Preparation method and application of Cr-NiFe MOF / cellulose aerogel composite material

Cr-NiFe MOF and cellulose airgel composite materials solve the problem of high overpotential of the anode oxygen evolution reaction in water electrolysis technology, achieving low-cost, mild electrocatalytic performance improvement and corrosion resistance, which is better than existing catalyst.

CN118852718AActive Publication Date: 2024-10-29NORTHWEST UNIV

Patent Information

Application Number
CN202410891580.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-29
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

In existing water electrolysis technology, the overpotential of the anode oxygen evolution reaction is high, which limits the improvement of water electrolysis efficiency. The poor pore structure of cellulose aerogels leads to unsatisfactory electrocatalytic performance. A low-cost, mild and widely applicable method is needed. method to improve its electrochemical performance.

Method used

Cr-NiFe MOF and cellulose airgel composite materials are used to increase the activity of NiFe MOF through the doping of high-priced metal Cr, and uniformly grow MOF particles on the cellulose airgel substrate, and adjust the doping ratio to achieve the best Catalytic activity, reducing agglomeration and improving stability.

Benefits of technology

It achieves excellent electrocatalytic oxygen production performance and ultra-long-term corrosion resistance under alkaline conditions. The cost is lower than the industrial catalyst RuO2, the activity is better than that of commercial catalysts, and it has large-scale application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852718A_ABST
    Figure CN118852718A_ABST
Patent Text Reader

Abstract

The invention discloses a method for universally synthesizing an MOFs / cellulose aerogel composite electrode material and application of the MOFs / cellulose aerogel composite electrode material in electro-catalytic oxygen evolution, and belongs to the technical field of electro-catalytic functional material preparation processes. The preparation method comprises the following steps: dissolving a Cr source, a Ni source and a Fe source in deionized water, adding the solution into an N, N-dimethylformamide solution containing terephthalic acid, uniformly stirring, transferring the solution into a Teflon reaction kettle, and reacting at 160 DEG C for 24 hours to obtain Cr-NiFe MOF; then, the obtained Cr-NiFe MOF powder is dispersed in a carboxymethyl cellulose solution, a certain amount of acetone is added, liquid nitrogen freezing is carried out after even mixing is carried out at the temperature of 80 DEG C, then freeze drying is carried out for 48 h, and the Cr-NiFe MOF / cellulose aerogel composite material can be obtained. When the composite electrode material is used as an electrocatalytic oxygen evolution material, the composite electrode material shows excellent activity and extremely high stability. Especially, the aerogel composite material shows a low overpotential of 235mV at 10mA. Cm <-2 >, a tafel slope of 53.7 mV.dec-1 and stability of more than 210 hours, is one of aerogel composite materials with the best catalytic performance at present, and has a better application prospect in the fields of catalysis and energy conversion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrocatalytic functional material preparation technology, and more specifically proposes a universal MOF-based / cellulose aerogel composite material synthesis strategy and its application in electrocatalytic oxygen evolution under alkaline conditions. Background Art

[0002] As a clean energy, hydrogen energy has been highly valued because of its flexibility, high efficiency, low carbon emissions, and wide range of applications. Producing hydrogen energy through low-carbon and efficient methods is a key challenge, and hydrogen production by water electrolysis is a promising strategy to solve this problem. Synthesizing electrocatalysts that improve the reaction kinetics of the oxygen evolution reaction (OER) is the most effective way to improve the efficiency of water electrolysis. Cellulose aerogels prepared from carboxymethyl cellulose have the advantages of low cost, green renewable, high specific surface area, easy to control porous structure, and stable electrocatalytic performance. However, due to the poor pore structure of cellulose aerogels themselves, their electrocatalytic performance is not ideal. It is necessary to improve their electrochemical performance by introducing low-cost and highly active subunits.

