Leaching method of laterite-nickel ore

The iron is removed through normal pressure hydrochloric acid leaching and heating hydrolysis steps, and combined with the nickel precipitation slag is recycled to neutralize the aluminum precipitation, achieving efficient nickel and cobalt recovery and solving the problems of low nickel and cobalt concentration and large amounts of neutralizing agent in the existing technology. , reduces production costs and equipment investment, and is suitable for large-scale industrial application.

CN118854076AInactive Publication Date: 2024-10-29INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310465299.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing laterite nickel ore leaching process, the concentration of nickel and cobalt elements is low, the amount of neutralizer is large, and the addition of oxidants is required, resulting in high production costs and large equipment investment, making it difficult to achieve large-scale industrial application.

Method used

The normal pressure hydrochloric acid leaching method is used to remove iron through a heating and hydrolysis step, and the nickel precipitation slag is reused in the neutralization and aluminum precipitation process, reducing the use of neutralizers, improving the nickel and cobalt recovery rate, and achieving the maximum oxidant through the secondary nickel precipitation process utilization.

Benefits of technology

It significantly increases the concentration of nickel and cobalt leachate, reduces equipment investment and production costs, simplifies the treatment process, reduces the introduction of impurities, and achieves efficient nickel and cobalt recovery and process economy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854076A_ABST
    Figure CN118854076A_ABST
Patent Text Reader

Abstract

The invention provides a laterite-nickel ore leaching method which comprises the following steps: mixing laterite-nickel ore with hydrochloric acid, and then leaching to obtain a leaching solution and leaching residues; heating and hydrolyzing the leachate to obtain iron slag and hydrolysate; the hydrolysate is subjected to neutralization and aluminum precipitation, and aluminum slag and aluminum precipitation liquid are obtained; performing nickel precipitation on the aluminum precipitation liquid to obtain nickel precipitation slag and nickel precipitation post-liquid, and pyrolyzing the nickel precipitation post-liquid to obtain regenerated magnesium oxide and hydrochloric acid; the nickel precipitation slag is reused in the neutralization and aluminum precipitation process; according to the leaching method, the solution treatment capacity can be greatly reduced, the adding and neutralizing times of a neutralizing agent are reduced, the nickel ion concentration in the solution is improved, the total investment of equipment is reduced, and the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy and relates to a leaching method of laterite nickel ore. Background Art

[0002] Nickel and cobalt are widely used and have been applied to various fields of industry and daily life, such as stainless steel, non-ferrous metal alloys, new energy vehicles, electroplating, chemicals, etc. With the depletion of nickel sulfide ore resources, the development and utilization of laterite nickel ore, which accounts for more than 70% of the world's nickel resources, has attracted much attention. The existing wet sulfuric acid pressure leaching process for laterite nickel ore has a high reaction temperature and produces a large amount of sulfur-containing waste slag that cannot be directly used. The hydrochloric acid leaching process has the advantages of mild reaction conditions and easy regeneration and circulation of the medium, and has been widely used; however, due to the low concentration of hydrochloric acid and the fact that most of the iron and magnesium will be leached during the leaching process, the subsequent nickel and cobalt concentration is low, and more neutralizers need to be added. The equipment occupies a large area and the impurity treatment is more complicated.

[0003] At the same time, the methods disclosed in the prior art for leaching laterite nickel ore with hydrochloric acid at normal pressure also have many other defects. For example, in the clean production method for leaching laterite nickel ore with hydrochloric acid at normal pressure disclosed in CN 103215446A, hydrochloric acid leaching and high-temperature calcination process are used to treat laterite nickel ore. The nickel and cobalt concentrations obtained by this process are low, and the leached impurities iron and magnesium cannot be separated from nickel and cobalt, making subsequent refining difficult and costly; CN 112226630A discloses a method for extracting valuable metal elements from laterite nickel ore and acid-base regeneration cycle by hydrochloric acid leaching, which uses hydrochloric acid pressure leaching for laterite nickel ore, has a high reaction temperature, a low nickel and cobalt concentration, and the subsequent separation of iron slag and silicon slag together is relatively complicated, affecting the process economy; CN In a method for extracting nickel and cobalt from laterite nickel ore by hydrochloric acid leaching disclosed in 109457111A, limonite-type and serpentine-type laterite nickel ore are used for leaching, and one or more ferrous ions selected from hydrogen peroxide, sodium peroxide, sodium hypochlorite, air, oxygen and ozone are used to oxidize ferrous ions. Therefore, either sodium ions are introduced, or expensive and highly toxic hydrogen peroxide is used, or the reaction time is long and the economic cost is high. In the treatment method of laterite nickel ore leachate disclosed in CN 109457112A, a scheme of stepwise oxidation and iron precipitation is adopted, in which seed crystals need to be added, the overall process flow is long, and many reagents are added.

