High-strength and high-plasticity quenching-partitioning steel based on dynamic partitioning and preparation method thereof

Through the dynamic partitioning process, martensite with high dislocation density and film-like austenite with low C content are obtained, which solves the problems of reduced dislocation density and excessive austenite stability during the isothermal partitioning process of traditional quenching-partitioning steel. , achieving better mechanical properties and higher production efficiency, suitable for industrial production.

CN118854033AActive Publication Date: 2024-10-29NORTHWESTERN POLYTECHNICAL UNIV

Patent Information

Application Number
CN202411048680.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-29
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The higher partitioning temperature of traditional quenching-partitioning steel during the isothermal partitioning process leads to a decrease in dislocation density and yield strength. Low-alloy quenching-partitioning steel retains a large amount of filmy austenite at low quenching temperature, resulting in excessive stability and deformation process. The uniform elongation of the medium material is reduced, and it is difficult to achieve long-term isothermal partitioning in industrial production, which limits the wide application of the quenching-partitioning process.

Method used

Using a dynamic partitioning process, through slow heating and rapid cooling, martensite with high dislocation density and film-like austenite with low C content are obtained, and the C content and dislocation recovery of austenite are controlled to form low-density austenite with excellent mechanical properties. Carbon quenching-partitioning steel overcomes the shortcomings of isothermal partitioning, improves production efficiency and reduces costs.

Benefits of technology

It achieves the improvement of martensite dislocation strengthening while ensuring the stability of austenite, expands the mechanical property control window of quenching and partitioning steel, and obtains better mechanical properties and low carbon quenching and partitioning steel that is more suitable for industrial production. It has strong theoretical research significance and market prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854033A_ABST
    Figure CN118854033A_ABST
Patent Text Reader

Abstract

The invention discloses high-strength and high-plasticity quenched-partition steel based on dynamic partition and a preparation method of the high-strength and high-plasticity quenched-partition steel, and relates to the technical field of high-strength steel machining. The method comprises the following steps: preparing a cast ingot of steel, homogenizing the cast ingot, and then forging into a steel billet; the steel billet is hot-rolled to be 10 mm thick; and the hot-rolled steel plate is heated to 800-900 DEG C, heat preservation is conducted for 30-180 s, then the hot-rolled steel plate is cooled to 180-250 DEG C, heat preservation is conducted for 10-60 s, then the hot-rolled steel plate is heated to 300-500 DEG C, then the hot-rolled steel plate is cooled to the room temperature, and the high-strength and high-plasticity quenched partition steel based on dynamic partition is obtained. According to the method, a large amount of martensite with high dislocation density and film-like austenite with low C are obtained through dynamic partition, dislocation strengthening in the martensite is improved while good stability of the whole austenite is guaranteed, and the method has important significance in expanding quenching-partition steel microstructure design and mechanical property regulation and control windows.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-strength steel processing, and in particular to a high-strength and high-plasticity quenching-partitioning steel based on dynamic partitioning and a preparation method thereof. Background Art

[0002] Steel materials, especially automotive steel materials, as the key to achieve and promote the dual carbon goal, need to continuously improve their comprehensive mechanical properties. Therefore, advanced high-strength steel with optimized mechanical properties has gradually become the main research object of the automotive industry. As a representative of advanced high-strength steel, quenching-partitioning steel has attracted widespread attention due to its excellent mechanical properties and low manufacturing cost. Its good ductility comes from the transformation induced plasticity (TRIP) effect of retained austenite during deformation, while martensite provides a hard matrix for the material.

[0003] At present, the performance improvement of quenching-partitioning steel includes the following aspects: (1) Increase the dislocation density of martensite and improve the yield strength of the material. Mishnev et al. [Mishnev R, Borisova Y, Gaidar S, et al. Q&P Response of a Medium Carbon Low Alloy Steel. Metals, 2023, 13(4): 689.] explored the relationship between the microstructure and mechanical properties of quenched-partitioned steel under different partitioning temperatures. The results showed that the lower the partitioning temperature, the higher the dislocation density in the martensite laths, and the higher the yield strength of the material under dislocation strengthening. (2) Increase the volume fraction and stability of austenite, and produce an efficient TRIP effect to improve the elongation of the material. According to the research on traditional quenched-partitioned steel, the volume fraction of retained austenite is largely affected by the quenching temperature. A report [Bansal GK, Tripathy S, Chandan AK, et al. Influence of quenching strategy on phase transformation and mechanical properties of low alloy steel. Materials Science and Engineering: A, 2021, 826: 141937.] states that as the quenching temperature increases, the volume fraction of retained austenite increases and the plasticity of the material improves. In addition, the stability of retained austenite in low alloy steel prepared by quenching and partitioning is also sensitive to the quenching temperature. For example, Liu et al. [Liu L, He BB, Cheng GJ, et al. Optimum properties of quenching and partitioning steels achieved by balancing fraction and stability of retained austenite. Scripta Materialia, 2018, 150: 1-6.] studied the microstructure formed at different quenching temperatures and found that when the quenching temperature was reduced from 240°C to 150°C, a large amount of blocky retained austenite was replaced by filmy retained austenite, and the C content continued to increase, which made the stability of the retained austenite continue to increase.