[0003] In recent years, although aerogels have been used as electrode materials for electrocatalytic oxygen evolution, their catalytic activity and stability are still not ideal. Metal organic frameworks (MOFs) have the advantages of easy regulation and modification, good catalytic activity, etc., and can be used as subunits to improve the electrocatalytic performance of cellulose-based aerogels. The MOFs / cellulose aerogel composite is used to prepare an electrode material that has the advantages of both. Not only can MOF agglomeration be avoided to provide more active sites, but the porous structure of the aerogel effectively promotes the diffusion of electrolytes and ion conduction, thereby greatly improving its electrochemical performance. Therefore, it is very challenging to develop a low-cost, mild and widely applicable method to allow MOF particles to grow uniformly and firmly on an aerogel substrate to reduce agglomeration and improve stability. Summary of the invention

[0004] The purpose of the present invention is to propose a preparation method of a Cr-NiFe MOF / cellulose aerogel composite material and its application in an electrocatalytic oxygen production reaction to solve the problem that the current development of water electrolysis technology is limited by the high overpotential of the anode oxygen evolution reaction. The present invention improves the activity of NiFe MOF by doping with high-valent metal Cr, and adjusts the doping ratio to achieve the best catalytic activity. The whole process is mild, low-cost and universal, and its catalytic activity and corrosion resistance are completely comparable to those of precious metal catalysts, and has the prospect of large-scale application.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The preparation method of the Cr-NiFe MOF / cellulose aerogel composite material comprises the following steps:

[0007] S1. Preparation of carboxymethyl cellulose solution: dissolving carboxymethyl cellulose and NaOH in deionized water and stirring evenly to obtain a carboxymethyl cellulose solution of a certain concentration;

[0008] Preparation of S2, Cr-NiFe MOF materials:

[0009] S2.1, dissolve Ni(NO3)2·6H2O, Fe(NO3)3·9H2O and Cr(NO3)3·9H2O in deionized water and stir, record it as solution A;

[0010] S2.2, dissolving terephthalic acid in an organic solvent N,N-dimethylformamide and stirring evenly, recorded as solution B;

[0011] S2.3, add solution A dropwise to solution B, continue stirring for a while and then transfer to a hydrothermal kettle for hydrothermal reaction;

[0012] S2.4 After the reaction mixture is cooled to room temperature, it is washed several times and dried overnight to obtain Cr-NiFe MOF;

[0013] S3. Preparation of Cr-NiFe MOF / cellulose aerogel electrode material: The obtained Cr-NiFe MOF powder is dispersed in a carboxymethyl cellulose solution, a certain amount of acetone is added, and the mixture is evenly mixed at a certain temperature. After sufficient reaction, the mixture is frozen with liquid nitrogen, and then freeze-dried to obtain a Cr-NiFe MOF / cellulose aerogel composite material.

[0014] Preferably, the amount of carboxymethyl cellulose in S1 is 350-370 mg, and the amount of NaOH is 15-25 mg. The carboxymethyl cellulose and NaOH are dissolved in 10-15 ml of deionized water.

[0015] Preferably, the amounts of Ni(NO3)2·6H2O and Fe(NO3)3·9H2O in S2.1 are 1-2 mmol and 0.75-1.25 mmol respectively, the amount of Cr(NO3)3·9H2O is 0.1-0.3 mmol, and the amount of terephthalic acid is 2-4 mmol.

[0016] Preferably, the solution A in S2.1 is 10 to 20 mL of deionized water, and the solution B in S2.2 is 10 to 20 mL of N,N-dimethylformamide solution.

[0017] Preferably, the hydrothermal reaction conditions in S2.3 are heating at 150-170° C. for 24 hours; the detergent includes but is not limited to deionized water and anhydrous ethanol.

[0018] Preferably, the amount of Cr-NiFe MOF in S3 is 0.3-0.5 g, the amount of acetone is 0.2-0.4 mL, and the amount of deionized water is 10-20 mL.

[0019] Preferably, after uniform mixing in S3, the reaction temperature is controlled to be 70-90° C., and the reaction time is 2-4 hours; the liquid nitrogen freezing time is 5-15 minutes; and the freeze-drying time is 48 hours.

