High-matching glass powder for LTCC (Low Temperature Co-Fired Ceramic), copper conductor paste as well as preparation method and application of high-matching glass powder

By designing high-matching glass powder and copper conductor paste, combined with MnO, CaO, and BaO oxides in the SiO2-B2O3-Na2O ternary glass system, the sintering density of the copper conductor paste and the shrinkage matching of the porcelain body in LTCC technology are solved Solve the problem of insufficient performance and realize low-cost, high-reliability copper conductor paste, improving the electrical performance and reliability of LTCC products.

CN118851580APending Publication Date: 2024-10-29EAST CHINA UNIV OF SCI & TECH
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410893084.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In LTCC technology, the sintering density of the copper conductor paste and the shrinkage matching of the porcelain body are insufficient, resulting in abnormal connectivity and unstable performance. The existing precious metal paste is costly and difficult to localize, making it difficult to achieve low-cost, high-reliability rapid develop.

Method used

Design a high-matching glass powder and copper conductor slurry, by introducing MnO, CaO, BaO oxides in the SiO2-B2O3-Na2O ternary glass system, combined with copper powder, to improve the matching and matching between glass powder and LTCC green porcelain The sintering bonding force adopts the integrated process of debinding and sintering to enhance the interface bonding force and avoid defects such as cracks.

Benefits of technology

It realizes the low cost and high reliability of copper conductor paste, ensures the high bonding strength and dense sintering of the conductor and LTCC substrate, avoids cracks and crack defects, and improves the electrical performance and reliability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004928173930000011
    Figure HDA0004928173930000011
  • Figure HDA0004928173930000012
    Figure HDA0004928173930000012
  • Figure HDA0004928173930000021
    Figure HDA0004928173930000021
Patent Text Reader

Abstract

The invention discloses high-matching glass powder for LTCC (Low Temperature Co-Fired Ceramic), copper conductor paste as well as a preparation method and application of the high-matching glass powder and the copper conductor paste, and belongs to the field of electronic materials. The chemical composition of the glass powder comprises the following components in percentage by weight: 15 to 30 percent of SiO2, 23 to 32 percent of B2O3, 3 to 9 percent of Na2O and 0 to 50 percent of MO (M is Mn, Ba and Ca). According to the method, MnO, CaO and BaO oxides are introduced into SiO2-B2O3-Na2O in a ternary glass system, the matching performance of glass powder and LTCC raw ceramic is improved, the binding force of copper paste and raw ceramic during sintering is improved, specifically, in the sintering process, Ca and Ba in the glass powder and Ca and Ba in a raw ceramic tape are mutually diffused, copper in copper conductor paste can be diffused into the LTCC tape, Cu, Ca and Ba are diffused into an LTCC substrate from a conductor after sintering, and the bonding force between the copper paste and the raw ceramic is improved. Therefore, the bonding strength between the conductor and the LTCC substrate is improved. Besides, manganese exists on an interface between a conductor and an LTCC substrate in the form of Cu-Mn alloy or oxide, so that the interface bonding strength is enhanced, the defects of cracks, cracks and the like formed on the interface between the conductor and the substrate in acidic and alkaline solutions are effectively avoided, meanwhile, the electrical property sheet resistance of the conductive copper paste prepared from the glass powder is smaller than 2 m omega / square, and the conductivity of the conductive copper paste is greatly improved. The method has the advantages of low porosity and high sintering densification degree.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electronic materials technology, specifically relating to a high-matching glass powder and copper conductor paste for LTCC, their preparation methods and applications. Background Technology

[0002] The miniaturization, integration, low cost, and high reliability of electronic products have greatly driven the rapid development of information technology. Lightweight ceramic capacitors (LTCCs) represent a major trend in component manufacturing process integration and, due to their excellent thermodynamic, electronic, and mechanical properties, have become a priority development direction in the fields of electronic components, integrated devices, and microwave devices, showing promising application prospects. The demand for low-cost LTCCs has led to the gradual adoption of base metals in LTCC electronic pastes. Copper powder, as a functional phase in conductive pastes, has conductivity second only to silver, and possesses low cost and low diffusion characteristics, currently enjoying widespread application in electronic pastes.

