Anti-reflection liquid for glass surface of photovoltaic module as well as preparation method and application of anti-reflection liquid
The anti-reflection liquid of mesoporous silica microspheres and rhamnolipid pre-impregnated nano-titanium dioxide is prepared by biological enzymes, which solves the problem of the stability of the anti-reflection film on the surface of photovoltaic glass in harsh environments and achieves efficient light transmittance and Long life reduces costs and maintenance requirements.
Patent Information
- Application Number
- CN202410881550.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-29
AI Technical Summary
The anti-reflection coating on the surface of existing photovoltaic glass is prone to falling off, bubbling, and discoloration in high temperature, high humidity or high temperature difference environments, affecting its optical performance and service life, and the preparation cost is high.
It uses bioenzyme mesoporous silica microspheres and rhamnolipid pre-impregnated nano titanium dioxide as the main component of the anti-reflection liquid. By adjusting the nanoparticle accumulation and void volume ratio, the effective refractive index of the film is increased, forming a stain-resistant and weather-resistant form. film layer.
It significantly improves the power generation efficiency and service life of photovoltaic modules, reduces cleaning and maintenance costs, and maintains good dirt resistance in polluted environments. The anti-reflection rate is increased by more than 4%, and the power generation gain is more than 8%.
Smart Images

Figure CN118851583A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanomaterials, and in particular is a permeability-enhancing liquid used for the glass surface of a photovoltaic module, and a preparation method and application thereof. Background Art
[0002] Today, my country has become the world's largest producer of photovoltaic industry. However, there are still some obstacles to the development of solar power generation. One of the main problems is how to improve the efficiency of solar power generation and reduce the cost. To solve this problem, reducing the reflection of photovoltaic glass to sunlight and improving the transmittance are the main research directions. The current direction mainly focuses on coating a layer of anti-reflection film on the surface of photovoltaic glass to reduce the reflection of sunlight.
[0003] Anti-reflection film, also known as anti-reflection film, is applied to the surface of the material to reduce reflection. As an optical coating, it is widely used in various optical devices. Anti-reflection film can effectively increase the transmittance of sunlight on photovoltaic cover glass, thereby improving the power generation efficiency of solar cells and increasing the power generation of components. Thus, the power generation can be increased at a lower cost. There are many methods for coating the surface of solar photovoltaic glass, such as evaporation or sputtering. The performance-price ratio of these two methods is not ideal and the cost is high. The sol-gel process has the advantages of simple process control and good anti-reflection performance of thin films. It has a series of advantages such as low coating cost, simple coating, easy cleaning, easy large-area film formation and good optical performance, and has attracted much attention. ZnS, TiO2, ZrO2, ZnS, Al2O3, SiO2 and MgF2 are often used as anti-reflection materials. As a coating material, the preparation method of SiO2 thin film is simple, which can effectively reduce the refractive index and has obvious anti-reflection effect. However, there are a large number of hydroxyl groups on the surface of SiO2 films prepared by the sol-gel method, which easily adsorb pollutants and reduce the transmittance and service life.
[0004] Existing anti-reflection films, whether single-layer anti-reflection films or two-layer / multi-layer composite anti-reflection films, have certain deficiencies to a greater or lesser extent. For example, problems such as shedding, bubbling, and discoloration may occur under high temperature and high humidity or high temperature difference. Under long-term use or in harsh environments, the anti-reflection film may be worn or discolored, affecting its optical performance and service life.
[0005] Therefore, there is an urgent need in the art for an anti-reflection liquid for the glass surface of photovoltaic modules with better anti-reflection rate and longer service life, so as to obtain a higher power generation rate. Summary of the invention
[0006] The purpose of the present invention is to provide a permeability-enhancing liquid for the glass surface of a photovoltaic module, and a preparation method and application thereof. The permeability-enhancing liquid of the present invention adopts mesoporous silica microspheres prepared by bio-enzymes and nano-titanium dioxide pre-impregnated with rhamnolipid as main components, and utilizes the volume ratio of voids and the accumulation of different nanoparticles to adjust the effective refractive index of the permeability-enhancing liquid film, so that its overall permeability-enhancing rate is significantly increased, thereby greatly improving the power generation efficiency of solar cells.
[0007] The invention discloses an anti-permeability liquid for the surface of photovoltaic module glass, which is composed of the following components in parts by weight: 0.1 to 3 parts of rhamnolipid pre-impregnated nano titanium dioxide, 1 to 5 parts of mesoporous silica microspheres prepared by biological enzymes, 10 to 80 parts of deionized water, 0.1 to 2 parts of defoaming agent, and 1 to 20 parts of alcohol solvent.
