Method for inhibiting generation of acid iron in normal-pressure wet copper leaching process
By using iodine-containing agents and Thiobacillus ferrooxidans technology during the atmospheric wet copper leaching process, the redox potential is controlled and pyrite oxidation is inhibited, thereby solving the problem of excessive production of acid iron in low-grade secondary copper sulfide ores. Improved copper leaching efficiency and sustainability of environmentally friendly processes.
Patent Information
- Application Number
- CN202410901835.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the biological copper leaching process of low-grade secondary copper sulfide ores, pyrite oxidation leads to excessive production of acid iron, which increases environmental neutralization costs and environmental treatment loads. Moreover, traditional suppression methods are ineffective and affect copper leaching efficiency.
Using iodine-containing chemicals to immerse copper under normal pressure by wet method, by changing the density of the passivation film on the surface of copper sulfide minerals and regulating the redox potential, the oxidation of pyrite is inhibited and the production of acid iron is reduced. Specific methods include using iodine-containing chemicals for leaching, controlling the pH value and ferric ion concentration, using activated carbon to adsorb iodide ions, and oxidizing ferrous ions with Thiobacillus ferrooxidans to control the redox potential.
It effectively inhibits the oxidation of pyrite, reduces the production of acid iron, reduces neutralization costs, increases copper ore processing capacity, reduces the burden on environmental protection processes, and achieves production results with low chemical consumption and low cost.
Smart Images

Figure CN118854073A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of nonferrous metal hydrometallurgy, and in particular to a method for inhibiting the generation of acid iron in a normal pressure wet copper leaching process. Background Art
[0002] The "bio-leaching copper-extraction-electrodeposition" process has the advantages of low cost and low energy consumption, and has become the preferred process for low-grade secondary copper sulfide ores. However, in the bio-heap leaching process of some low-grade copper ores, the ore has a high pyrite content and a high sulfur-copper ratio. The use of the permanent heap method (i.e., heap leaching of the ore layer by layer, and no heap removal after leaching) causes the pyrite in the accumulation layer to continuously oxidize and dissolve to produce acid and iron. When the acid-consuming gangue components in the ore are relatively small, the leaching system has excess acid iron. Excess acid iron brings great harm to production:
[0003] (1) The cost of end-of-life environmental protection and neutralization remains high, which compresses the profit margin of cathode copper products and increases the environmental treatment load and potential environmental risks under extreme climatic conditions.
[0004] (2) The amount of slag produced by lime neutralization in environmental wastewater treatment is large, and the storage capacity restricts the sustainable development of the process.
[0005] (3) The high amount of iron transferred during the extraction process results in a low current efficiency (<90%) during the electrolytic process, leading to inefficient production operation.
[0006] In the traditional copper bioleaching system, the redox potential of the solution mainly depends on the ratio of trivalent iron ions to divalent iron ions in the solution. 3+ / Fe 2+ ] concentration ratio, that is, solution potential, is the key factor affecting the dissolution of pyrite. When the leaching of copper sulfide ore is completed, continuing to maintain a high redox potential will accelerate the oxidation leaching of pyrite, and produce excessive acid and iron in the later stage of leaching. Therefore, it is crucial to regulate the potential to inhibit the oxidation of pyrite while not affecting or even promoting the leaching of copper sulfide ore.
[0007] At present, the main methods for inhibiting pyrite oxidation include soil isolation, surface passivation and acid neutralization. (1) The soil isolation method usually uses a material with poor permeability to wrap pyrite so that pyrite does not come into contact with water and oxygen, thereby inhibiting pyrite oxidation. However, this treatment method is mainly used for the covering operation of abandoned leaching heaps and cannot be effectively implemented in production operations. (2) The surface passivation method protects pyrite from oxidation from a microscopic perspective, mainly including phosphate passivation, silicate passivation and organic salt passivation. However, the effect of these passivators in treating pyrite in actual production environments is not very ideal, and the cost of the reagents is relatively high; at the same time, the secondary pollution problem caused by the passivator itself is also an important factor restricting the development of the passivation method. (3) Some studies have used the addition of limestone ore to heap leaching ore to inhibit pyrite oxidation leaching. Although pyrite oxidation is inhibited and the amount of acid iron generated in the system is reduced, the copper leaching process is also inhibited. Taking into account factors such as economic benefits, inhibition effects and operating methods, there is still no method to achieve ideal results in the treatment of copper sulfide ore. Summary of the invention
[0008] In view of the shortcomings of the prior art, the present invention aims to provide a method for inhibiting the generation of acid iron during the atmospheric pressure wet copper leaching process. On the one hand, the density of the passivation film on the surface of the copper sulfide mineral can be changed, the activation energy of the oxidation reaction of the copper sulfide ore can be reduced, and the trivalent iron ions can be greatly promoted to pass through the passivation film and react with the copper mineral. On the other hand, the redox potential of the leaching solution can be regulated to be in a relatively low potential range for a long time, so as to effectively inhibit the oxidation of pyrite, reduce the generation of acid iron in the heap, alleviate the back-end environmental protection neutralization pressure, and reduce the neutralization cost.