[0003] Conductive copper paste, as a co-fired conductive paste used in LTCC technology, is printed on the outer surface of LTCC components to achieve their connection with external circuits. Poor sintering density of the copper layer and defects such as internal cracking can lead to abnormal internal and external connections and product performance failure. Therefore, the sintering density of the paste, its shrinkage matching with the ceramic body, and its adhesion have a decisive impact on the reliability of LTCC products.

[0004] In commercial applications of LTCC, high-compatibility and high-bonding conductor pastes are mainly precious metal pastes such as silver and gold pastes. For example, TDK Corporation of Japan provides a paste for Ag / Au precious metal conductors and a glass-ceramic substrate in JP2012-221765A. CN115691855A, CN116344099A, and CN116900328A provide silver and gold conductor pastes, respectively. These conductive pastes have good co-firing compatibility with ceramic raw material tapes and exhibit good performance after printing and sintering, but the sintering temperature and cost are relatively high.

[0005] The patent CN112509727A, which is similar to this one, mainly focuses on the pretreatment of copper powder and preferably uses 38SiO2-6HfO2-8Al2O3-38CuO glass to achieve excellent co-firing compatibility, printability, and conductivity between the electrode copper paste and the LTCC substrate.

[0006] In order to accelerate the development of domestic LTCC technology towards low cost and high reliability, and to expedite the localization of key raw materials for LTCC, there is an urgent need in this field to develop copper conductor pastes that are more suitable for co-firing LTCC. Summary of the Invention

[0007] To address the problems mentioned above, this invention starts with the design of glass powder composition and combines it with commercial copper powder to design a high-matching glass powder and high-bonding-strength copper conductor paste for LTCC. By improving the compatibility between the glass powder and the green ceramic of LTCC and forming a dense interface through sintering, high bonding force between the copper paste and the green ceramic is achieved during sintering, thereby meeting the requirements of low cost and high reliability for conductor paste for LTCC.

[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0009] In a first aspect, the present invention provides a glass powder whose chemical composition comprises, by weight percentage, the following components: (15-30%) SiO2-(23-32%) B2O3-(3-9%) Na2O-(0-50%) MO (M = Mn, Ba, Ca). MnO, CaO, and BaO oxides are introduced into the SiO2-B2O3-Na2O system.

[0010] In a second aspect, the present invention provides a copper conductor paste for LTCC, the conductor paste comprising, by weight percentage: 77-90% copper powder, 2-8% glass powder of the present invention, 8-15% organic carrier, and 0-5% additives.

[0011] Thirdly, the present invention also provides a method for preparing a copper electrode paste, comprising the following steps:

[0012] S1. Weigh the solvent and resin, and dissolve the resin evenly in the solvent at 80-90℃, stirring thoroughly to form a uniform organic carrier.

[0013] S2. Weigh out glass powder, copper powder, and the organic carrier prepared in step S1 according to the specified proportions and stir them evenly to form a slurry. Then, use a three-roll mill to thoroughly grind and filter the slurry to finally prepare a copper paste that meets the performance requirements.

[0014] Fourthly, this invention provides a sintering process for LTCC copper conductors. The sintering process includes a debinding process and a sintering process. The debinding process involves heating from room temperature at a rate of 3–5°C / min to 500–650°C and holding at that temperature for 300–400 min, with a wet N2 atmosphere. During the sintering process, the debinding ends at the starting temperature, and the temperature is then increased to 900–950°C at a rate of 10–30°C / min and held for 30–60 min. The sintering atmosphere is N2.

[0015] In a preferred embodiment of the present invention, the glass powder, by mass percentage, comprises the following components: Na₂O 3–9%, CaO 0–16%, BaO 25–40%, MnO 0–10%, B₂O₃ 23–30%, and SiO₂ 16–24%, wherein the sum of the CaO and BaO contents in the glass is greater than 40%. Glass within this elemental range exhibits good sintering activity, good chemical stability, and good adhesion to LTCC substrates.

[0016] As a preferred embodiment of the present invention, copper powder with smaller particle size has higher sintering activity, lower bulk density, and severe shrinkage after sintering. Therefore, the present invention preferably combines spherical copper powder with D50 = 7 μm and D50 = 2 μm with flake copper powder with D50 = 4 μm. When the mass ratio of spherical copper to flake copper is in the range of 1 to 3, dense sintering of the electrode can be achieved.

[0017] In a preferred embodiment of the present invention, the organic carrier comprises 75-85% solvent and 15-25% resin by weight percentage. Preferred solvents include two or more of diethylene glycol butyl ether acetate, dipropylene glycol propyl ether, and terpineol; the resins include one or two of ethyl cellulose and acrylic resin.