[0004] Based on the above research, the existing laterite nickel ore leaching process has the problems of low concentration of nickel and cobalt elements, large amount of neutralizer, and need to add oxidant, etc., and it is necessary to provide a laterite nickel ore leaching method, which is clean and efficient, has a high leaching rate and low equipment investment, and can make the process have greater economic value and can be applied on a large scale in industry. Summary of the invention

[0005] The object of the present invention is to provide a leaching method of laterite nickel ore, and in particular to a hydrochloric acid atmospheric pressure leaching method of laterite nickel ore, wherein the leaching method can significantly reduce the solution processing amount, reduce the addition of a neutralizing agent and the number of neutralization times, increase the nickel ion concentration in the solution, reduce the overall equipment investment, and reduce the production cost.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a method for leaching laterite nickel ore, the method comprising the following steps:

[0008] (1) mixing laterite nickel ore with hydrochloric acid, and then leaching to obtain leachate and leached residue;

[0009] (2) heating and hydrolyzing the leaching solution of step (1) to obtain iron slag and hydrolyzate;

[0010] (3) neutralizing the hydrolyzate obtained in step (2) and precipitating aluminum to obtain an aluminum precipitation liquid;

[0011] (4) subjecting the aluminum precipitation liquid in step (3) to nickel precipitation to obtain nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid to obtain regenerated magnesium oxide and hydrochloric acid;

[0012] The nickel precipitation slag is recycled for the neutralization and aluminum precipitation process in step (3).

[0013] The leaching method of the present invention can realize atmospheric pressure leaching of laterite nickel ore to obtain a leachate, avoid the introduction of a large amount of neutralizing agent to generate substances that are difficult to filter and easy to adsorb iron hydroxide, simplify the treatment process, reduce the introduction of impurities, make the hydrolyzate contain higher content of nickel and cobalt, improve the nickel and cobalt recovery rate, and greatly reduce equipment investment; and in the subsequent aluminum precipitation process, the present invention uses the nickel precipitation slag generated in the nickel precipitation process, utilizes the manganese oxide therein to oxidize and precipitate iron, and avoids the introduction of other oxidants as much as possible. Therefore, the overall process of the present invention is simple, can greatly reduce the production cost and equipment investment, and can achieve large-scale industrial application.

[0014] The laterite nickel ore in step (1) of the present invention is ground laterite nickel ore powder.

[0015] Preferably, the hydrolyzate of step (2) is also added during the mixing process of step (1).

[0016] Since the present invention removes iron by heating and hydrolysis, iron removal is achieved without adding an additional neutralizing agent or adjusting the pH. Therefore, the obtained hydrolyzate contains residual acid, so that the hydrolyzate can be reused in the leaching step of step (1), saving the amount of acid used and the leaching effect will not be affected.

[0017] Preferably, the concentration of the hydrochloric acid in step (1) is above 30%, for example, 30%, 31%, 33%, 35% or 38%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0018] Preferably, after the leaching in step (1), solid-liquid separation is further performed to obtain the leaching solution and leaching residue.

[0019] Preferably, the leached slag in step (1) comprises silicon slag.

[0020] Preferably, the leaching temperature in step (1) is 80-120°C, for example, 80°C, 90°C, 100°C, 110°C or 120°C, and the leaching time is 1-3h, for example, 1h, 2h or 3h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] Preferably, the leaching in step (1) is carried out in a reactor.

[0022] Preferably, the temperature of the heating hydrolysis in step (2) is 130-180°C, for example, 130°C, 150°C, 170°C or 180°C, and the time is 2-5h, for example, 2h, 3h, 4h or 5h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0023] The temperature of the heating hydrolysis in step (2) of the present invention will affect the removal of iron, etc. If the temperature of the heating hydrolysis is too high, the production energy consumption will be high and the equipment operability will be worse. If the temperature of the heating hydrolysis is too low, the iron will not easily undergo hydrolysis reaction and the reaction effect will be poor.

[0024] Preferably, 20-50% of the hydrolyzate in step (2) is recycled to the leaching process in step (1), for example, it can be 20%, 30% or 50%, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0025] Preferably, in the hydrolyzate of step (2), the concentration of nickel is 3-10 g / L, for example, 3 g / L, 5 g / L or 10 g / L, and the concentration of iron is less than 20 g / L, for example, 18 g / L, 10 g / L or 5 g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0026] The hydrolyzate of the present invention contains a relatively high concentration of nickel and a relatively low concentration of iron, which is beneficial to the subsequent preparation of battery-grade nickel compounds and also indicates that the iron removal efficiency of the present invention is relatively high.

