catalyst carbon carrier to be corroded, resulting in the detachment and agglomeration of the Pt particles in the catalyst layer, which will lead to a decrease in the electrochemical active area (ECSA). At the same time, a large amount of heat will be generated when the reverse polarity occurs, which will form local high-temperature points, accelerate the degradation of the proton exchange membrane, form holes, reduce the open circuit voltage, and even form a short circuit in severe cases. Therefore, it is necessary to select carbon materials with special structures as carriers to synthesize highly durable Pt / C catalysts.

[0003] Graphitized carbon carrier is a porous carbon material. Due to its unique structure and properties, it has excellent resistance to high potential corrosion and is widely used in catalysis, adsorption, energy storage and other fields. However, the treatment of graphitized carbon carriers often requires high temperatures (above 2000°C), which consumes a lot of energy. Traditional heating methods will result in temperature gradients and uneven heating, which limits its large-scale application. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a graphitized carbon carrier and a low-temperature preparation method and application thereof. The present invention adopts microwave low-temperature to prepare the graphitized carbon carrier, and the obtained graphitized carbon carrier has excellent durability, and the platinum-carbon catalyst formed after loading platinum has good electrocatalytic performance.

[0005] In order to achieve the above technical objectives, the technical solution adopted by the embodiment of the present invention is: In a first aspect, an embodiment of the present invention provides a low-temperature preparation method of a graphitized carbon carrier, comprising the following steps: (1) Dispersing carbon powder evenly in 50-500 mL of water, adding inorganic metal salt or metal element to the dispersion, stirring magnetically for 1-5 hours, and then stirring and evaporating in a water bath to obtain a solid mixture; (2) The solid mixture in step (1) is transferred to a microwave reactor for graphitization treatment, argon is introduced for 30-60 minutes, the air in the reactor is removed, the microwave power is 2000-6000W, the microwave time is 10-90 minutes, and the reaction temperature is 600-1300°C. After the graphitization treatment is completed, the solid is washed with acid solution, then rinsed with deionized water until neutral, filtered and dried to obtain a graphitized carbon carrier.

[0006] Furthermore, the carbon powder in step (1) is one or more of XC-72, Ketjen black, acetylene black or PANi-10.

[0007] Furthermore, in step (1), the mass ratio of the inorganic metal salt or metal element to the carbon powder is 1:1-1:10; The inorganic metal salt is one or more of nickel chloride, cobalt chloride, ferric chloride, ferric nitrate, cobalt nitrate and ferric nitrate; The metal element is one or more of nickel, iron, cobalt and molybdenum.

[0008] Furthermore, in step (2), the microwave power is 3000-4000 W, the microwave time is 20-30 min, and the reaction completion temperature is 800-1000° C.

[0009] Furthermore, the acid solution in step (2) is one or more of sulfuric acid, nitric acid, acetic acid, hydrochloric acid and carbonic acid solution, and the concentration of the acid solution is 0.1-4 mol / L.

[0010] In a second aspect, an embodiment of the present invention provides a graphitized carbon carrier, which is prepared by the preparation method described in the first aspect.

[0011] In a third aspect, an embodiment of the present invention provides an application of the graphitized carbon carrier described in the second aspect, wherein the graphitized carbon carrier is used to prepare a platinum-carbon catalyst.

[0012] Furthermore, the preparation method of the platinum-carbon catalyst comprises the following steps: Step S1, adding 1-5 g of graphitized carbon carrier to 30-300 mL of ethylene glycol, stirring evenly with magnetic force, adding 3-20 g of chloroplatinic acid hexahydrate, dispersing evenly with ultrasonic force, adding 5-8 g of sodium carbonate to the solution, ultrasonicating until the sodium carbonate is completely dissolved, and adjusting the pH value of the solution to between 6-12; Step S2, transferring the solution obtained in step S1 to a sealed reactor, placing the reactor in an oven, setting the oven temperature to 100-200°C, and maintaining for 1-5 hours. After the reaction is completed, cooling the reactor to room temperature, taking out the product and separating it by centrifugation or filtration for multiple times, and drying in an oven at 50-120°C to obtain a platinum-carbon catalyst.