[0004] It is worth noting that although a lot of research has been carried out on the design of quenching-partitioning process, the following shortcomings still exist: (1) In the traditional isothermal partitioning process, the partitioning temperature is high, the recovery of dislocations is intensified, resulting in a decrease in dislocation density, which in turn reduces the yield strength of the material; (2) In traditional low-alloy quenching-partitioning steel, not only a large amount of film austenite is retained at the low quenching temperature, but also due to its high C content, the stability of the residual austenite is too high, and the uniform elongation of the material during deformation is reduced; (3) In the actual industrial production process, it is difficult to achieve long-term isothermal partitioning, the temperature in the furnace is very likely to fluctuate, and the partitioning temperature will also determine the volume fraction and C content of the retained austenite, which restricts the large-scale application of the quenching-partitioning process in industrial production. Summary of the invention

[0005] In view of the deficiencies in the above-mentioned background technology, the present invention provides a high-strength and high-plasticity quenching-partitioning steel based on dynamic partitioning and a preparation method thereof. The present invention utilizes dynamic partitioning to obtain a large amount of martensite with high dislocation density and low-C film-like austenite, which improves the dislocation strengthening in the martensite while ensuring the good stability of the overall austenite, and is of great significance for expanding the microstructure design and mechanical property regulation window of quenching-partitioning steel. At the same time, the invention not only overcomes the shortcomings of isothermal C partitioning, but also improves production efficiency and reduces production costs. The present invention successfully obtains low-carbon quenching-partitioning steel with better mechanical properties by adopting a dynamic partitioning process, which has extremely strong theoretical research significance and broad market prospects.

[0006] The first object of the present invention is to provide a method for preparing high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning, comprising the following steps: Prepare steel ingots, keep the ingots at 1100-1250°C for 2-4 hours for homogenization, and then forge them into 40-60mm thick billets at 1050-1150°C; The steel billet is kept at 1100-1200°C for 2-4 hours, and then hot-rolled to a thickness of 10 mm to obtain a hot-rolled steel plate; The hot-rolled steel plate is heated to 800-900°C at a heating rate of 2-10°C / s, kept warm for 30-180s, then cooled to 180-250°C at a cooling rate of 5-15°C / s, kept warm for 10-60s, heated to 300-500°C again, and then cooled to room temperature to obtain high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning.

[0007] Preferably, the heating rate when heating to 300-500°C is 0.5-1.5°C / s; the cooling rate to room temperature is 5-15°C / s.

[0008] Preferably, the hot-rolled steel plate is heated to 800-900°C at a heating rate of 2-10°C / s, kept warm for 30-180s to obtain austenite, and then cooled to 180-250°C at a cooling rate of 5-15°C / s, kept warm for 10-60s to obtain martensite.

[0009] Preferably, during hot rolling, the initial rolling temperature is 1050-1100°C, and the rolling termination temperature is not less than 850-900°C.

[0010] Preferably, the following components in mass percentage are selected when preparing the steel ingot: C: 0.2-0.4%, Mn: 2-5%, Si: 1-3%, P: ≤0.005%, S: ≤0.005%, and the balance is Fe.

[0011] Preferably, the steel ingot is produced by weighing raw materials according to the mass percentage of chemical components and then smelting them.

[0012] The second object of the present invention is to provide a high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning.

[0013] The third object of the present invention is to provide a high-strength and high-plasticity quenching-partitioning steel based on dynamic partitioning for use in automobile manufacturing.