[0027] Preferably, after the heating and hydrolysis in step (2), solid-liquid separation is also performed to obtain the iron slag and the hydrolyzate.

[0028] Preferably, the temperature for neutralizing the precipitated aluminum in step (3) is 40-80°C, for example, 40°C, 60°C or 80°C, and the time is 2-5h, for example, 2h, 3h or 5h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] Preferably, after the neutralization of aluminum precipitation in step (3), solid-liquid separation is also performed to obtain the aluminum slag and aluminum precipitation liquid.

[0030] Preferably, the regenerated magnesium oxide in step (4) is reused in the neutralization and aluminum precipitation process in step (3).

[0031] Preferably, the nickel deposition in step (4) includes a primary nickel deposition and a secondary nickel deposition performed sequentially.

[0032] Preferably, the secondary nickel precipitation obtains secondary nickel precipitation slag and the nickel precipitation liquid of step (4), and the secondary nickel precipitation slag is reused as a neutralizing agent in the neutralization aluminum precipitation process of step (3).

[0033] Preferably, the primary nickel precipitation slag obtained by the primary nickel precipitation includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate.

[0034] The present invention not only realizes the recovery of nickel-cobalt slag through two nickel precipitations, but also can use the secondary nickel precipitation slag as a neutralizer to neutralize the precipitated aluminum. Therefore, the refining of the primary nickel precipitation slag of the present invention obtains battery-grade nickel compounds, and the secondary nickel precipitation slag is fully recycled, further avoiding the addition of additional oxidants.

[0035] Preferably, the nickel precipitation agent used in the first nickel precipitation comprises the regenerated magnesium oxide described in step (4).

[0036] Preferably, the nickel deposition agent used in the secondary nickel deposition comprises the regenerated magnesium oxide described in step (4).

[0037] In the nickel precipitation process, the invention adopts the regenerated product finally obtained by the invention as the nickel precipitation agent, thus realizing the maximum application of resources.

[0038] Preferably, the hydrochloric acid in step (4) is reused in the leaching process in step (1).

[0039] The leaching method of the present invention finally obtains hydrochloric acid, thereby realizing the recycling of the hydrochloric acid.

[0040] Preferably, the pyrolysis temperature in step (4) is 600-800°C, for example, 600°C, 700°C or 800°C, and the time is 1-3h, for example, 1h, 2h or 3h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] As a preferred technical solution of the present invention, the leaching method comprises the following steps:

[0042] (1) mixing laterite nickel ore, hydrochloric acid and the hydrolyzate of step (2), and then leaching at a temperature of 80-120° C. for 1-3 hours, and performing solid-liquid separation after the leaching to obtain a leachate and silicon slag;

[0043] (2) heating the leaching solution of step (1) at a temperature of 130-180° C. for 2-5 hours, and then performing solid-liquid separation to obtain iron slag and hydrolyzed solution, wherein 20-50% of the hydrolyzed solution is reused in the leaching process of step (1);

[0044] In the hydrolyzate, the concentration of nickel is 3-10 g / L, and the concentration of iron is less than 20 g / L;

[0045] (3) neutralizing the remaining hydrolyzate of step (2) at a temperature of 40-80° C. for 2-5 hours to precipitate aluminum, and then performing solid-liquid separation to obtain aluminum slag and aluminum precipitate liquid;

[0046] (4) subjecting the aluminum precipitation liquid in step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation slag, secondary nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid to obtain regenerated magnesium oxide and hydrochloric acid;

[0047] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;

[0048] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation process and the secondary nickel precipitation process, and is also reused as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the hydrochloric acid obtained by pyrolysis is reused in the leaching process in step (1).