[0013] The technical solution provided by the embodiment of the present invention has the following beneficial effects: (1) The traditional heating method will cause temperature gradient and uneven heating. The present invention uses microwaves, which can evenly penetrate the carbon material. The carbon atoms in the carbon carrier are excited by the microwave energy, and current is generated inside, resulting in heat generated inside the carbon material, thereby achieving rapid and uniform heating. The preparation method of the present invention does not require high temperature, high pressure and other operating conditions, has a mild reaction, is safe and simple, and has uniform graphitization treatment. The resulting graphitized carbon carrier has excellent durability.

[0014] (2) The processing method of graphitized carbon carriers often requires high temperature (above 2000°C), which consumes a lot of energy. Microwave heating is internal heating with high energy utilization rate. Therefore, graphitization can be achieved at a lower temperature, reducing energy consumption and avoiding burning of the sample surface without producing harmful substances. It is a green and environmentally friendly processing method.

[0015] (3) Microwave heating can adjust the microwave power within a few seconds without affecting the normal preparation process. After adjusting the microwave output power, the heating state of the material changes instantly without inertia, achieving instant heating and real-time adjustment, which is convenient for automation and continuous production.

[0016] (4) The obtained graphitized carbon carrier is used in the Pt / C catalyst synthesis reaction through a simple one-step hydrothermal reduction reaction. The reaction is mild and easy to operate. The Pt / C catalyst has good carrier durability.

[0017] (5) The addition of metal salts or metal elements reduces the graphitization temperature of carbon materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is the XRD spectra of XC-72 carbon powder before and after graphitization treatment in Example 1 and Comparative Example 1.

[0019] Figure 2 This is the Raman spectrum of the XC-72 carbon powder after graphitization treatment in Example 1.

[0020] Figure 3 This is the Raman spectrum of the XC-72 carbon powder in Comparative Example 1.

[0021] Figure 4 It is a constant potential test diagram of the XC-72 carbon powder before and after graphitization treatment in Example 1 and Comparative Example 1.

[0022] Figure 5 It is the CV curve of the platinum-carbon catalyst prepared in Example 1.

[0023] Figure 6 This is the CV graph of the platinum-carbon catalyst prepared in Example 1 before and after testing the durability of the carbon carrier.

[0024] Figure 7 This is the CV graph of the platinum-carbon catalyst prepared in Example 2 before and after testing the durability of the carbon carrier. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0026] Example 1 A low-temperature preparation method for a graphitized carbon carrier comprises the following steps: (1) Weigh 2 g of XC-72 carbon powder and evenly disperse it in 150 mL of deionized water. Then add 0.5 g of nickel chloride. After magnetic stirring for 2 h, put it in a water bath and evaporate to dryness at 80 °C to obtain a solid mixture. (2) The solid mixture obtained in step (1) is transferred to a microwave reactor, and argon is introduced for 30-60 minutes to remove the air in the reactor. The microwave power is 3500 W, the microwave time is 30 minutes, and the reaction temperature is 900°C. After the graphitization treatment is completed, the solid is washed with 0.1M sulfuric acid, then rinsed with deionized water until neutral, filtered, and dried to obtain a graphitized carbon carrier.

[0027] The preparation of a platinum-carbon catalyst using the graphitized carbon carrier comprises the following steps: Take 2g of graphitized carbon carrier and add it to 50mL of ethylene glycol, stir it evenly with magnetic stirring, then add 5.3g of chloroplatinic acid hexahydrate, disperse it evenly with ultrasonic stirring, add 6g of sodium carbonate to the solution, and ultrasonicate until the sodium carbonate is completely dissolved. The pH value of the solution is 9. The above solution is transferred to a sealed reactor, the oven temperature is set to 180°C, and maintained for 3h. After the reaction is completed, the reactor is cooled to room temperature, the product is taken out and separated by centrifugation or filtration for multiple times, and dried at 80°C for 12h to obtain a platinum-carbon catalyst.

[0028] The process of this embodiment is simple, the obtained XC-72 graphitized carbon carrier has excellent durability, and the platinum-carbon catalyst formed after loading platinum has good electrocatalytic performance.

[0029] Example 2 A low-temperature preparation method for a graphitized carbon carrier comprises the following steps: (1) Weigh 2 g of XC-72 carbon powder and evenly disperse it in 150 mL of deionized water. Then add 0.5 g of nickel chloride and stir it magnetically for 2 h. Then put it in a water bath and evaporate it at 80 °C to obtain a solid mixture. (2) The solid mixture obtained in step (1) is transferred to a microwave reactor, and argon is introduced for 30-60 minutes to remove the air in the reactor. The microwave power is 4000 W, the microwave time is 40 minutes, and the reaction temperature is 1000°C. After the graphitization treatment is completed, the solid is washed with 0.1M sulfuric acid, then rinsed with deionized water until neutral, filtered, and dried to obtain a graphitized carbon carrier.