[0020] A Cr-NiFe MOF / cellulose aerogel electrode material prepared by the method.

[0021] An application of the Cr-NiFe MOF / cellulose aerogel electrode material prepared as above for electrocatalytic oxygen evolution under alkaline conditions.

[0022] Compared with the prior art, the present invention provides a preparation method and application of a Cr-NiFe MOF / cellulose aerogel composite material, which has the following beneficial effects:

[0023] (1) The preparation method proposed in the present invention uses the main raw materials for synthesizing the Cr-NiFe MOF / cellulose aerogel composite material as nickel salt, iron salt, chromium salt and carboxymethyl cellulose, which is low in cost and the synthesis method is simple and universal, greatly reducing the cost of the catalyst.

[0024] (2) In the present invention, carboxymethyl cellulose, which is widely available, is used as a raw material to synthesize a cellulose aerogel with a three-dimensional network structure as a substrate to uniformly load MOF particles. Compounding the MOFS structure from a brittle powder crystal state to a flexible multi-layer cellulose aerogel carrier will expose more active sites, greatly accelerate mass transfer, and enhance the activity of the catalyst.

[0025] (3) The Cr-NiFe MOF / cellulose aerogel of the present invention exhibits excellent electrocatalytic oxygen production performance and ultra-long-term corrosion resistance under alkaline conditions. Not only is its cost much lower than the current industrial catalyst RuO2, but its activity is also significantly better than commercial catalysts. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is the XRD diagram of the Cr-NiFe MOF / cellulose aerogel mentioned in the embodiment of the present invention;

[0027] Figure 2 The SEM images of the Cr-NiFe MOF / cellulose aerogel mentioned in the embodiment of the present invention, wherein the scale of (a) is 150 μm, and the scale of (b) is 10 μm;

[0028] Figure 3TEM, HAADF STEM and elemental mapping images of the Cr-NiFe MOF / cellulose aerogel composite material mentioned in the embodiment of the present invention, wherein (a) the TEM image of the sample with a scale of 500 nm, (b) the HAADF STEM image with a scale of 200 nm, and (cg) the elemental mapping image with a scale of 200 nm;

[0029] Figure 4 FT-IR image of the Cr-NiFe MOF / cellulose aerogel composite material mentioned in the embodiment of the present invention;

[0030] Figure 5 This is an XPS graph of the Cr-NiFe MOF / cellulose aerogel composite material mentioned in the embodiment of the present invention;

[0031] Figure 6 : is the LSV curve of the Cr-NiFe MOF / cellulose aerogel composite material mentioned in the embodiment of the present invention in 1M KOH electrolyte;

[0032] Figure 7 is the Tafel slope of the Cr-NiFe MOF / cellulose aerogel composite material mentioned in the embodiment of the present invention;

[0033] Figure 8 The double-layer capacitance (C) of the Cr-NiFe MOF / cellulose aerogel composite material mentioned in the embodiment of the present invention measured at 1.15 V vs. RHE dl )value;

[0034] Fig. 9 : is the EIS graph of the Cr-NiFe MOF / cellulose aerogel composite material mentioned in the embodiment of the present invention;

[0035] Fig.10 This is a long-term stability test of the Cr-NiFe MOF / cellulose aerogel composite material mentioned in the embodiments of the present invention. DETAILED DESCRIPTION

[0036] The following examples further illustrate the specific implementation of the present application, but the protection scope of the present application is not limited by these specific implementations, but is determined by the appendix claims. Unless otherwise specified, the raw materials used are conventional products purchased from the market.