[0049] Compared with the prior art, the present invention has the following beneficial effects:

[0050] In view of the problems arising from the existing wet leaching process, the present invention treats laterite nickel ore by a method of normal pressure reaction, high temperature hydrolysis and partial return recycling, so the present invention has the following advantages:

[0051] (1) The present invention can obtain relatively pure silicon slag, iron slag and aluminum slag respectively, which reduces the pressure of subsequent waste slag treatment and is conducive to the final preparation of iron, aluminum and silicon products;

[0052] (2) The present invention can recycle part of the hydrochloric acid, reduce the amount of hydrochloric acid added, and reduce production costs;

[0053] (3) The hydrolyzate for subsequent neutralization treatment has high nickel and cobalt content, which can significantly reduce equipment investment;

[0054] (4) Most of the iron is removed by hydrolysis, avoiding the introduction of a large amount of neutralizing agent to generate iron hydroxide that is difficult to filter and easy to adsorb, simplifying the treatment process, reducing the introduction of impurities, and improving the recovery rate of nickel and cobalt;

[0055] (5) Using secondary nickel precipitation slag as a neutralizer for neutralizing aluminum precipitation, and using the manganese oxide in it to oxidize and precipitate iron, avoiding the introduction of other oxidants;

[0056] (6) The present invention has the advantages of simple process, can greatly reduce production cost and equipment investment, and can be applied on an industrial scale. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 This is a flow chart of the leaching method described in Example 1 of the present invention. DETAILED DESCRIPTION

[0058] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0059] Example 1

[0060] This embodiment provides a leaching method for laterite nickel ore, and the flow chart of the leaching method is as follows: Figure 1 As shown, the leaching method comprises the following steps:

[0061] (1) mixing the ground laterite nickel ore powder, 36% hydrochloric acid and the hydrolyzate of step (2), and then leaching in a reactor at a temperature of 105° C. for 2 h, and filtering after leaching to obtain a leachate and silicon slag;

[0062] (2) heating and hydrolyzing the leaching solution of step (1) at a temperature of 130° C. for 5 hours, and then filtering to obtain iron slag and hydrolyzate, wherein 40% of the hydrolyzate is reused in the leaching process of step (1);

[0063] (3) neutralizing the remaining 60% of the hydrolyzate in step (2) at 80° C. for 2 h to precipitate aluminum, and then filtering to obtain aluminum slag and aluminum precipitation liquid;

[0064] (4) subjecting the aluminum precipitation liquid in step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation slag, secondary nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid at 600° C. for 3 h to obtain regenerated magnesium oxide and hydrochloric acid;

[0065] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;

[0066] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation process and the secondary nickel precipitation process, and is also reused as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the hydrochloric acid obtained by pyrolysis is reused in the leaching process in step (1).

[0067] Example 2

[0068] This embodiment provides a leaching method for laterite nickel ore, the leaching method comprising the following steps:

[0069] (1) mixing the ground laterite nickel ore powder, 31% hydrochloric acid and the hydrolyzate of step (2), and then leaching in a reactor at a temperature of 120° C. for 3 h, and filtering after leaching to obtain a leachate and silicon slag;

[0070] (2) heating and hydrolyzing the leaching solution of step (1) at a temperature of 140° C. for 4 hours, and then filtering to obtain iron slag and hydrolyzate, wherein 30% of the hydrolyzate is reused in the leaching process of step (1);

[0071] (3) neutralizing the remaining 70% of the hydrolyzate in step (2) at 70° C. to precipitate aluminum for 2 hours, and then filtering to obtain aluminum slag and aluminum precipitation liquid;

[0072] (4) subjecting the aluminum precipitation liquid in step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation slag, secondary nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid at a temperature of 650° C. for 2.5 h to obtain regenerated magnesium oxide and hydrochloric acid;

[0073] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;

[0074] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation process and the secondary nickel precipitation process; the hydrochloric acid obtained by pyrolysis is reused in the leaching process of step (1).

[0075] Example 3

[0076] This embodiment provides a leaching method for laterite nickel ore, the leaching method comprising the following steps:

[0077] (1) mixing the ground laterite nickel ore powder, 33% hydrochloric acid and the hydrolyzate of step (2), and then leaching in a reactor at 90° C. for 1 h, filtering after leaching to obtain a leachate and silicon slag;

[0078] (2) heating and hydrolyzing the leaching solution of step (1) at a temperature of 180° C. for 3 hours, and then filtering to obtain iron slag and hydrolyzate, wherein 20% of the hydrolyzate is reused in the leaching process of step (1);

[0079] (3) neutralizing the remaining 80% of the hydrolyzate in step (2) at a temperature of 50° C. to precipitate aluminum for 5 hours, and then filtering to obtain aluminum slag and aluminum precipitation liquid;

[0080] (4) subjecting the aluminum precipitation liquid in step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation slag, secondary nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid at 700° C. for 2 h to obtain regenerated magnesium oxide and hydrochloric acid;

[0081] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;

[0082] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation process and the secondary nickel precipitation process; the hydrochloric acid obtained by pyrolysis is reused in the leaching process of step (1).