[0008] The rhamnolipid pre-impregnated nano-titanium dioxide is obtained by immersing nano-titanium dioxide in rhamnolipid for infiltration treatment; specifically, nano-titanium dioxide with a particle size of 3 to 50 nm and a crystal form of anatase is immersed in rhamnolipid for 30 to 60 minutes. The bio-enzyme-made mesoporous silica microspheres are obtained by the following preparation method: after the polymer microsphere colloid, soluble starch, solvent, and modifier are mixed, a grafting reaction is carried out, and after gelatinization, impurities and solvents are removed by vacuuming at low temperature to obtain starch grafted modified microspheres; silicon source solution is added dropwise to the starch grafted modified microspheres, and the silicon source is adsorbed on the surface of the starch grafted modified microspheres by stirring; the reaction is stirred at a temperature of 40°C to 60°C and a speed of 80 to 200 rpm for 6 to 18 hours, and the silicon source undergoes a gelation reaction to form a silica shell layer; amylase is added to remove the template to obtain nano-scale mesoporous silica microspheres, and the diameter of the microspheres is 5 to 200 nanometers. The defoamer can be an aqueous defoamer containing mineral oil, silicone, polysiloxane, ethylene bis stearamide (EBS), paraffin, ester wax. The alcohol solvent can be an alcohol organic solvent such as methanol, ethanol, ethylene glycol, isopropanol, and a blend thereof.
[0009] Specifically, the bio-enzyme-made mesoporous silica microspheres are obtained by the following preparation method:
[0010] (1) Preparation of starch grafted modified microspheres: 50 parts of polymer microsphere colloid, 10 parts of soluble starch, 10-15 parts of solvent, and 0.5-5 parts of modifier are added into a reaction vessel and stirred to form a mixture; in a microwave synthesis / extraction device, the temperature is kept at 30°C to 80°C to graft the starch with the polymer; after the mixture is gelatinized, the temperature is lowered to 40°C and low-temperature vacuum is applied to remove small molecular impurities and solvent to obtain starch grafted modified microspheres.
[0011] (2) Adding silicon source solution to the treated starch grafted modified microspheres: adsorbing silicon source on the surface of starch grafted modified microspheres by stirring; controlling the weight ratio of silicon dioxide theoretical content to starch grafted modified microspheres to be 2:1 to 3.5:1, controlling the solid content of the reaction system by deionized water, and controlling the solid content to be less than 20% of the reaction system. The silicon source solution can be commercially available silica sol, sodium silicate solution or sodium silicate, tetraethyl silicate hydrolyzate, etc.
[0012] (3) Gelation: The reaction is stirred at 40°C to 60°C and 80 to 200 rpm for 6 to 18 hours, and the silicon source undergoes a gelation reaction to form a silica shell. The reaction ends when the system viscosity no longer changes.
[0013] (4) Removal of template: Add amylase, stir at 36°C to 40°C at 20 to 60 rpm for 24 to 48 hours to degrade starch, then add deionized water and stir at high speed to elute the starch decomposition products, decompose and embrittle the polymer microspheres into smaller pieces, and remove the silicon oxide. After several separations and elutions by centrifuge, nano-scale mesoporous silica microspheres can be obtained. The diameter of the obtained microspheres is 5 to 200 nanometers.
[0014] The present invention also provides a method for preparing the permeability-enhancing liquid for the surface of photovoltaic module glass: taking half of the deionized water in the formula, adding in sequence about half of the alcohol solvent, the whole amount of rhamnolipid pre-impregnated nano-titanium dioxide, the whole amount of enzyme-made mesoporous silica microspheres, and the whole amount of defoaming agent, stirring evenly at a speed of 1000 to 20000 rpm with a high-speed disperser, and finally slowly adding the remaining deionized water and alcohol solvent at a speed of 200 to 800 rpm with a paddle disperser, and stirring evenly.
[0015] The invention also provides an application of an anti-permeability liquid for the glass surface of a photovoltaic module. The anti-permeability liquid of the invention can be used in a photovoltaic power station and directly sprayed on the photovoltaic module to form a film layer, thereby increasing power generation gain and reducing cleaning and maintenance costs.
[0016] The anti-reflection liquid of the present invention can be used to prepare high anti-reflection solar glass, specifically, any coating method among spraying, dipping, pulling, roller coating, spin coating, flow coating or brush coating is adopted, and the anti-reflection liquid is coated on the cleaned and dried solar cell encapsulation glass substrate, and the high anti-reflection solar glass is obtained after the surface is dried.
[0017] The present invention has the following beneficial effects:
[0018] 1. The anti-reflection liquid of the present invention is coated on the photovoltaic glass plate to make the photovoltaic glass have anti-reflection and anti-fouling properties. The formed nano coating uses the volume ratio of voids and the accumulation of different nanoparticles to adjust the effective refractive index of the film, thereby increasing its overall anti-reflection rate.
[0019] Experiments show that the photovoltaic module glass can increase the light transmittance of the glass by more than 4% on average within the wavelength range of 380 to 1100 nm after being coated with the anti-permeability liquid of the present invention, and the film layer can maintain the anti-fouling performance of the photovoltaic module for a long time. Compared with the uncoated photovoltaic module, after the anti-permeability liquid is used to form a film layer on the surface of the photovoltaic module glass, the coated photovoltaic module can generate an additional gain of more than 4%. More prominently, the anti-permeability liquid of the present invention has good anti-fouling properties. Experiments show that the photovoltaic module coated with the anti-permeability liquid of the present invention can generate an additional gain of more than 8% in a polluted environment.