[0037] Example 1

[0038] The preparation method of the Cr-NiFe MOF / cellulose aerogel composite electrode material comprises the following steps:

[0039] (1) Preparation of Cr-NiFe MOF

[0040] Cr-NiFe MOF was synthesized by a simple one-step solvothermal method. Typically, 1.5mmol of Ni(NO3)2·6H2O, 1mmol of Fe(NO3)3·9H2O and (0.125, 0.25, 0.375 and 0.5mmol) of Cr(NO3)3·9H2O were dissolved in 15ml of deionized water and stirred for 30min, which was recorded as solution A. Then, 3mmol of terephthalic acid was dissolved in 15ml of N,N-dimethylformamide solution and stirred evenly, which was recorded as solution B. Solution A was slowly added dropwise to solution B and stirred for 1h. The mixed solution was transferred to a hydrothermal reactor and heated at 160℃ for 24h. It was washed with ethanol and deionized water several times and vacuum dried at 70℃ overnight to obtain NiFe MOF doped with 5%, 10%, 15% and 20% Cr, respectively.

[0041] (2) Preparation of Cr-NiFe MOF / cellulose aerogel

[0042] 0.4 g of the Cr-NiFe MOF prepared above was added to 0.36 g of carboxymethyl cellulose, 20 mg of NaOH, and 0.3 mL of acetone dissolved in 15 ml of deionized water, reacted in an oil bath at 80 ° C for 3 h, cooled to room temperature and frozen with liquid nitrogen. Subsequently, freeze-dried for 48 h, the final sample Cr-NiFe MOF / cellulose aerogel was obtained.

[0043] Example 2

[0044] The preparation of NiFe MOF / cellulose aerogel composite electrode material comprises the following steps:

[0045] (1) Preparation of NiFe MOF

[0046] NiFe MOF was synthesized by a simple one-step solvothermal method. Typically, 1.5 mmol of Ni(NO3)2·6H2O and 1 mmol of Fe(NO3)3·9H2O were dissolved in 15 ml of deionized water and stirred for 30 min, which was recorded as solution A. Then, 3 mmol of terephthalic acid was dissolved in 15 ml of N,N-dimethylformamide solution and stirred evenly, which was recorded as solution B. Solution A was slowly added dropwise to solution B and stirred for 1 h. The mixed solution was transferred to a hydrothermal reactor and heated at 160 ° C for 24 h. Washed with ethanol and deionized water several times, and vacuum dried at 70 ° C overnight, NiFe MOF was prepared.

[0047] (2) Preparation of NiFe MOF / cellulose aerogel

[0048] 0.4 g of the prepared NiFe MOF was added to 0.36 g of carboxymethyl cellulose, 20 mg of NaOH, and 0.3 mL of acetone dissolved in 15 ml of deionized water, reacted in an oil bath at 80 ° C for 3 h, cooled to room temperature and frozen with liquid nitrogen. Subsequently, freeze-dried for 48 h, the sample NiFe MOF / cellulose aerogel was obtained.

[0049] Example 3

[0050] The preparation of Cr-NiFe MOF electrode material comprises the following steps:

[0051] (1) Preparation of 10% Cr-NiFe MOF

[0052] Cr-NiFe MOF was synthesized by a simple one-step solvothermal method. Typically, 1.5mmol Ni(NO3)2·6H2O, 1mmol Fe(NO3)3·9H2O and 0.25mmol Cr(NO3)3·9H2O were dissolved in 15ml deionized water and stirred for 30min, which was recorded as solution A. Then, 3mmol terephthalic acid was dissolved in 15ml N,N-dimethylformamide solution and stirred evenly, which was recorded as solution B. Solution A was slowly added dropwise to solution B and stirred for 1h. The mixed solution was transferred to a hydrothermal reactor and heated at 160℃ for 24h. Washed with ethanol and deionized water several times, and vacuum dried at 70℃ overnight to obtain 10% Cr-NiFe MOF.

[0053] Example 4

[0054] (1) Preparation of cellulose aerogel electrode materials

[0055] 0.36 g of carboxymethyl cellulose and 20 mg of NaOH acetone were dissolved in 15 ml of deionized water, reacted in an oil bath at 80 °C for 3 h, cooled to room temperature and frozen with liquid nitrogen. Subsequently, freeze-dried for 48 h, cellulose aerogel was obtained.