[0009] In order to achieve the above object, the present invention adopts the following technical solution:
[0010] A method for inhibiting the generation of acid iron during atmospheric pressure wet copper leaching comprises leaching copper-containing ore with an iodine-containing agent, wherein the iodine-containing agent has a pH of 1.0-1.8, a trivalent iron ion concentration of 2-20 g / L, and an iodine concentration of 10-500 ppm.
[0011] Furthermore, the iodine is derived from an inorganic salt containing iodine (such as potassium iodide, potassium iodate) or elemental iodine, or an organic agent containing iodine (such as iodoacetic acid).
[0012] Furthermore, the leaching is carried out by biological heap leaching or stirred tank leaching; in biological heap leaching, after each layer of copper-containing ore is completely leached, a new layer of copper-containing ore is covered on the old heap to continue biological heap leaching; during heap leaching, iodine-containing reagents are added to the copper-containing ore by spraying or directly adding; in stirred tank leaching, iodine-containing reagents are used as leaching agents to stir and leach the copper-containing ore.
[0013] Furthermore, the method also includes the following process: air is blown into the copper leaching solution obtained by leaching, the pH of the copper leaching solution is 1-1.8, the free iodine ions in the copper leaching solution are converted into elemental iodine, and then the solution is passed through an activated carbon column to adsorb iodine on the activated carbon, and finally an adsorbed liquid with an iodine content of less than 0.1 ppm is obtained.
[0014] Furthermore, the method also includes the following process: extracting, stripping and electrowinning the adsorbed liquid to obtain cathode copper; sending the copper raffinate obtained after extraction to a reaction pool rich in Thiobacillus ferrooxidans, blowing air into the reaction pool, and under the action of Thiobacillus ferrooxidans, ferrous ions in the copper raffinate are oxidized to trivalent ferrous ions, and the pH is controlled to be 1-1.8, and the redox potential is 600-650mV vs.Ag / AgCl.
[0015] Furthermore, the method also includes the following process: passing the sodium sulfite solution through the loaded activated carbon column to desorb the agent in the activated carbon column.
[0016] Furthermore, in the biological heap leaching of step S1, when the iodine-containing agent is added by spraying, the ore pile is sprayed at room temperature; when the iodine-containing agent is added by direct addition, the iodine-containing agent is sprayed or applied to the copper-containing ore during the crushing, agglomeration, transportation and / or heaping of the copper-containing ore.
[0017] Furthermore, in the stirring tank leaching of step S1, the ore is ground to a particle size D 80 =74um, and adjust the slurry mass concentration to 20-50%, and stir and leach for 1-8h at room temperature -90℃.
[0018] Furthermore, in step S2, the flow rate of the solution flowing through the activated carbon column is controlled at 0.2-5 L / s.
[0019] Furthermore, in step S5, the mass concentration of the sodium sulfite solution is 5%.
[0020] The beneficial effects of the present invention are as follows: the method of the present invention utilizes the chemical catalytic properties of iodine-containing agents to eliminate the passivation film density problem encountered in conventional oxidation leaching processes of copper sulfide ores, and promotes efficient leaching of copper sulfide ores while realizing the regulation of the redox potential of the leaching system, reducing the potential of the leaching system, and inhibiting the oxidation and dissolution of pyrite, thereby reducing the external production of acid and iron. The method of the present invention can be subsequently connected with the conventional "extraction electrowinning" process to achieve an increase in the copper ore processing capacity, while effectively reducing the acid iron processing capacity of the back-end neutralization and environmental protection process, reducing the consumption of neutralization agents, and having extraordinary significance for the leaching process of low-grade copper sulfide ores with high sulfur copper ratio. In addition, the key materials such as iodine-containing catalytic agents and trivalent iron ions involved in the process of the method of the present invention can be recycled, with low agent consumption and low production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a flow chart of the method of embodiment 1 of the present invention;
[0022] Figure 2 The graph is a variation curve of the copper leaching rate of Example 1 of the present invention and Comparative Example 1 with the leaching time;
[0023] Figure 3 It is a curve diagram showing the change of the iron leaching rate with the leaching time of Example 1 of the present invention and Comparative Example 1;
[0024] Figure 4 The graph is a graph showing the change of acid consumption per ton of ore with leaching time in Example 1 of the present invention and Comparative Example 1;
[0025] Figure 5 The graph is a graph showing the change of the redox potential of the leaching solution of Example 1 of the present invention and Comparative Example 1 with the leaching time. DETAILED DESCRIPTION
[0026] The present invention will be further described below in conjunction with the accompanying drawings. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to this embodiment.