[0018] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0019] A glass powder with high compatibility and high chemical stability is provided. MnO, CaO, and BaO oxides are introduced into the SiO2-B2O3-Na2O system to improve the compatibility between the glass powder and LTCC green ceramic, and to enhance the bonding force between the copper paste and the green ceramic during sintering.

[0020] This paper provides a method to enhance interfacial bonding and compatibility. Interfacial bonding is enhanced through diffusion and interfacial alloying. During sintering, Ca and Ba in the glass powder and Ca and Ba in the green ceramic tape undergo interdiffusion, while copper in the copper conductor paste diffuses into the LTCC ceramic tape. After sintering, Cu, Ca, and Ba diffuse from the conductor into the LTCC substrate, thereby improving the bonding strength between the conductor and the LTCC substrate. Manganese exists at the interface between the conductor and the LTCC substrate in the form of Cu-Mn alloy or oxide, further enhancing the interfacial bonding strength and effectively preventing defects such as cracks and fissures at the conductor-substrate interface in acidic or alkaline solutions.

[0021] This invention innovatively employs an integrated debinding and sintering method, solving the problems of difficulty in removing organic carriers from copper paste at low temperatures and easy oxidation during high-temperature sintering. This achieves porosity-controlled sintering at the conductor-LTCC ceramic tape interface. It reduces the phenomenon of poor device electrical performance and decreased reliability caused by sintering mismatch, achieving a dense bond between the electrode and the ceramic body.

[0022] The copper conductor paste prepared by this invention, when applied to LTCC green ceramic tape, exhibits high printing resolution, a smooth, burr-free surface, a flat sintered appearance, and excellent bonding strength performance, with a sheet resistance of less than 2 mΩ / □. It possesses advantages such as low porosity and high sintering density, and shows no defects such as cracks or fissures after acid soaking and cleaning. The LTCC product demonstrates high reliability. Attached Figure Description

[0023] Figure 1 The chemical stability of the glass powders A to C described in Examples 1-3, the copper films A to C sintered in Example 4, and the copper films D to F sintered in Example 5 in solutions with pH = 1, 7, and 13.

[0024] Figure 2 The images show the SEM microstructures of copper films A to C sintered in Example 4 and copper films D to F sintered in Example 5.

[0025] Figure 3 The bonding strength between the copper films A to C sintered in Example 4 and the copper films D to F sintered in Example 5 and the ceramic tape.

[0026] Figure 4 Sheet resistance of copper films A-C sintered in Example 4 and copper films D-F sintered in Example 5. Detailed Implementation

[0027] To better illustrate the objectives, technical solutions, and advantages of this invention, the invention will be further described below with reference to specific embodiments. The described embodiments are merely some examples of the invention. Other embodiments obtained by those skilled in the art based on this invention are also covered within the scope of protection of this invention.

[0027] Unless otherwise specified, all materials and reagents used in the following examples are commercially available.

[0028] Example 1

[0029] A glass powder and copper conductor paste for LTCC and their preparation method

[0030] Design and preparation method of glass powder: The glass component raw materials Na2O, CaO, BaO, MnO, B2O3 and SiO2 powders were weighed in a mass percentage ratio of 4:6:36:5:30:19 and ball-milled to form a uniform solid powder. The powder was placed in a platinum crucible and heated to 1400℃ at a heating rate of 10℃ / min and held for 120min to ensure that the glass raw materials were completely melted into glass liquid. The glass liquid was poured into a two-roll mill for quenching to form glass slag. The glass slag was then subjected to two steps of coarse grinding and fine grinding in a planetary ball mill and passed through a 600-mesh inspection sieve to prepare glass powder A with a D50 particle size of 2.5μm.

[0031] Composition and preparation method of conductor paste: The raw materials are weighed and mixed according to the following proportions: 50% spherical copper A, 10% spherical copper B, 20% flake copper powder, 8% glass powder A, and 12% organic carrier. The paste mixture is then dispersed 5 times using a high-speed planetary disperser. Next, the paste is thoroughly ground 15 times using a three-roll mill, and then filtered through a 600-mesh filter to finally prepare a copper paste that meets the performance requirements.