[0020] 2. The preparation process is more environmentally friendly and has lower costs. The present invention prepares mesoporous silica microspheres through an original method of preparing mesoporous silica by decomposing mesoporous silica using biological enzymes. Environmentally friendly and easily degradable starch is used as a pore-forming agent. After forming a silica shell, the starch is decomposed into a series of intermediates and final products such as carbon dioxide and water by amylase. Finally, impurities can be separated by simple washing to obtain pure nano-scale mesoporous silica microspheres. This process is green and environmentally friendly, consumes very little energy, has little three wastes, has a mild reaction, and produces efficient and pure products.
[0021] 3. Good stability. It is not easy to fall off, bubble, discolor and other problems in high temperature, high humidity, high temperature difference and acidic environment. The anti-reflection film is not easy to wear or discolor in long-term use or harsh environment, which prolongs the optical performance and service life. Weather resistance index tests include heat cycle test, humidity and heat test, UV test, acid test and other test results are excellent.
[0022] The invention is an original biological enzyme-prepared nano-scale mesoporous silica microsphere, which has a dense structure and uniform particle size, increases the adhesion performance on the glass and reduces shedding. In addition, the nano-scale silica microsphere has a low reflectivity, and can effectively improve the light transmittance and photocatalytic activity when mixed with rhamnolipid pretreated titanium oxide particles, increase the compatibility with biological enzyme-prepared mesoporous silica, and can simultaneously meet the anti-reflection and self-cleaning properties of the anti-reflection film, make the cured film layer more dense, and improve chemical stability and durability.
[0023] The anti-permeability liquid prepared by the method of the present invention can be coated on the photovoltaic glass plate and can form a flat and dense film layer by self-drying at room temperature. The film layer has good adhesion to the surface of the photovoltaic glass. The film layer not only has high light transmittance, but also has excellent self-cleaning performance, thereby achieving long-term anti-fouling performance, thereby increasing the power generation of the photovoltaic module and greatly reducing the cleaning and maintenance costs of the photovoltaic module. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a SEM image (×100k) of the glass surface coating after coating the permeability-enhancing liquid of the present invention in Experimental Example 1.
[0025] Figure 2This is a SEM image (×30k) of the cross section of the glass after coating with the permeability-enhancing liquid of the present invention in Experimental Example 1; the upper part of the image is the permeability-enhancing liquid layer and the lower part is the photovoltaic glass. DETAILED DESCRIPTION
[0026] The present invention is further described below with reference to specific examples. Unless otherwise specified, the compounds described in the present invention are generally used in the art or are commercially available products; the methods described are generally used in the art unless otherwise specified.
[0027] Example 1: A permeability-enhancing liquid for the glass surface of a photovoltaic module, comprising the following components in parts by weight: 1 part of rhamnolipid pre-impregnated nano-titanium dioxide, 1 part of mesoporous silica microspheres prepared by bio-enzyme, 80 parts of deionized water, 0.1 part of BYK-28 (defoaming agent), 10 parts of ethanol, and 8 parts of isopropanol.
[0028] The preparation method is as follows:
[0029] 1. Preparation of rhamnolipid pre-impregnated nano-titanium dioxide: Take 50g of nano-titanium dioxide with an average particle size of 20nm and anatase crystal form, and immerse it in 300g of rhamnolipid at room temperature for 40 minutes to obtain rhamnolipid pre-impregnated nano-titanium dioxide. The rhamnolipid should at least immerse the nano-titanium dioxide. Drain and set aside.
[0030] 2. Preparation of mesoporous silica microspheres made by bio-enzyme:
[0031] (1) Preparation of starch grafted modified microspheres: 50 g polymer microspheres (ThermoScientific TM 5000 series 0.03 μm polymer particle suspension, the total solid content is regulated to 8%), 10g soluble corn starch, and then add 10g DMF, 0.5g maleic anhydride and stir evenly to form a mixture; in a microwave synthesis / extraction instrument, the microwave constant temperature is controlled at 60°C, and the magnetic stirring rate is controlled at 120rpm. After 2h, the temperature is lowered to 40°C for low-temperature vacuum removal of small molecular impurities and various solvents to obtain starch grafted modified microspheres.
[0032] (2) Adding sodium silicate solution to the starch grafted modified microspheres of step (1), and adsorbing the silicon source on the surface of the starch grafted modified microspheres at a stirring rate of 150 rpm. The weight ratio of the theoretical content of silicon dioxide to the starch grafted modified microspheres is calculated based on the content of the sodium silicate solution and controlled at 3:1. The solid content of the system is controlled to be 18% by deionized water.
[0033] (3) Gelation: The reaction was stirred at 40°C and 150 rpm for 10 h, and the silicon source was gelled to form a silica shell. This step of the reaction was monitored by a rotational viscometer, and the end point was when the viscosity of the system no longer changed.