[0027] Example 1
[0028] The composition of a low-grade copper sulfide ore is Cu 0.25%, Fe 4.05%, and S 5.20%. The main copper minerals in the ore are blue chalcocite, covellite, and arsenic sulfide, of which blue chalcocite accounts for about 50%. The pyrite content is 3.91%. The main gangue minerals are feldspar, quartz, and sericite. Figure 1 As shown in the figure, the ore is crushed to a particle size of less than 40 mm and then subjected to biological heap leaching. The ore heap is 12 m high and the heap plane is inclined at 5°. During the heap leaching process, an iodine-containing agent is sprayed onto the ore heap. The iodine-containing agent contains Fe 3+ The concentration is 10g / L, pH is about 1.5, and the iodine addition is 200ppm (using potassium iodide as the source of iodine). After 250 days of leaching, the copper leaching rate is 85.2%, the leaching solution potential is controlled at about 420mV (vs Ag / AgCl), the total iron leaching rate is about 3.6%, and the acid consumption per ton of ore is about 3.7kg.
[0029] After leaching is completed, air is blown into the copper leachate obtained by leaching, the pH of the copper leachate is 1.5, and the free iodine ions in the copper leachate are converted into iodine element, and then the solution is allowed to flow through the activated carbon column at a flow rate of 5L / s, so that the iodine is adsorbed on the activated carbon, and finally the adsorption liquid with an iodine content of less than 0.1ppm is obtained. The adsorption liquid is extracted, stripped, and electrolytically obtained to obtain cathode copper; the copper raffinate obtained after extraction is sent to a reaction pool rich in ferrothiobacillus ferrooxidans, and air is blown into the reaction pool. Under the action of ferrothiobacillus ferrooxidans, the ferrous ions in the copper raffinate are oxidized to trivalent iron ions, and the pH is controlled to be 1.5, and the redox potential is 600-650mVvs.Ag / AgCl. A sodium sulfite solution with a mass concentration of 5% is passed through the loaded activated carbon column to desorb the agent in the activated carbon column.
[0030] Example 2
[0031] This embodiment is substantially the same as embodiment 1, except that the iodine addition amount in the iodine-containing agent of this embodiment is 300 ppm (using potassium iodide as the iodine element source). After 250 days, the copper leaching rate is 88.4%, the iron leaching rate is 3.1%, the solution potential is controlled at about 410 mV (vs Ag / AgCl), and the acid consumption per ton of ore is about 4.4 kg.
[0032] Example 3
[0033] This embodiment is substantially the same as embodiment 1, except that the iodine addition amount in the iodine-containing agent of this embodiment is 100 ppm (using potassium iodide as the iodine element source). After 250 days, the copper leaching rate is 82.3%, the total iron leaching rate is 3.9%, the solution potential is controlled at about 430 mV (vs Ag / AgCl), and the acid consumption per ton of ore is about 3.3 kg.
[0034] Example 4
[0035] This embodiment is substantially the same as embodiment 1, except that the iodine addition amount in the iodine-containing agent of this embodiment is 50 ppm (using potassium iodide as the iodine element source). After 250 days, the copper leaching rate is 80.8%, the iron leaching rate is 4.2%, the solution potential is controlled at about 440 mV (vs Ag / AgCl), and the acid consumption per ton of ore is about 2.8 kg.
[0036] Example 5
[0037] This embodiment is substantially the same as embodiment 1, except that the iodine addition amount in the iodine-containing agent of this embodiment is 25 ppm (using potassium iodide as the iodine element source). After 250 days, the copper leaching rate is 78.2%, the iron leaching rate is 4.3%, the solution potential is controlled at about 450 mV (vs Ag / AgCl), and the acid consumption per ton of ore is about 2.7 kg.