[0056] In summary, Figure 1 The X-ray powder diffraction patterns of the products obtained in Examples 1, 3, and 4 are shown. Both 10% Cr-NiFe MOF and 10% Cr-NiFe MOF / cellulose aerogels show three obvious peaks at 9.59°, 16.02°, and 18.09°, which are consistent with the crystal structure of Ni MOF (No.985792, CCDC). The peaks at 22.94, 24.06, 25.89, and 32.14 in Cr-NiFe MOF / cellulose aerogels are characteristic peaks of cellulose aerogels. This indicates that Cr-NiFe MOF / cellulose aerogels were successfully prepared with good crystallinity.

[0057] Figure 2 The SEM image of 10% Cr-NiFe MOF / cellulose aerogel obtained in Example 1 shows an interconnected network structure, and MOF is evenly dispersed on the skeleton of the aerogel ( Figure 2 ab).

[0058] Figure 3 TEM, HAADF-STEM and EDS elemental mapping images of the product obtained in Example 1. The TEM image of 10% Cr-NiFeMOF / cellulose aerogel clearly shows the aerogel lamellae and the nanosphere and nanorod structures of 10% Cr-NiFe MOF ( Figure 3 a). HAADF-STEM and EDS elemental mapping ( Figure 3 bg) Energy spectra show that Cr, Ni, and Fe elements are evenly distributed on the nanospheres, while only Cr and Ni elements can be observed on the nanorods, proving that the incorporation of Cr is beneficial to the formation of nanorod-like structures.

[0059] Figure 4 Infrared spectroscopic tests of the products obtained in Examples 1 and 3 were performed to analyze the functional groups in the 10% Cr-NiFe MOF and 10% Cr-NiFe MOF / cellulose aerogel catalysts. -1 The stretching vibration peak of OH is at 2806cm -1 The peaks at 1472 and 1355 cm are the stretching vibrations of -CH2. -1 The two characteristic peaks at belong to the symmetric vibration and asymmetric vibration of -COOH, respectively. Compared with Cr-NiFe MOF, the intensity of the characteristic peak of -COOH in the material composited with cellulose aerogel is higher, which proves the successful composite of Cr-NiFe MOF and cellulose aerogel.

[0060] Figure 5 XPS tests of the products obtained in Examples 1 and 2 were performed to determine the elements and valence states of the 10% Cr-NiFe MOF / cellulose aerogel and the NiFe MOF / cellulose aerogel. Figure 5 a It can be seen from the full spectrum that the catalyst contains Ni, Fe, Cr, C and O elements. The Ni 2p spectra of Cr-NiFe MOF / cellulose aerogel and NiFe MOF / cellulose aerogel are shown in Figure 2. Figure 5 b. The binding energies at 856.03 and 873.98 eV are respectively attributed to Ni 2+ 2p 3 / 2 and Ni 2+ 2p 1 / 2, and the other two satellite peaks are located at 861.13 eV and 880.52 eV, respectively. Compared with NiFe MOF / cellulose aerogel, the binding energy of Cr-NiFe MOF / cellulose aerogel shifts to the negative direction by about 0.7 eV. Figure 5 c, the high-resolution spectrum of Fe 2p shows that Fe 2p 3 / 2 and Fe 2p 1 / 2 The peaks are located at 711.18 and 724.65 eV, respectively, and the satellite peak is at 717.67 eV, indicating that the Fe element exists at +3 valence. Similarly, compared with NiFe MOF / cellulose aerogel, the binding energy of Fe 2p in Cr-NiFe MOF / cellulose aerogel shifts to the negative direction by about 0.3 eV. After Cr doping, the binding energy of Ni 2p and Fe 2p shifts negatively, which indicates that there is a strong electronic interaction between NiFe MOF and Cr. Figure 5 d) The Cr 2p of Cr-NiFe MOF / cellulose aerogel shows two groups of peaks corresponding to Cr2p 3 / 2 and 2p 1 / 2 , where the peaks at 577.52 and 587.63 eV correspond to Cr 3+ , the peaks at 579.98 and 591.71 eV correspond to Cr 6+ .