[0014] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning and a preparation method thereof. The high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning provided by the present invention has a low C content in the film-like austenite in the retained austenite and has good stability. The present invention first heats the steel to A C3 The above short-term heat preservation obtains austenite, and then a certain amount of martensite is obtained by quenching, and then dynamic partitioning occurs during the slow heating process. Since the partitioning temperature is lower than the traditional isothermal partitioning, the C content of austenite is slightly lower after the partitioning. During the secondary quenching cooling process, with the formation of fresh martensite, a large amount of low-C film-like austenite is retained at room temperature, showing a uniform elongation of 12%~16.7% during the stretching process.

[0015] In the process of slowly heating up the temperature, the dislocations are also dynamically recovered as the dynamic partitioning proceeds. Compared with the isothermal recovery process, the recovery temperature in the dynamic process is lower, resulting in slower recovery of dislocations in the martensite, increasing the dislocation density in the martensite, and finally obtaining a yield strength of 1069-1178MPa and a tensile strength of 1649-1722MPa at room temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The invention discloses a heat treatment process diagram of a high-strength and high-plasticity quenching-partitioning steel based on dynamic partitioning.

[0017] Figure 2 : is a SEM image of the microstructure of Example 1, and the KAM value of martensite at room temperature.

[0018] Figure 3 It is the SEM image of the microstructure of conventional quenching-partitioning steel 1 and the KAM value of martensite at room temperature.

[0019] Figure 4 is the half-width at half maximum (FWHM) of the austenite XRD peak of Example 1 and conventional quenching-partitioning Steel 1.

[0020] Figure 5 1 is the room temperature tensile engineering stress-strain curve of Example 1 and conventional quenching-partitioning steel 1.

[0021] Figure 6 2 are the room temperature tensile engineering stress-strain curves of Example 2 and conventional quenching-partitioning steel 2. DETAILED DESCRIPTION

[0022] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention.

[0023] The first aspect of the present invention provides a method for preparing high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning, comprising the following steps: Prepare steel ingots, keep the ingots at 1100-1250°C for 2-4 hours for homogenization, and then forge them into 40-60mm thick billets at 1050-1150°C; The steel billet is kept at 1100-1200°C for 2-4 hours, and then hot-rolled to a thickness of 10 mm to obtain a hot-rolled steel plate; The hot-rolled steel plate is heated to 800-900°C at a heating rate of 2-10°C / s, kept warm for 30-180s, then cooled to 180-250°C at a cooling rate of 5-15°C / s, kept warm for 10-60s, heated to 300-500°C again, and then cooled to room temperature to obtain high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning.

[0024] The heating rate when heating to 300-500°C is 0.5-1.5°C / s; the cooling rate to room temperature is 5-15°C / s.

[0025] The hot rolled steel plate is heated to 800-900°C at a heating rate of 2-10°C / s, kept warm for 30-180s to obtain austenite, and then cooled to 180-250°C at a cooling rate of 5-15°C / s, kept warm for 10-60s to obtain martensite.

[0026] During hot rolling, the initial rolling temperature is 1050~1100℃, and the rolling termination temperature is not lower than 850-900℃.

[0027] When preparing the steel ingot, the following components are selected in mass percentage: C: 0.2-0.4%, Mn: 2-5%, Si: 1-3%, P: ≤0.005%, S: ≤0.005%, and the balance is Fe.

[0028] Steel ingots are produced by weighing raw materials according to the mass percentage of chemical composition and smelting them.

[0029] In one embodiment, a high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning and a preparation method thereof, wherein the composition by mass percentage is: C: 0.2-0.4%, Mn: 2-5%, Si: 1-3%, P: ≤0.005%, S: ≤0.005%, and the remainder is Fe and unavoidable impurities.

[0030] See also Figure 1 As shown, a dynamic partitioning high-strength and high-plasticity quenching-partitioning steel and its preparation method, using slow heating, on the one hand, slows down the dislocation recovery in martensite, on the other hand, reduces the C content in austenite, and after subsequent rapid cooling, forms a low-C film austenite at room temperature, providing a new preparation idea for a new generation of high-strength and high-plasticity quenching-partitioning steel. A specific method for preparing high-strength and high-plasticity quenching-partitioning steel based on dynamic partitioning includes the following steps: (1) Smelting an ingot according to the mass percentage of the chemical composition, and homogenizing the ingot at 1200° C. for 2 h, then forging the ingot at 1100° C. into a 40-60 mm thick billet, keeping the billet at 1150° C. for 2 h, and then hot rolling the billet to 10 mm, wherein the rolling termination temperature is not less than 850-900° C., and finally cooling the billet to room temperature to form a hot-rolled martensitic steel plate.