[0034] (4) Template removal: Add amylase, stir at 50 rpm at 36°C for 48 h, then add 200 g of deionized water and stir at 5000 rpm for 1 min, elute the solution through a centrifuge, and repeat twice. Nano-scale mesoporous silica microspheres can be obtained. The diameter of the microspheres is 5 to 200 nanometers, and the average particle size is about 10 to 50 nm.
[0035] 3. Prepare the permeability-enhancing liquid: take half of the deionized water in the formula, add about half of the alcohol solvent, the whole amount of rhamnolipid pre-impregnated nano-titanium dioxide, the whole amount of enzyme-made mesoporous silica microspheres, and the whole amount of defoaming agent in turn, stir evenly with a high-speed disperser at a speed of 15000rpm, and finally slowly add the remaining deionized water and alcohol solvent at a speed of 300rpm of a paddle disperser and stir evenly.
[0036] The properties of the permeability-enhancing liquid prepared in this example are: light blue transparent liquid, with a viscosity of 0.936 mPa·s at 25° C. and a pH value of neutral.
[0037] Example 2: A permeability-enhancing liquid for the glass surface of a photovoltaic module, comprising the following components in parts by weight: 0.5 parts of rhamnolipid pre-impregnated nano-titanium dioxide, 4 parts of mesoporous silica microspheres prepared by bio-enzyme, 76 parts of deionized water, 0.2 parts of BYK-28 (defoaming agent), 8 parts of ethanol, and 12 parts of isopropanol.
[0038] The preparation method is as follows:
[0039] 1. Preparation of rhamnolipid pre-impregnated nano-titanium dioxide: Take 50g of nano-titanium dioxide with an average particle size of 10nm and anatase crystal form, and immerse it in 300g of rhamnolipid at room temperature for 30 minutes to obtain rhamnolipid pre-impregnated nano-titanium dioxide. The rhamnolipid should at least immerse the nano-titanium dioxide. Drain and set aside.
[0040] 2. Preparation of mesoporous silica microspheres made by bio-enzyme:
[0041] (1) Preparation of starch grafted modified microspheres: 50 g polymer microspheres (ThermoScientific TM 5000 series 0.03 μm polymer particle suspension, the total solid content is regulated to 8%), 10g soluble corn starch, 10g DMF, 0.5g maleic anhydride are added and stirred evenly into a mixture; in a microwave synthesis / extraction instrument, the microwave constant temperature is 60°C, the magnetic stirring rate is controlled to 120rpm, after 2h, the temperature is lowered to 40°C for low-temperature vacuum removal of small molecular impurities and solvents, and starch grafted modified microspheres are obtained.
[0042] (2) Adding sodium silicate solution to the starch grafted modified microspheres of step (1), and adsorbing the silicon source on the surface of the starch grafted modified microspheres at a stirring rate of 150 rpm. The weight ratio of the theoretical content of silicon dioxide to the starch grafted modified microspheres is calculated to be 2:1 based on the content of the sodium silicate solution, and the solid content of the reaction system is controlled to be 18% by deionized water.
[0043] (3) Gelation: The reaction was stirred at 50°C and 150 rpm for 6 hours, and the silicon source underwent gelation to form a silica shell. This step of the reaction was monitored by a rotational viscometer, and the end point was when the system viscosity no longer changed.
[0044] (4) Template removal: Add amylase, stir at 40 rpm for 40 h at 37 °C, then add 200 g of deionized water and stir at 5000 rpm for 1 min. Elute the solution through a centrifuge, repeat twice. Nano-scale mesoporous silica microspheres with a diameter of 5 to 200 nanometers and an average particle size of about 10 to 50 nm can be obtained.
[0045] 3. Prepare the permeability-enhancing liquid: take half of the deionized water in the formula, add about half of the alcohol solvent, the whole amount of rhamnolipid pre-impregnated nano-titanium dioxide, the whole amount of enzyme-made mesoporous silica microspheres, and the whole amount of defoaming agent in turn, stir evenly with a high-speed disperser at a speed of 15000rpm, and finally slowly add the remaining deionized water and alcohol solvent at a speed of 300rpm of a paddle disperser and stir evenly.
[0046] The properties of the permeability-enhancing liquid prepared in this example are: a light blue transparent liquid, a viscosity of 0.992 mPa·s at 25° C., and a pH value of neutral.
[0047] Example 3: A permeability-enhancing liquid for the glass surface of a photovoltaic module, composed of the following components in parts by weight: 2 parts of rhamnolipid pre-impregnated nano-titanium dioxide, 2 parts of mesoporous silica microspheres prepared by bio-enzyme, 78 parts of deionized water, 0.3 parts of BYK-28 (defoaming agent), 2 parts of ethylene glycol, 10 parts of ethanol, and 6 parts of isopropanol.
[0048] The preparation method is as follows:
[0049] 1. Preparation of rhamnolipid pre-impregnated nano-titanium dioxide: Take 50g of nano-titanium dioxide with an average particle size of 50nm and anatase crystal form, and immerse it in 300g of rhamnolipid for 60 minutes to obtain rhamnolipid pre-impregnated nano-titanium dioxide. The rhamnolipid should at least immerse the nano-titanium dioxide. Drain and set aside.