[0061] Figure 6 For Examples 1, 2, 3 and 4, the -1 The electrochemical LSV test of the product was obtained by scanning the rate to evaluate the OER activity of the composite electrode catalyst. All measured potential results were referenced to the reversible hydrogen electrode (vs. RHE). Figure 6 a The Cr doping amount was determined to be 10% for the example 1 amount, which was the best catalytic performance. It only needed to provide a low overpotential of 235 mV to drive 10 mA cm -2 .at the same time, Figure 5 b shows that the catalytic activity of Cr-NiFe MOF / cellulose aerogel (235 mV) is much better than that of NiFe MOF / cellulose aerogel (298 mV) and Cr-NiFe MOF (317 mV), cellulose aerogel (381 mV), and also better than the commercial catalyst RuO2 (310 mV), indicating that the doping of Cr and the composite of MOF and aerogel jointly promote the improvement of OER.

[0062] Figure 7 The Tafel slopes of the products and commercial RuO2 were obtained for Examples 1, 2, 3 and 4 to study their reaction kinetics. The Tafel slope of 10% Cr-NiFe MOF / cellulose aerogel is only 53.7 mV·dec -1, which is lower than that of other Cr-doped samples (5% Cr-NiFe MOF / cellulose aerogel (87.1 mV·dec -1 ), 15% Cr-NiFe MOF / cellulose aerogel (53.7 mV·dec -1 ), 20% Cr-NiFe MOF / cellulose aerogel (76.3mV·dec -1 ), which is also much smaller than other comparative samples NiFe MOF / cellulose aerogel (82.4 mV·dec -1 ), Cr-NiFe MOF (70.3mV·dec -1 ), cellulose aerogel (173.7mV·dec -1 ),RuO2(103.4mV·dec -1 ), indicating that Cr doping significantly improved the OER reaction kinetics of the catalyst, and further improved its reaction kinetics after being composited with cellulose aerogel.

[0063] Figure 8 The Cdl of the products obtained in Examples 1, 2, 3 and 4 was measured. The evaluation of the electrochemically active surface area (ECSA) is crucial for studying the number of catalytically active sites. Cdl can be used to estimate the electrochemically active surface area. Figure 8 As shown in Figure 2, the Cdl of 10% Cr-NiFe MOF / cellulose aerogel is 27.9 mF·cm -2 , which is higher than NiFe MOF / cellulose aerogel (21.1 mF·cm -2 ), 10% Cr-NiFe MOF (16.1mF·cm -2 ) and cellulose aerogel (10.1mF·cm -2 ). The exposed area of ​​the active sites of 10% Cr-NiFeMOF / cellulose aerogel is significantly larger than that of the uncomposite MOF and cellulose aerogel materials, proving that the combination of the two can provide a better electrocatalytic site for OER.

[0064] Fig. 9 The impedance test of the products obtained in Examples 1, 2, 3 and 4 showed that the charge transfer resistance of 10% Cr-NiFe MOF / cellulose aerogel in 1 M KOH was 1.98 Ω, showing the smallest impedance value, further proving that the incorporation of Cr and its composite with cellulose aerogel reduced the kinetic barrier in the OER process.

[0065] Fig.10 This is the long-term stability test of Example 1. Fig.10a shows that after 1000 CV cycles, the current density of the oxygen evolution reaction of the catalyst maintained good stability at each test potential, and there was no obvious decay before and after the cycle. -2 The catalyst can be stable for more than 210h ( Fig.10 b).

[0066] Based on the above content, it can be seen that the Cr-NiFe MOF / cellulose aerogel prepared in the present invention exhibits excellent electrocatalytic oxygen production performance and ultra-long-term corrosion resistance under alkaline conditions. Not only is its cost much lower than the current industrial catalyst RuO2, but its activity is also significantly better than commercial catalysts.

[0067] The above are only preferred specific implementation modes of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a Cr-NiFe MOF / cellulose aerogel composite material, characterized in that: The following steps are involved: S1. Preparation of carboxymethyl cellulose solution: dissolving carboxymethyl cellulose and NaOH in deionized water and stirring evenly to obtain a carboxymethyl cellulose solution of a certain concentration; Preparation of S2, Cr-NiFe MOF materials: S2.