[0031] (2) Heating the hot-rolled steel plate to the austenitizing end temperature (A C3 ) and keep warm for a short time, and completely austenitize the martensite through reverse austenite transformation, the heating rate is 2-10℃ / s, the heating temperature is 800-900℃, and the holding time is 30-180s.

[0032] (3) Rapidly cool the austenite to between the start and end temperatures of the martensitic phase transformation (Ms-Mf) and briefly hold the temperature, so that part of the austenite is transformed into martensite. The cooling rate is 5-15°C / s, the end temperature is 180-250°C, and the holding time is 10-60s.

[0033] (4) Then slowly heat to a certain temperature and then quickly cool to room temperature to obtain high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning. The heating rate is 0.5-1.5°C / s, the heating temperature is 300-500°C, and the cooling rate is 5-15°C / s.

[0034] The present invention optimizes the traditional partitioning process parameters, designs the isothermal partitioning process as dynamic partitioning, utilizes the slower dislocation recovery during the heating process to produce high dislocation density martensite, and appropriately reduces the C content of the film-like residual austenite. Specifically, during the slow heating process of step (4), the process parameters such as the partitioning temperature and the partitioning time are optimized, and by controlling the dislocation recovery of the martensite and the C content of the austenite during the dynamic partitioning process, a two-phase structure of martensite with high dislocation density and C-poor film-like austenite is obtained. In the subsequent quenching process, a small amount of C-poor austenite is transformed into secondary martensite, while more C-poor film-like austenite is retained at room temperature. At the same time, the isothermal partitioning is designed as a dynamic temperature change process to reduce the instability of the organization and mechanical properties caused by the fluctuation of the partitioning temperature, making the process more suitable for industrial large-scale production.

[0035] The second aspect of the present invention provides a high-strength and high-plasticity quenching-partitioning steel based on dynamic partitioning.

[0036] A third aspect of the present invention provides an application of high-strength and high-plasticity quenching-partitioning steel based on dynamic partitioning in automobile manufacturing.

[0037] It should be noted that the experimental methods used in the present invention are all conventional methods unless otherwise specified; the reagents and materials used are all commercially available unless otherwise specified.

[0038] Example 1 Alloy composition (mass percentage): 0.38% C, 2.98% Mn, 1.49% Si, and the rest is Fe.

[0039] Preparation process: (1) The material of the selected chemical composition is placed in a vacuum furnace for smelting to obtain an ingot, which is then homogenized at 1200°C for 2 hours and forged at 1100°C into a 50 mm thick billet, which is then kept at 1150°C for 2 hours and then hot rolled to 10 mm, wherein the initial rolling temperature is 1050°C and the rolling end temperature is not less than 870°C, and finally cooled to room temperature to form a hot-rolled martensitic steel plate; (2) Using a thermal expansion instrument, the hot-rolled martensitic steel plate was heated to 850°C at a rate of 5°C / s and kept at this temperature for 60s; (3) The sample was cooled from 850 °C to 195 °C at a rate of 10 °C / s and kept at that temperature for 30 s. The sample was then heated to 450 °C at a rate of 0.85 °C / s and finally cooled to room temperature at a rate of 10 °C / s to obtain a quenched and partitioned steel.

[0040] Organization: The room temperature organization obtained by the process of Example 1 is as follows Figure 2 As shown in the figure, it contains 80% martensite (gray area) and 20% retained austenite (white area), and the retained austenite has a higher core average orientation (KAM) value. Figure 4 As shown in FIG. 1 , the FWHM of the austenite XRD peak of Example 1 is high and the C content is low. The room temperature structure of conventional quenching-partitioning steel 1 is as follows Figure 3 As shown, it contains martensite (gray area) and retained austenite (white area), where the volume fraction of martensite is 70% and the volume fraction of retained austenite is 30%. Martensite has a high KAM value. Figure 4 As shown, the FWHM of the austenite XRD peak in the conventional quenching-partitioning steel 1 is low, indicating that its C content is higher.

[0041] Mechanical properties test results, such as Figure 5 As shown: the conventional quenching-partitioning steel 1 having the same nominal composition as Example 1 and isothermal partitioning at 450°C for 300s has a yield strength of 1028MPa, a tensile strength of 1634MPa, and a uniform elongation of 15.7%; while in Example 1, the yield strength of the dynamically partitioned quenching-partitioning steel is increased to 1178MPa, the tensile strength is increased to 1722MPa, and the uniform elongation is 14.7%.