[0050] 2. Preparation of mesoporous silica microspheres made by bio-enzyme:
[0051] (1) Preparation of starch grafted modified microspheres: 50 g of polymer microspheres (polystyrene microparticle suspension, 0.05 μm, total solid content controlled to 6%), 10 g of soluble cassava starch, 8 g of DMF, and 0.4 g of maleic anhydride were added into a reaction container and stirred to form a mixture; in a microwave synthesis / extraction apparatus, the microwave constant temperature of the mixture was controlled at 50° C., and the magnetic stirring rate was controlled at 80 rpm. After 1.5 h, the mixture was cooled to 40° C. and vacuumed at low temperature to remove small molecular impurities and various solvents to obtain starch grafted modified microspheres.
[0052] (2) Adding sodium silicate solution to the starch grafted modified microspheres of step (1), and adsorbing the silicon source on the surface of the starch grafted modified microspheres at a stirring rate of 100 rpm. The weight ratio of the theoretical content of silicon dioxide to the starch grafted modified microspheres is calculated to be 3.5:1 based on the content of the sodium silicate solution, and the solid content of the system is controlled to be 16% by deionized water.
[0053] (3) Gelation: The reaction was stirred at 45°C and 120 rpm for 5 h, and the silicon source was gelled to form a silica shell. This step of the reaction was monitored by a rotational viscometer, and the end point was when the viscosity of the system no longer changed.
[0054] (4) Template removal: Add amylase, stir at 60 rpm at 36°C for 36 h, then add 200 g of deionized water and stir at 4000 rpm for 1 min. Elute the solution through a centrifuge, repeat 3 times. Nano-scale mesoporous silica microspheres can be obtained. The diameter of the microspheres is 5 to 200 nanometers, and the average particle size is about 15 to 80 nm.
[0055] 3. Prepare the permeability-enhancing liquid: take half of the deionized water in the formula, add about half of the alcohol solvent, the whole amount of rhamnolipid pre-impregnated nano-titanium dioxide, the whole amount of enzyme-made mesoporous silica microspheres, and the whole amount of defoaming agent in turn, stir evenly with a high-speed disperser at a speed of 12000rpm, and finally slowly add the remaining deionized water and alcohol solvent at a speed of 200rpm with a paddle disperser and stir evenly.
[0056] The properties of the permeability-enhancing liquid prepared in this example are: a light blue transparent liquid, a viscosity of 0.992 mPa·s at 25° C., and a pH value of neutral.
[0057] Example 4: A permeability-enhancing liquid for the glass surface of a photovoltaic module, composed of the following components in parts by weight: 3 parts of rhamnolipid pre-impregnated nano-titanium dioxide, 1 part of mesoporous silica microspheres prepared by bio-enzyme, 80 parts of deionized water, 0.1 part of Dow Corning DC-65 (defoaming agent), 4 parts of ethylene glycol, 10 parts of ethanol, and 2 parts of isopropanol.
[0058] The preparation method is as follows:
[0059] 1. Preparation of rhamnolipid pre-impregnated nano-titanium dioxide: Take 50g of nano-titanium dioxide with an average particle size of 40nm and anatase crystal form, immerse it in 300g of rhamnolipid for 55 minutes to obtain rhamnolipid pre-impregnated nano-titanium dioxide. The rhamnolipid should at least immerse the nano-titanium dioxide. Drain and set aside.
[0060] 2. Preparation of mesoporous silica microspheres made by bio-enzyme:
[0061] (1) Preparation of starch grafted modified microspheres: 50 g of polymer microspheres (commercially available or homemade polystyrene microparticle suspension, 0.05 um, total solid content controlled to 6%) and 10 g of soluble cassava-derived starch were added to a reaction container, and 8 g of DMF and 0.4 g of maleic anhydride were added and stirred to form a mixture; in a microwave synthesis / extraction device, the microwave constant temperature of the mixture was controlled at 50° C., and the magnetic stirring rate was controlled at 80 rpm. After 1.5 h, the mixture was cooled to 40° C. and low-temperature vacuum was performed to remove small molecular impurities and various solvents to obtain starch grafted modified microspheres.
[0062] (2) tetraethyl silicate was added dropwise to the starch grafted modified microspheres of step (1), and the silicon source was adsorbed on the surface of the starch grafted modified microspheres at a stirring rate of 100 rpm. The weight ratio of the theoretical content of silicon dioxide to the starch grafted modified microspheres was calculated based on the content of tetraethyl silicate and controlled at 2.5:1. The solid content of the system was controlled to be 16% by deionized water.
[0063] (3) Gelation: The reaction was stirred at 45°C and 120 rpm for 5 h, and the silicon source was gelled to form a silica shell. This step of the reaction was monitored by a rotational viscometer, and the end point was when the viscosity of the system no longer changed.
[0064] (4) Template removal: Add amylase, stir at 60 rpm at 36°C for 36 h, then add 200 g of deionized water and stir at 4000 rpm for 1 min, and elute the solution through a centrifuge. Repeat 3 times. Nano-scale mesoporous silica microspheres can be obtained. The diameter of the microspheres is 5 to 200 nanometers. The average particle size is about 15-60 nm.