[0032] Example 2

[0033] A glass powder and copper conductor paste for LTCC and their preparation method

[0034] The glass component raw materials Na2O, CaO, BaO, MnO, B2O3 and SiO2 powders were weighed in a mass percentage ratio of 6:8:36:7:25:18 and ball-milled to form a uniform solid powder. The powder was placed in a platinum crucible and heated to 1300℃ at a heating rate of 10℃ / min and held for 120min to ensure that the glass raw materials were completely melted into glass liquid. The glass liquid was poured into a two-roll mill for quenching to form glass slag. The glass slag was then subjected to two steps of coarse grinding and fine grinding in a planetary ball mill and passed through a 600-mesh inspection sieve to prepare glass powder B with a D50 particle size of 2.5μm.

[0035] Composition and preparation method of conductor paste: The raw materials are weighed and mixed according to the following proportions: 47% spherical copper A, 10% spherical copper B, 30% flake copper powder, 4% glass powder B, and 9% organic carrier. The paste mixture is then dispersed 5 times using a high-speed planetary disperser. Next, the paste is thoroughly ground 15 times using a three-roll mill, and filtered through a 600-mesh filter to finally prepare a copper paste that meets the performance requirements.

[0036] Example 3

[0037] A glass powder and copper conductor paste for LTCC and their preparation method

[0038] The glass component raw materials Na2O, CaO, BaO, MnO, B2O3 and SiO2 powders were weighed in a mass percentage ratio of 9:15:30:7:23:16 and ball-milled to form a uniform solid powder. The powder was placed in a platinum crucible and heated to 1200℃ at a heating rate of 10℃ / min and held for 120min to ensure that the glass raw materials were completely melted into glass liquid. The glass liquid was poured into a two-roll mill for quenching to form glass slag. The glass slag was then subjected to two steps of coarse grinding and fine grinding in a planetary ball mill and passed through a 600-mesh inspection sieve to prepare glass powder with a D50 particle size of 2.5μm.

[0039] Composition and preparation method of conductor paste: The raw materials are weighed and mixed according to the following proportions: 35% spherical copper A, 5% spherical copper B, 40% flake copper powder, 6% glass powder A, and 14% organic carrier. The paste mixture is then dispersed 5 times using a high-speed planetary disperser. Next, the paste is thoroughly ground 15 times using a three-roll mill, and then filtered through a 600-mesh filter to finally prepare a copper paste that meets the performance requirements.

[0040] Example 4

[0042] A sintering process for LTCC copper conductors

[0043] Under a humid nitrogen atmosphere, the adhesive is discharged from 200℃ at a heating rate of 5℃ / min to 550-600℃ and held for 400min. After discharge, the temperature is increased to 900-920℃ at a heating rate of 30℃ / min and held for 60min.

[0044] Example 5

[0045] A sintering process for LTCC copper conductors

[0046] Under a humid nitrogen atmosphere, the adhesive is removed from 200℃ at a heating rate of 5℃ / min to 600-650℃ and held for 400min. After removal, the temperature is increased to 920-950℃ at a heating rate of 30℃ / min and held for 60min.

[0047] Copper paste usage and testing methods

[0048] Printing and Drying: The prepared copper paste was printed on an LTCC substrate by screen printing and dried in an oxygen-rich environment at 120-140°C for 20-40 minutes. Then, the paste was debonded and sintered using the sintering process described in Examples 4-5 to form a film with a thickness of 25±1μm.

[0048] Electrical performance testing: The electrical properties of the sintered copper film were measured using a four-probe resistance meter. In this invention, sheet resistance represents the resistance between two opposite sides of a square thin-film conductive material.

[0049] Adhesion test: The sintered electrode substrate was plated with nickel and tin layers in the electroplating solution, and then soldered with lead-free solder paste and reflow soldered three times. The adhesion test was completed on a universal mechanical testing machine.

[0050] Acid resistance test of glass: Glass powder was basically sintered into a button shape, then placed in a container with pH=1, 7, or 13 and heated to 90°C for 90 minutes. After immersion, the surface was cleaned with anhydrous ethanol. After the substrate dried, the masses W1 and W2 before and after immersion were weighed using a balance. Weight loss within 5% is considered acceptable. Then, SEM is used to observe the morphology for the presence of microcracks.