1. Dissolve Ni(NO3)2·6H2O, Fe(NO3)3·9H2O and Cr(NO3)3·9H2O in deionized water and stir, which is called solution A. S2.2, dissolving terephthalic acid in an organic solvent N,N-dimethylformamide and stirring evenly, recorded as solution B; S2.3, add solution A dropwise to solution B, continue stirring for a while and then transfer to a hydrothermal kettle for hydrothermal reaction; S2.4 After the reaction mixture is cooled to room temperature, it is washed several times and dried overnight to obtain Cr-NiFe MOF; S3. Preparation of Cr-NiFe MOF / cellulose aerogel electrode material: The obtained Cr-NiFe MOF powder is dispersed in a carboxymethyl cellulose solution, a certain amount of acetone is added, and the mixture is evenly mixed at a certain temperature. After sufficient reaction, the mixture is frozen with liquid nitrogen, and then freeze-dried to obtain a Cr-NiFe MOF / cellulose aerogel composite material.

2. The method for preparing the Cr-NiFe MOF / cellulose aerogel composite material according to claim 1, characterized in that: The amount of carboxymethyl cellulose used in S1 is 350-370 mg, and the amount of NaOH used is 15-25 mg. The carboxymethyl cellulose and NaOH are dissolved in 10-15 ml of deionized water.

3. The method for preparing the Cr-NiFe MOF / cellulose aerogel composite material according to claim 1, characterized in that: The amounts of Ni(NO3)2·6H2O and Fe(NO3)3·9H2O used in S2.1 are 1-2 mmol and 0.75-1.25 mmol respectively, the amount of Cr(NO3)3·9H2O used is 0.1-0.3 mmol, and the amount of terephthalic acid used is 2-4 mmol.

4. The method for preparing the Cr-NiFe MOF / cellulose aerogel composite material according to claim 1, characterized in that: The solution A in S2.1 is 10-20 mL of deionized water, and the solution B in S2.2 is 10-20 mL of N,N-dimethylformamide solution.

5. The method for preparing the Cr-NiFe MOF / cellulose aerogel composite material according to claim 1, characterized in that: The hydrothermal reaction conditions in S2.3 are heating at 150-170° C. for 24 hours; the detergent includes but is not limited to deionized water and anhydrous ethanol.

6. The method for preparing the Cr-NiFe MOF / cellulose aerogel composite material according to claim 1, characterized in that: The amount of Cr-NiFe MOF used in S3 is 0.3-0.5 g, the amount of acetone used is 0.2-0.4 mL, and the amount of deionized water used is 10-20 mL.

7. The method for preparing the Cr-NiFe MOF / cellulose aerogel composite material according to claim 1, characterized in that: After uniform mixing in S3, the reaction temperature is controlled to be 70-90° C., and the reaction time is 2-4 hours; the liquid nitrogen freezing time is 5-15 minutes; and the freeze drying time is 48 hours.

8. A Cr-NiFe MOF / cellulose aerogel electrode material prepared by any one of the methods described in claims 1-7.

9. Use of the Cr-NiFe MOF / cellulose aerogel electrode material prepared as claimed in claim 8 for electrocatalytic oxygen evolution under alkaline conditions.

Citation Information

Patent Citations

  • Transition metal doped MIL-88 aerogel material as well as preparation method and application thereof

    CN114669329A

  • Trimetal MOF (Metal Organic Framework) oxygen evolution catalyst as well as preparation method and application thereof

    CN116925373A

  • Method for preparing transition metal-based electrocatalytic water decomposition anode catalytic material and application of transition metal-based electrocatalytic water decomposition anode catalytic material

    CN118186400A

  • KR20230118756A

Cited By

  • Rare earth phosphomolybdic acid-MOF composite catalyst as well as preparation method and application thereof

    CN121250450A