[0065] 3. Prepare the permeability-enhancing liquid: take half of the deionized water in the formula, add about half of the alcohol solvent, the whole amount of rhamnolipid pre-impregnated nano-titanium dioxide, the whole amount of enzyme-made mesoporous silica microspheres, and the whole amount of defoaming agent in turn, stir evenly with a high-speed disperser at a speed of 12000rpm, and finally slowly add the remaining deionized water and alcohol solvent at a speed of 200rpm with a paddle disperser and stir evenly.
[0066] The properties of the permeability-enhancing liquid prepared in this example are: a light blue transparent liquid, a viscosity of 0.992 mPa·s at 25° C., and a pH value of neutral.
[0067] Experimental Example 1: Performance Test
[0068] 1. SEM detection of the permeability-enhancing liquid coating of the present invention
[0069] The permeability enhancement liquid was coated on a 3.2 mm thick transparent glass with a soft silicone scraper. After natural drying, a film layer of about 600 nm was formed, and an electron microscope scan was performed. The permeability enhancement liquid plane SEM image is shown in Figure 1 , SEM image of glass cross section is shown in Figure 2 .
[0070] Scanning the images shows that the permeability-enhancing liquid of the present invention can be coated on a photovoltaic glass plate and then dried at room temperature to form a smooth and dense film layer.
[0071] 2. Test of light transmittance of the anti-reflection liquid coating of the present invention applied to low-iron ultra-clear patterned glass
[0072] Sample description: The permeability enhancement liquid of the present invention is coated on a 3.2 mm thick low-iron ultra-white embossed glass using soft silica gel. After drying at room temperature (26° C.), the coating thickness is about 600 nm.
[0073] Test conditions: Test environment: (23±2)℃, (50±5)%RH
[0074] Test method: After the coating is dry, place the sample at the measuring hole for measurement until the data is stable and no longer fluctuates, and measure 5 different positions within the predetermined range to obtain 5 stable values.
[0075] Test results: The transmittance comparison test results of 5 positions of low-iron ultra-clear embossed glass before and after coating are shown in Table 1.
[0076] Table 1 Comparative test results of light transmittance at 5 positions of low iron ultra-clear patterned glass before and after coating
[0077]
[0078]
[0079] From the data in the above table, it can be seen that the anti-reflection coating formed by coating the anti-reflection liquid of the present invention on the low-iron ultra-white embossed glass has an obvious anti-reflection effect in the visible light band, with a visible light transmittance of 3-6% and an average value greater than 4%.
[0080] In addition, in order to obtain authoritative data, samples were sent to the National Photovoltaic Product Inspection and Certification Center for inspection. Tests by the National Inspection Center showed that the overall visible light transmittance after coating with the anti-reflection liquid of the present invention was greater than 4%, which was basically consistent with the laboratory data of the inventor.
[0081] 3. Water contact angle test of the anti-permeability liquid coating of the present invention applied to low-iron ultra-white patterned glass
[0082] Sample description: The permeability enhancement liquid of the present invention is coated on a 3.2 mm thick low-iron ultra-white embossed glass using soft silica gel. After drying at room temperature (26° C.), the coating thickness is about 600 nm.
[0083] Test conditions: Test environment: (23±2)℃, (50±5)%RH
[0084] Test method: After the coating is dry, measure the water contact angle at 5 different locations within the predetermined range.
[0085] Test results: The water contact angle results at 5 locations of the low-iron ultra-white embossed glass after coating are shown in Table 2.
[0086] Table 2 Water contact angles at five positions of low iron ultra-white patterned glass after coating
[0087] Position 1 Position 2 Location 3 Position 4 Location 5 Water contact angle 6.1° 5.5° 5.2° 6.5° 5.9°
[0088] Table 2 shows that the water contact angle of the glass coated with the permeability-enhancing liquid of the present invention is between 5.2° and 6.5°, indicating that the permeability-enhancing liquid of the present invention is hydrophilic.
[0089] In addition, in order to obtain authoritative data, the National Photovoltaic Product Inspection and Certification Center was used for inspection. The hydrophilic angle test value in the report is basically consistent with the laboratory data of the present invention.
[0090] 4. Weathering resistance index test of the anti-permeability liquid coating of the present invention applied to low-iron ultra-white embossed glass
[0091] Weather resistance index tests include heat cycle resistance test, humidity and heat resistance test, UV resistance test, and acid resistance test.
[0092] 4.1 Heat cycle test
[0093] Test conditions and results are shown in Table 3:
[0094] Table 3 Thermal cycle test conditions and test results
[0095]
[0096] From the heat-resistant cycle test results in Table 3, it can be seen that the film layer has no obvious shedding, peeling and wrinkling after the heat-resistant cycle, and the attenuation of the effective transmittance of sunlight before and after the heat-resistant cycle is 0.5-0.6, which is less than 1%, indicating that the heat-resistant cycle performance of the anti-permeability liquid coating of the present invention is good.