[0030] Example 3 A low-temperature preparation method for a graphitized carbon carrier comprises the following steps: (1) Weigh 2 g of XC-72 carbon powder and evenly disperse it in 150 mL of deionized water. Then add 0.5 g of nickel chloride and stir it magnetically for 2 h. Then put it in a water bath and evaporate it at 80 °C to obtain a solid mixture. (2) The solid mixture obtained in step (1) is transferred to a microwave reactor, and argon is introduced for 30-60 minutes to remove the air in the reactor. The microwave power is 2000 W, the microwave time is 90 minutes, and the reaction temperature is 1300°C. After the graphitization treatment is completed, the solid is washed with 0.1M sulfuric acid, then rinsed with deionized water until neutral, filtered, and dried to obtain a graphitized carbon carrier.

[0031] Example 4 A low-temperature preparation method for a graphitized carbon carrier comprises the following steps: (1) Weigh 2 g of XC-72 carbon powder and evenly disperse it in 150 mL of deionized water. Then add 0.5 g of nickel chloride and stir it magnetically for 2 h. Then put it in a water bath and evaporate it at 80 °C to obtain a solid mixture. (2) The solid mixture obtained in step (1) is transferred to a microwave reaction furnace, and argon gas is introduced for 30-60 minutes to remove the air in the reaction furnace. The microwave power is 6000 W, the microwave time is 20 minutes, and the reaction temperature is 1000°C. After the graphitization treatment is completed, the solid is washed with 0.1M sulfuric acid, then rinsed with deionized water until neutral, filtered, and dried to obtain a graphitized carbon carrier.

[0032] Example 5 A low-temperature preparation method for a graphitized carbon carrier comprises the following steps: (1) Weigh 3 g of Ketjen black and evenly disperse it in 200 mL of deionized water, then add 0.5 g of metallic nickel, stir magnetically for 2 h, place in a water bath, and evaporate to dryness at 80 °C to obtain a solid mixture; (2) The solid mixture obtained in step (1) was transferred to a microwave reactor, and argon gas was introduced for 30 minutes to remove the air in the reactor. The microwave power was set to 3500 W and the microwave time was 30 minutes. After the graphitization treatment was completed, the solid was washed with 0.1 M sulfuric acid, then rinsed with deionized water until neutral, filtered and dried to obtain a graphitized carbon carrier.

[0033] The preparation of a platinum-carbon catalyst using the graphitized carbon carrier comprises the following steps: Take 2 g of the above-mentioned graphitized carrier and add it to 50 mL of ethylene glycol. Stir it evenly with a magnetic stirrer. Then add 5.3 g of chloroplatinic acid hexahydrate and disperse it evenly with an ultrasonic stirrer. Then add 6 g of sodium carbonate to the solution and disperse it evenly with an ultrasonic stirrer until the sodium carbonate is completely dissolved. The pH value of the solution is 9. The above-mentioned solution is transferred to a sealed reactor and the oven temperature is set to 180°C for 3 hours. After the reaction is completed, the reactor is cooled to room temperature. The product is taken out and separated by centrifugation or filtration for multiple times. After drying at 80°C, a platinum-carbon catalyst is obtained.

[0034] Example 6 A low-temperature preparation method for a graphitized carbon carrier comprises the following steps: (1) Weigh 3 g of acetylene black and evenly disperse it in 200 mL of deionized water. Then add 0.5 g of metallic nickel to the mixture. After magnetic stirring for 2 h, place the mixture in a water bath and evaporate to dryness at 80 °C to obtain a solid mixture. (2) The solid mixture obtained in step (1) was transferred to a microwave reactor, and argon gas was introduced for 30 minutes to remove the air in the reactor. The microwave power was set to 3500 W and the microwave time was 30 minutes. After the graphitization treatment was completed, the solid was washed with 0.1 M sulfuric acid, then rinsed with deionized water until neutral, filtered and dried to obtain a graphitized carbon carrier.