[0038] Example 6
[0039] The composition of a low-grade copper sulfide ore is Cu 0.31%, Fe 2.38%, and S 3.84%. The main copper mineral in the ore is secondary copper sulfide ore, accounting for about 95%. The pyrite content is 2.16%. The main gangue minerals are feldspar, quartz, and sericite. The ore is crushed to a particle size of less than 40mm and then subjected to biological heap leaching. The heap is 12m high and the heap plane is inclined at 5°. During the heap leaching process, an iodine-containing agent is sprayed on the ore heap. In the iodine-containing agent, Fe 3+ The concentration is 10g / L, pH is about 1.5, and the iodine addition amount is 200ppm (using potassium iodide as the iodine source). After 250 days of leaching, the copper leaching rate is 93.4%, the leaching solution potential is controlled at about 410mV (vs Ag / AgCl), the iron leaching rate is about 2.8%, and the acid consumption per ton of ore is about 6.5kg.
[0040] Example 7
[0041] The composition of a low-grade copper sulfide ore is Cu 0.31%, Fe 2.38%, S 3.84%. The main copper mineral in the ore is secondary copper sulfide ore, accounting for about 95%. The pyrite content is 2.16%. The main gangue minerals are feldspar, quartz, and sericite. The above ore sample, which is finely ground to -0.074mm and accounts for 80%, is mixed with a leaching agent (Fe 3+ The concentration is 10g / L, pH is about 1.5, and the iodine addition amount is 200ppm (potassium iodide is used as the iodine element source) to prepare a 30% slurry concentration. Continuous stirring and leaching for 6 hours at 60℃, the copper leaching rate is 84.8%, the leaching solution potential is controlled at about 410mV (vs Ag / AgCl), the iron leaching rate is about 4.3%, and the acid consumption per ton of ore is about 5.2kg.
[0042] Comparative Example 1
[0043] The difference from Example 1 is that potassium iodide or other iodine-containing catalyst is not added. After 250 days, the copper leaching rate is 49%, the total iron leaching rate is 16.5%, the solution potential is about 600mV (vs Ag / AgCl), and the acid consumption per ton of ore is about -2.1kg (i.e., the net acid production per ton of ore is 2.1kg).
[0044] Figure 2 The graph is a graph showing the change of the copper leaching rate of Example 1 and Comparative Example 1 with the leaching time. In the early stage of leaching, the copper leaching curves of Example 1 and Comparative Example 1 are basically overlapped. After 22 days of leaching, the copper leaching rate is relatively close (about 38%); as the leaching cycle is extended, the copper leaching rate curve corresponding to Comparative Example 1 rises slowly and gradually tends to be flat, while the copper leaching curve of Example 1 rises significantly. After 250 days of leaching, the corresponding copper leaching rates of Comparative Example 1 and Example 1 are 49% and 84%, respectively.
[0045] Figure 3 The iron leaching rate of Example 1 and Comparative Example 1 varies with the leaching time. During the entire leaching period, the iron leaching rate of Comparative Example 1 is significantly lower than that of Example 1. The iron leaching curve corresponding to Comparative Example 1 continues to rise rapidly with the leaching period, while the iron leaching rate curve of Example 1 rises slowly. After leaching for 250 days, the iron leaching rates of Comparative Example 1 and Example 1 are approximately 4% and 17%, respectively.
[0046] Figure 4 The graph of the change of the acid consumption per ton of ore with the leaching time of Example 1 and Comparative Example 1 shows that the acid consumption per ton of ore of Comparative Example 1 is significantly higher than that of Example 1 during the entire leaching cycle. Due to the presence of acid-consuming gangue in the ore, the acid consumption per ton of ore curve of Comparative Example 1 first rises in the early stage of leaching, and then with the continuous oxidation of the ore, the pyrite continues to oxidize and produce acid, resulting in a continuous decrease in the acid consumption per ton of ore. In Example 1, due to the addition of iodine-containing catalyst potassium iodide, the oxidation of pyrite is inhibited, so the amount of acid produced to the outside is very small, and the acid consumption per ton of ore curve first rises and then tends to be flat. When leaching for 250 days, the iron leaching rates corresponding to Comparative Example 1 and Example 1 are approximately -2kg / t (acid production) and 3.7kg / t (acid consumption), respectively.