[0042] Example 2 Alloy composition (mass percentage): 0.38% C, 2.98% Mn, 1.49% Si, and the rest is Fe.

[0043] Preparation process: (1) Smelting the ingot according to the selected chemical composition, and homogenizing the ingot at 1200°C for 2 hours, then forging the ingot at 1100°C into a 50 mm thick ingot, keeping the ingot at 1150°C for 2 hours, and then hot rolling it to 10 mm, wherein the initial rolling temperature is 1100°C, the rolling end temperature is not less than 870°C, and finally cooling it to room temperature to form a hot-rolled martensitic steel plate; (2) Using a thermal expansion instrument, the hot-rolled martensitic steel plate was heated to 850°C at a rate of 5°C / s and kept at this temperature for 60s; (3) The sample was cooled from 850 °C to 195 °C at a rate of 10 °C / s and kept at that temperature for 30 s. The sample was then heated to 450 °C at a rate of 1.25 °C / s and finally cooled to room temperature at a rate of 10 °C / s to obtain a quenched and partitioned steel.

[0044] Mechanical properties test results (such as Figure 6As shown): The conventional quenched-partitioned steel 2 having the same nominal composition as Example 2 and isothermally partitioned at 450°C for 200s has a yield strength of 1015 MPa, a tensile strength of 1632 MPa, and a uniform elongation of 15.3%; while in Example 2, the yield strength of the dynamically partitioned quenched-partitioned steel is increased to 1095 MPa, the tensile strength is increased to 1685 MPa, and the uniform elongation is 14.5%.

[0045] The present invention describes preferred embodiments and their effects. However, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0046] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning, characterized in that: The following steps are involved: Prepare steel ingots, keep the ingots at 1100-1250°C for 2-4 hours for homogenization, and then forge them into 40-60mm thick billets at 1050-1150°C; The steel billet is kept at 1100-1200°C for 2-4 hours, and then hot-rolled to a thickness of 10 mm to obtain a hot-rolled steel plate; The hot-rolled steel plate is heated to 800-900°C at a heating rate of 2-10°C / s, kept warm for 30-180s, then cooled to 180-250°C at a cooling rate of 5-15°C / s, kept warm for 10-60s, heated to 300-500°C again, and then cooled to room temperature to obtain high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning.

2. The method for preparing high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning according to claim 1, characterized in that: The heating rate when heating to 300-500°C is 0.5-1.5°C / s; the cooling rate to room temperature is 5-15°C / s.

3. The method for preparing high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning according to claim 1, characterized in that: The hot rolled steel plate is heated to 800-900°C at a heating rate of 2-10°C / s, kept warm for 30-180s to obtain austenite, and then cooled to 180-250°C at a cooling rate of 5-15°C / s, kept warm for 10-60s to obtain martensite.

4. The method for preparing high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning according to claim 1, characterized in that: During hot rolling, the initial rolling temperature is 1050~1100℃, and the rolling termination temperature is not lower than 850-900℃.

5. The method for preparing high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning according to claim 1, characterized in that: When preparing the steel ingot, the following components are selected in mass percentage: C: 0.2-0.4%, Mn: 2-5%, Si: 1-3%, P: ≤0.005%, S: ≤0.005%, and the balance is Fe.

6. The method for preparing high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning according to claim 5, characterized in that: Steel ingots are produced by weighing raw materials according to the mass percentage of chemical composition and smelting them.

7. A high-strength and high-plastic quenching-partitioning steel based on dynamic partitioning obtained by the method according to any one of claims 1 to 6.

8. Use of the high-strength and high-plasticity quenching-partitioning steel based on dynamic partitioning as claimed in claim 7 in automobile manufacturing.

Citation Information

Patent Citations

  • Low-alloy high-strength C-Mn-Al Q & P steel and method of manufacturing the same

    CN101487096A

  • Process method for improving ductility and toughness of Cr-containing high-strength steel by utilizing carbon distribution

    CN101705345A

  • Preparation method of medium manganese steel with low manganese content

    CN115181913A

  • Mn chemical non-uniformity-based high-strength and high-plasticity quenched-partitioned steel and preparation method thereof

    CN116875906A

  • Highly thick steel material having excellent low-temperature impact toughness and manufacturing method therefor

    US20240035107A1

Cited By

  • Wear-resistant martensitic stainless steel and preparation method thereof

    CN120330437A

  • Wear-resistant martensitic stainless steel and preparation method thereof

    CN120330437B