[0035] The preparation of a platinum-carbon catalyst using the graphitized carbon carrier comprises the following steps: Take 2 g of the above-mentioned graphitized carrier and add it to 50 mL of ethylene glycol. Stir it evenly with a magnetic stirrer. Then add 5.3 g of chloroplatinic acid hexahydrate and disperse it evenly with an ultrasonic stirrer. Then add 6 g of sodium carbonate to the solution and disperse it evenly with an ultrasonic stirrer until the sodium carbonate is completely dissolved. The pH value of the solution is 9. The above-mentioned solution is transferred to a sealed reactor and the oven temperature is set to 180°C for 3 hours. After the reaction is completed, the reactor is cooled to room temperature. The product is taken out and separated by centrifugation or filtration for multiple times. After drying at 80°C, a platinum-carbon catalyst is obtained.

[0036] Comparative Example 1 Untreated XC-72 toner.

[0037] Comparative Example 2 XC-72 carbon powder loaded with platinum: Take 2g of XC-72 carbon powder and add it to 50mL of ethylene glycol, stir it evenly with a magnetic stirrer, then add 5.3g of chloroplatinic acid hexahydrate, disperse it evenly with an ultrasonic stirrer, then add 6g of sodium carbonate to the solution, and ultrasonicate until the sodium carbonate is completely dissolved, and the pH value of the solution is 9. The above solution is transferred to a sealed reactor, and the oven temperature is set to 180°C and maintained for 3h. After the reaction is completed, the reactor is cooled to room temperature, the product is taken out and separated by centrifugation or filtration for multiple times, and dried at 80°C to obtain a platinum-carbon catalyst.

[0038] By the attached Figure 1 It can be seen that the XRD of XC-72 carbon powder does not change before and after graphitization, and the (002) crystal plane peak intensity becomes larger after graphitization, indicating that the degree of graphitization increases. The structure of the carbon powder is not changed after treatment. Figure 2 and Figure 3 As shown in the figure, the ratio ID / IG of the D peak and the G peak represents the degree of graphitization of the carbon carrier. The smaller the ratio, the higher the degree of graphitization, and the stronger the corrosion resistance of the carbon carrier at high potential. As shown in the figure, the XC-72 carbon powder that has been graphitized has a higher degree of graphitization. Figure 4 This is a high potential corrosion resistance test of XC-72 carbon powder before and after graphitization. The test was conducted at a constant potential of 1.2V vs RHE for 1h. The smaller the current, the stronger the resistance to high potential corrosion, which further reflects that the graphitization treatment has better corrosion resistance.

[0039] Figure 5 and Figure 6 It shows that the graphitized XC-72 carbon powder loaded with platinum has excellent electrocatalytic performance, with an electrochemical active area (ECSA) of 59.39 m 2 / g, and after 5000 cycles of carrier durability testing at 1-1.5V (vs RHE), it only decayed by 2.44%. The electrochemical active area is calculated using the following formula: ECSA=100S / (V·M·C) The adsorption area of ​​S-hydrogen is in A·V. Note: The integral area is the integral area from 0.40 V to 0.05 V minus the integral area from 0.40 V to 0 A.

[0040] V-scan rate mV / s; M- platinum loading of catalyst on glassy carbon electrode (g); C - Hydrogen adsorption constant of smooth platinum, unit is 0.210mC / cm 2 ; Note: Only applicable in acid electrolyte.

[0041] Figure 7The durability of the carrier was tested after platinum was loaded on XC-72 without graphitization treatment. After 5000 cycles of the carrier durability test, the carrier decayed by 18.42%, indicating that the platinum-carbon catalyst synthesized on the carbon carrier after this graphitization treatment has excellent carrier durability.