[0097] 4.2 Heat and humidity resistance test
[0098] Test conditions and results are shown in Table 4:
[0099] Table 4 Moisture and heat resistance test conditions and test results
[0100]
[0101] Table 4 shows the results of the moisture and heat resistance test. After the moisture and heat treatment, the film layer has no obvious shedding, peeling, or wrinkling. The attenuation of the effective transmittance of sunlight before and after the moisture and heat resistance test is 0.6, which is less than 1%, indicating that the moisture and heat resistance performance of the anti-permeability liquid coating of the present invention is good.
[0102] 4.3 UV resistance test
[0103] Test conditions and results are shown in Table 5:
[0104] Table 5 UV resistance test conditions and test results
[0105]
[0106] From the UV resistance test results in Table 5, it can be seen that the film layer has no obvious shedding, peeling and wrinkling after UV irradiation treatment, and the effective transmittance of sunlight before and after the UV resistance test is attenuated to 0.2, which is far lower than 1%, indicating that the anti-permeability liquid coating of the present invention has significant UV resistance.
[0107] 4.4 Acid resistance test
[0108] Test conditions and results are shown in Table 6:
[0109] Table 6 Acid resistance test conditions and test results
[0110]
[0111] From the acid resistance test results in Table 6, it can be seen that the film layer has no obvious shedding, peeling and wrinkling after being immersed in the acid solution. The attenuation of the effective transmittance of sunlight before and after the acid resistance test is 0.2-0.3, which is far lower than 1%, indicating that the permeability-enhancing liquid coating of the present invention has significant acid resistance.
[0112] Experimental Example 2: Application test of the components of the present invention
[0113] The specific method is: communicate and cooperate with the component factory and the glass factory, and the glass factory provides 12 pieces of low-iron ultra-white tempered bare glass that are not coated with any material. The glass size is the conventional version of the cooperative component factory (2272×1128mm). The component factory invests in completely consistent raw materials, uses 10 of the 12 pieces of glass to produce 10 test components, and tests the relevant electrical performance parameters. After cleaning the surface of these 10 components, apply the anti-reflection self-cleaning liquid of the present invention, and test the electrical performance parameters of the 10 components again. In both tests, each component is tested three times in a row, and the average value is taken as the final test result. The final test power and increase ratio are shown in Table 7:
[0114] Table 7 Comparative test results of electrical performance parameters of photovoltaic modules before and after coating
[0115]
[0116] It can be judged from the data in Table 7 that the application effect of the anti-reflection liquid coating of the present invention on the anti-reflection of photovoltaic modules meets expectations and is basically consistent with the transmittance data of laboratory tests. The above-mentioned components adopt a manual coating process. Although the consistency of the effect needs to be further improved, it also proves that the anti-reflection liquid of the present invention has great application space. The uniformity problem of the anti-reflection effect in production can be solved by using automated coating methods, which can obtain a higher and more consistent anti-reflection effect.
[0117] Experimental Example 3: Demonstration of outdoor photovoltaic power station
[0118] The specific method is:
[0119] A photovoltaic power station near a highway in Guangdong Province, a 2.36MW distributed photovoltaic power station on the rooftop with pollution from roads and construction dust, conducted outdoor empirical experiments under natural weather conditions. The experiment was divided into two phases:
[0120] The first stage is to select six sets of inverters with basically the same power generation capacity. The method is to fully confirm the specifications of the components on the entire roof, the specifications of the inverter, the component installation inclination and azimuth, as well as external shading and pollution, to ensure consistency. Then all the photovoltaic components are cleaned, and the data is tracked for two weeks. The power generation data with a difference of no more than 0.2% is selected as the experimental group. A total of 6 sets of inverters are selected.
[0121] The second stage is to select six groups of photovoltaic modules connected to the inverters and verify their actual power generation capacity in pairs without any treatment, cleaning and spraying. Two groups of photovoltaic modules are not treated and continue to track their power generation hour data; two groups of photovoltaic modules are only cleaned without coating to verify the impact of environmental pollution on power generation; two groups of photovoltaic modules are sprayed with the anti-reflection self-cleaning liquid to form a film. Then collect power generation data from June 21 to September 20, 2023.
[0122] Experiments show that the permeability-enhancing liquid of the present invention has good anti-fouling and permeability-enhancing properties after coating. It is not easy to fall off, bubble, discolor and other problems when the temperature is high and the humidity is high or the temperature difference is high. The film layer has good adhesion to the surface of the photovoltaic glass. It not only has high light transmittance, but also has excellent self-cleaning performance, achieving long-term anti-fouling performance and better improving the power generation of photovoltaic modules. As can be seen from Table 8, after the photovoltaic modules are sprayed with the permeability-enhancing and self-cleaning liquid, the power generation gain dominated by the permeability-enhancing function in the first month can reach more than 4%. With the continuous influence of the surrounding environmental pollution, the increase in power generation caused by the self-cleaning function and the increase in power generation caused by the permeability-enhancing function continue to be superimposed. The data in Table 8 show that after the permeability-enhancing liquid of the present invention is applied, there is no need to clean it, and the average power generation gain in three months is more than 8% higher than that of the cleaning group. Therefore, the use of the permeability-enhancing liquid of the present invention to coat photovoltaic modules can greatly reduce the cleaning and maintenance costs of photovoltaic modules.