[0047] Figure 5 The following is a graph showing the change of the redox potential of the leaching solution of Example 1 and Comparative Example 1 with the leaching time. During the entire leaching period, the potential of Comparative Example 1 is significantly higher than that of Example 1. In Example 1, due to the addition of potassium iodide, an iodine-containing catalyst, the catalyst reacts with the oxidant in the system, causing the redox potential of the leaching system to decrease (~400mV), while in Comparative Example 1, no iodine-containing catalyst is added, and the system potential remains at a relatively high level (~550mV).
[0048] Comparative Example 2
[0049] The difference from Example 7 is that potassium iodide or other iodine-containing catalysts are not added. Leaching for 6 hours, the copper leaching rate is 62.4%, the iron leaching rate is 7.7%, the solution potential is about 520mV (vs Ag / AgCl), and the acid consumption per ton of ore is about 2.4kg. Under the same fine grinding particle size conditions, within a shorter action time, the iodine-containing catalyst can still play a role in promoting copper ore leaching and suppressing acid and iron production. By adding iodine-containing catalysts, the reaction solution potential is reduced to 410mV from 520mV, the iron leaching rate is reduced to 4.3% from 7.7%, the acid consumption per ton of ore is reduced to 2.4kg / t from 5.2kg / t, and the copper leaching rate is increased to 84.8% from 62.4%.
[0050] For those skilled in the art, various corresponding changes and modifications can be made according to the above technical solutions and concepts, and all of these changes and modifications should be included in the protection scope of the claims of the present invention.
Claims
1. A method for inhibiting the generation of acid iron during atmospheric pressure wet copper leaching, characterized in that: The method comprises leaching the copper-containing ore with an iodine-containing agent, wherein the pH of the iodine-containing agent is 1.0-1.8, the concentration of trivalent iron ions is 2-20 g / L, and the concentration of iodine is 10-500 ppm.
2. The method according to claim 1, characterized in that The iodine is derived from an iodine-containing inorganic salt, elemental iodine or an iodine-containing organic agent.
3. The method according to claim 1, characterized in that The leaching is carried out by biological heap leaching or stirred tank leaching. In biological heap leaching, after each layer of copper-containing ore is completely leached, a new layer of copper-containing ore is covered on the old heap to continue biological heap leaching. During heap leaching, an iodine-containing agent is added to the copper-containing ore by spraying or directly adding. In stirred tank leaching, the iodine-containing agent is used as a leaching agent to stir and leach the copper-containing ore.
4. The method according to claim 1, characterized in that: The method also includes the following process: air is blown into the copper leaching solution obtained by leaching, the pH value of the copper leaching solution is 1-1.8, free iodine ions in the copper leaching solution are converted into elemental iodine, and then the solution is passed through an activated carbon column to adsorb iodine on the activated carbon, and finally an adsorbed solution with an iodine content of less than 0.1 ppm is obtained.
5. The method according to claim 4, characterized in that The method also includes the following steps: extracting, stripping and electrowinning the adsorbed liquid to obtain cathode copper; sending the copper raffinate obtained after extraction to a reaction pool rich in Thiobacillus ferrooxidans, blowing air into the reaction pool, and under the action of Thiobacillus ferrooxidans, oxidizing ferrous ions in the copper raffinate to trivalent ferrous ions, controlling the pH to be 1-1.8, and the redox potential to be 600-650 mV vs. Ag / AgCl.
6. The method according to claim 4, characterized in that The method also includes the following process: allowing the sodium sulfite solution to pass through the loaded activated carbon column to desorb the reagent in the activated carbon column.
7. The method according to claim 3, characterized in that In the biological heap leaching of step S1, when the iodine-containing agent is added by spraying, the ore heap is sprayed at room temperature; when the iodine-containing agent is added by direct addition, the iodine-containing agent is sprayed or applied to the copper-containing ore during the crushing, agglomeration, transportation and / or heaping of the copper-containing ore.
8. The method according to claim 3, characterized in that In the stirred tank leaching of step S1, the ore is ground to a particle size D 80 =74um, and adjust the slurry mass concentration to 20-50%, and stir and leach for 1-8h at room temperature -90℃.
9. The method according to claim 4, characterized in that In step S2, the flow rate of the solution flowing through the activated carbon column is controlled at 0.2-5 L / s.
10. The method according to claim 6, characterized in that In step S5, the mass concentration of the sodium sulfite solution is 5%.