[0042] The preparation method of the present invention adopts microwave treatment, which can realize the rapid preparation of graphitized carbon carrier at a lower temperature, greatly reducing energy consumption. When microwave radiation irradiates the carbon material, current will be generated due to the interaction between the free electrons in the carbon material and the microwave field. These currents will cause heat to be generated inside the carbon material, thereby realizing rapid heating. Since microwave heating is internal heating, graphitization can be achieved at a lower temperature, reducing energy consumption and avoiding sample surface burning. In the microwave treatment process, the carbon material can be used not only as a carrier but also as a reducing agent. Microwave heating can provide energy to promote the reaction of carbon atoms in the carbon material with other elements (such as oxygen, hydrogen, etc.), thereby realizing graphitization. This reduction reaction helps to improve the graphitization degree and performance of the graphitized carbon carrier. In addition, microwave heating can realize the adjustment of microwave power within a few seconds, without affecting the normal progress of the preparation process. After adjusting the microwave output power, the heating state of the material changes instantly, without inertia, realizing instant heating and real-time adjustment, and facilitating automation and continuous production. The degree of graphitization can be adjusted by controlling the time, power and temperature of microwave heating. The higher the degree of graphitization, the better the conductivity and thermal stability of the carbon carrier. The present invention synthesizes a highly durable Pt / C catalyst by microwave treatment of the carbon carrier and a simple hydrothermal reaction method, thereby improving the durability of the Pt / C catalyst.

[0043] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A low-temperature preparation method for a graphitized carbon carrier, It is characterized in that The following steps are involved: (1) Dispersing carbon powder evenly in 50-500 mL of water, adding inorganic metal salt or metal element to the dispersion, stirring magnetically for 1-5 hours, and then stirring and evaporating in a water bath to obtain a solid mixture; (2) The solid mixture in step (1) is transferred to a microwave reactor for graphitization treatment, argon is introduced for 30-60 minutes, the air in the reactor is removed, the microwave power is 2000-6000W, the microwave time is 10-90 minutes, and the reaction temperature is 600-1300°C. After the graphitization treatment is completed, the solid is washed with acid solution, then rinsed with deionized water until neutral, filtered and dried to obtain a graphitized carbon carrier.

2. The method for preparing a graphitized carbon carrier at low temperature according to claim 1, It is characterized in that The carbon powder in step (1) is one or more of XC-72, Ketjen black, acetylene black or PANi-10.

3. The method for preparing a graphitized carbon carrier at low temperature according to claim 1, It is characterized in that In step (1), the mass ratio of the inorganic metal salt or metal element to the carbon powder is 1:1-1:10; The inorganic metal salt is one or more of nickel chloride, cobalt chloride, ferric chloride, ferric nitrate, cobalt nitrate and ferric nitrate; The metal element is one or more of nickel, iron, cobalt and molybdenum.

4. The method for preparing a graphitized carbon carrier at low temperature according to claim 1, It is characterized in that In step (2), the microwave power is 3000-4000 W, the microwave time is 20-30 min, and the reaction completion temperature is 800-1000° C.

5. The method for preparing a graphitized carbon carrier at low temperature according to claim 1, It is characterized in that The acid solution in step (2) is one or more of sulfuric acid, nitric acid, acetic acid, hydrochloric acid and carbonic acid solution, and the concentration of the acid solution is 0.1-4 mol / L.

6. A graphitized carbon carrier, It is characterized in that The method is prepared by the preparation method according to any one of claims 1 to 5.

7. Use of the graphitized carbon carrier according to claim 6, It is characterized in that The graphitized carbon carrier is used for preparing a platinum-carbon catalyst.

8. Use of the graphitized carbon carrier according to claim 7, It is characterized in that The preparation method of the platinum-carbon catalyst comprises the following steps: Step S1, adding 1-5 g of graphitized carbon carrier to 30-300 mL of ethylene glycol, stirring evenly with magnetic force, adding 3-20 g of chloroplatinic acid hexahydrate, dispersing evenly with ultrasonic force, adding 5-8 g of sodium carbonate to the solution, ultrasonicating until the sodium carbonate is completely dissolved, and adjusting the pH value of the solution to between 6 and 12; Step S2, transferring the solution obtained in step S1 to a sealed reactor, placing the reactor in an oven, setting the oven temperature to 100-200°C, and maintaining for 1-5 hours. After the reaction is completed, cooling the reactor to room temperature, taking out the product and separating it by centrifugation or filtration for multiple times, and drying in an oven at 50-120°C to obtain a platinum-carbon catalyst.

Citation Information

Patent Citations

  • Fuel cell catalyst graphitized carbon carrier, preparation method thereof and fuel cell catalyst employing graphitized carbon carrier

    CN108649243A

  • Graphite crystallization treatment method of amorphous carbon material, product generated during recovering graphite and graphite

    JP2017145151A

  • Carbon-supported platinum group metal catalyst, preparation method therefor and use thereof

    US20230364587A1

  • Carbon-supported platinum group metal catalyst, preparation method therefor and application thereof

    US20230369609A1