[0123] Table 8 Comparison of monthly full-power hours test data of photovoltaic modules
[0124]
Claims
1. A permeability-enhancing liquid for the glass surface of a photovoltaic module, characterized in that: The permeability enhancement liquid is composed of the following components in parts by weight: 0.1 to 3 parts of rhamnolipid pre-impregnated nano-titanium dioxide, 1 to 5 parts of enzyme-made mesoporous silica microspheres, 10 to 80 parts of deionized water, 0.1 to 2 parts of defoaming agent, and 1 to 20 parts of alcohol solvent; The rhamnolipid pre-impregnated nano-titanium dioxide is obtained by immersing nano-titanium dioxide in rhamnolipid; The enzyme-made mesoporous silica microspheres are obtained by the following preparation method: after polymer microsphere colloid, soluble starch, solvent and modifier are mixed, grafting reaction is carried out, impurities and solvent are removed by vacuuming at low temperature after gelatinization, and starch grafted modified microspheres are obtained; silicon source solution is added dropwise to the starch grafted modified microspheres, and the silicon source is adsorbed on the surface of the starch grafted modified microspheres by stirring; the reaction is carried out at a temperature of 40°C to 60°C and a speed of 80 to 200 rpm for 6 to 18 hours, and the silicon source undergoes gelation reaction to form a silica shell layer; amylase is added to remove the template to obtain nano-scale mesoporous silica microspheres, and the diameter of the microspheres is 5 to 200 nanometers.
2. The anti-permeability liquid for the surface of photovoltaic module glass according to claim 1, characterized in that: The bio-enzyme-made mesoporous silica microspheres are obtained by the following preparation method: (1) Preparation of starch grafted modified microspheres: 50 parts of polymer microsphere colloid, 10 parts of soluble starch, 10-15 parts of solvent, and 0.5-5 parts of modifier are added into a reaction container and stirred to form a mixture; in a microwave synthesis / extraction device, the temperature is kept at 30°C to 80°C to graft the starch with the polymer; after the mixture is gelatinized, the temperature is lowered to 40°C and low-temperature vacuum is performed to remove small molecular impurities and solvent, thereby obtaining starch grafted modified microspheres; (2) adding a silicon source solution to the treated starch grafted modified microspheres: adsorbing the silicon source on the surface of the starch grafted modified microspheres by stirring; controlling the weight ratio of the theoretical content of silicon dioxide to the starch grafted modified microspheres to be 2:1 to 3.5:1, and controlling the solid content to be less than 20% of the reaction system; (3) Gelation: The reaction is stirred at 40°C to 60°C and 80 to 200 rpm for 6 to 18 hours, and the silicon source undergoes a gelation reaction to form a silica shell layer; (4) Removing the template: adding amylase, stirring the reaction at 36°C to 40°C and 20 to 60 rpm for 24 to 48 hours to degrade the starch, then adding deionized water and stirring at high speed to elute the starch decomposition products, and the polymer microspheres are decomposed and embrittled into smaller fragments to remove the silica, which are separated and eluted several times by a centrifuge to obtain nano-scale mesoporous silica microspheres.
3. The anti-permeability liquid for the surface of photovoltaic module glass according to claim 1, characterized in that: The rhamnolipid pre-soaked nano titanium dioxide is obtained by immersing nano titanium dioxide with a particle size of 3 to 50 nm and anatase crystal form in rhamnolipid for 30 to 60 minutes.
4. The anti-permeability liquid for the surface of photovoltaic module glass according to claim 1, characterized in that: The defoamer can be an aqueous defoamer containing mineral oil, silicone, polysiloxane, ethylene bis stearamide, paraffin, and ester wax; the alcohol solvent can be an alcohol organic solvent such as methanol, ethanol, ethylene glycol, isopropanol, and a blend thereof.
5. A method for preparing the anti-permeability liquid for the surface of photovoltaic module glass according to claim 1, characterized in that: Take half of the deionized water in the formula, add about half of the alcohol solvent, the whole amount of rhamnolipid pre-impregnated nano-titanium dioxide, the whole amount of enzyme-made mesoporous silica microspheres, and the whole amount of defoaming agent in sequence, stir evenly at a speed of 1000-20000rpm in a high-speed disperser, and finally slowly add the remaining deionized water and alcohol solvent at a speed of 200-800rpm in a paddle disperser and stir evenly.
6. The method for applying the anti-permeability liquid on the surface of photovoltaic module glass according to claim 1, characterized in that: The permeability-enhancing liquid is used in a photovoltaic power station and is directly sprayed on a photovoltaic module to form a film layer.
7. A high anti-reflection solar glass, characterized in that: The high anti-reflection solar glass is obtained by coating the anti-reflection liquid described in claim 1 on a solar glass substrate using a coating method.