[0051] Copper film chemical stability test: The sintered substrate was immersed in a solution heated to 90°C at pH = 1, 7, and 13 for 90 minutes. The surface was then cleaned with anhydrous ethanol. After the substrate dried, the masses W1 and W2 before and after immersion were measured using a balance. Weight loss within 5% is considered acceptable. Then, use 3M tape to attach the electrode substrate and observe whether the electrodes detach.

[0052] In summary, this invention provides a high-compatibility glass powder and high-bonding-strength copper conductor paste for LTCC, its preparation method, and its application. By improving the compatibility between the glass powder and the green ceramic of LTCC and sintering to form a dense interface, high bonding strength between the copper paste and the green ceramic is achieved during sintering, thereby meeting the requirements of low cost and high reliability for conductor pastes used in LTCC.

[0053] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. By referring to the embodiments of the present invention, those skilled in the art can make various modifications to these embodiments without creative effort. Therefore, improvements and modifications made by those skilled in the art without departing from the principles of the present invention should be within the scope of protection of the present invention.

Claims

1. Highly matching glass powder and copper conductor paste for LTCC and their preparation method and application, It is characterized in that Glass powder contains the following components by weight percentage (15~30%) SiO 2 -(23~32%)B 2 O 3 -(3~9%)Na 2 O-(0~50%)MO(M=Mn,Ba,Ca).

2. The glass powder according to claim 1, It is characterized in that The glass blocks were prepared by conventional melting and quenching in a double-roll sheet mill, and the glass powder was prepared by planetary ball milling with a D50 particle size of 1.0-3.5 mm.

3. The method for preparing the glass powder according to claim 2, It is characterized in that In the process of sintering the raw material solid powder into glass liquid, the heating rate is 5-20°C / min, the sintering temperature is 1000-1400°C, and the sintering time is 60-150min; in the process of ball milling, a ball mill is used for ball milling, the ball mill speed is 300-500r / min, and the ball milling time is 90-240min; in the process of screening, the mesh size of the sieve is 200-800 meshes.

4. The electronic paste according to claim 1, It is characterized in that The slurry comprises 77-90 wt% of copper powder, 2-8 wt% of glass powder, 8-21 wt% of organic carrier, and 0-5 wt% of additives, wherein the copper powder is a mixture of spherical copper powder, spherical copper A, and B, and the D50 particle size is 2-8 μm. The additives are two or three of castor oil, lecithin, N-oleoylsarcosine, and polyamide.

5. The electronic paste according to claim 1, It is characterized in that The organic carrier comprises a solvent and a resin. The solvent comprises two or more of butyl carbitol acetate, alcohol ester-12, dipropylene glycol propyl ether, diethylene glycol butyl ether acetate, and terpineol; and the resin comprises one or two of ethyl cellulose, epoxy resin, and acrylic resin.

6. The electronic paste according to claim 1, It is characterized in that The preparation process includes the following three steps: S61, weighing a solvent and a resin, uniformly dissolving the resin in the solvent at 80-90° C., and fully stirring to form a uniform organic carrier; S62, weighing glass powder, copper powder and the organic vehicle prepared in step S21 in proportion and stirring them evenly to form a slurry. Then, fully grind the slurry with a three-roll mill; S63. Use a vacuum filter or filter (400-800 mesh) to filter the slurry, and finally prepare a copper slurry that meets the performance requirements.

7. The electronic paste according to claim 1, It is characterized in that The sintering process includes the debinding process and the sintering process. The debinding process is to increase the temperature from room temperature at a rate of 3-5 °C / min to 500-650 °C and keep it for 300-400 min. The sintering process is to increase the temperature from room temperature at a rate of 10-30 °C / min to 900-950 °C and keep it for 30-60 min. The sintering atmosphere is N 2 or wet N 2 .

8. The application scenario of the glass powder according to claim 1 is not limited to LTCC copper conductor paste, and high matching can be achieved in the fields of MLCC, chip resistors, inductors, etc.

Citation Information

Patent Citations

  • Inner electrode copper paste for low-temperature co-fired ceramic, and preparation method and application thereof

    CN112509727A

  • Conductive silver paste for low-temperature co-fired ceramic surface electrode and preparation method of conductive silver paste

    CN115691855A

  • Surface electrode slurry for LTCC (Low Temperature Co-Fired Ceramic) and preparation method thereof

    CN116344099A

  • Paste for conductor, glass ceramic substrate and electronic component module

    JP2012221765A

  • Printable copper external electrode slurry for MLCC (multilayer ceramic capacitor)

    CN115188589A