[0083] Example 4

[0084] This embodiment provides a leaching method for laterite nickel ore, the leaching method comprising the following steps:

[0085] (1) mixing the ground laterite nickel ore powder, 36% hydrochloric acid and the hydrolyzate of step (2), and then leaching in a reactor at a temperature of 105° C. for 1 hour, filtering after the leaching, and obtaining a leachate and silicon slag;

[0086] (2) heating and hydrolyzing the leaching solution of step (1) at a temperature of 150° C. for 3 hours, and then filtering to obtain iron slag and hydrolyzate, wherein 50% of the hydrolyzate is reused in the leaching process of step (1);

[0087] (3) neutralizing the remaining 50% of the hydrolyzate in step (2) at 40° C. for 2 h to precipitate aluminum, and then filtering to obtain aluminum slag and aluminum precipitation liquid;

[0088] (4) subjecting the aluminum precipitation liquid of step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation slag, secondary nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid at 750° C. for 1.5 h to obtain regenerated magnesium oxide and hydrochloric acid;

[0089] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;

[0090] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation process and the secondary nickel precipitation process; the hydrochloric acid obtained by pyrolysis is reused in the leaching process of step (1).

[0091] Example 5

[0092] This embodiment provides a leaching method for laterite nickel ore, the leaching method comprising the following steps:

[0093] (1) mixing the ground laterite nickel ore powder, 30% hydrochloric acid and the hydrolyzate of step (2), and then leaching in a reactor at a temperature of 120° C. for 2 h, and filtering after leaching to obtain a leachate and silicon slag;

[0094] (2) heating and hydrolyzing the leaching solution of step (1) at a temperature of 160° C. for 1 hour, and then filtering to obtain iron slag and hydrolyzate, wherein 40% of the hydrolyzate is reused in the leaching process of step (1);

[0095] (3) neutralizing the remaining 60% of the hydrolyzate in step (2) at 80° C. for 2 h to precipitate aluminum, and then filtering to obtain aluminum slag and aluminum precipitation liquid;

[0096] (4) subjecting the aluminum precipitation liquid in step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation slag, secondary nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid at 800° C. for 1 h to obtain regenerated magnesium oxide and hydrochloric acid;

[0097] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;

[0098] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation process and the secondary nickel precipitation process; the hydrochloric acid obtained by pyrolysis is reused in the leaching process of step (1).

[0099] Example 6

[0100] This embodiment provides a leaching method for laterite nickel ore, the leaching method comprising the following steps:

[0101] (1) mixing the ground laterite nickel ore powder, 33% hydrochloric acid and the hydrolyzate of step (2), and then leaching in a reactor at a temperature of 105° C. for 2 h, filtering after the leaching, and obtaining a leachate and silicon slag;

[0102] (2) heating and hydrolyzing the leaching solution of step (1) at a temperature of 150° C. for 5 hours, and then filtering to obtain iron slag and hydrolyzate, wherein 40% of the hydrolyzate is reused in the leaching process of step (1);

[0103] (3) neutralizing the remaining 60% of the hydrolyzate in step (2) at 60° C. to precipitate aluminum for 4 hours, and then filtering to obtain aluminum slag and aluminum precipitation liquid;

[0104] (4) subjecting the aluminum precipitation liquid in step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation slag, secondary nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid at a temperature of 650° C. for 2 h to obtain regenerated magnesium oxide and hydrochloric acid;

[0105] The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate;

[0106] The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation process and the secondary nickel precipitation process; the hydrochloric acid obtained by pyrolysis is reused in the leaching process of step (1).

[0107] Example 7

[0108] This embodiment provides a method for leaching laterite nickel ore, which is the same as that of Embodiment 1 except that the hydrolyzate of step (2) is not added in step (1), and the hydrolyzate is not recycled but replaced by hydrochloric acid of the same acid concentration.

[0109] Example 8

[0110] This embodiment provides a method for leaching laterite nickel ore, which is the same as that of Embodiment 1 except that the temperature of the heating hydrolysis in step (2) is 110°C.

[0111] Example 9

[0112] This embodiment provides a method for leaching laterite nickel ore, which is the same as that of Embodiment 1 except that the temperature of the heating hydrolysis in step (2) is 200°C.

[0113] Example 10

[0114] The present embodiment provides a method for leaching laterite nickel ore, which is the same as that of Example 1 except that the nickel precipitating agent used in the first and second nickel precipitating in step (4) is commercial magnesium oxide, and the regenerated magnesium oxide in step (4) is not reused as a nickel precipitating agent.

[0115] Embodiment 11

[0116] This embodiment provides a method for leaching laterite nickel ore, which is the same as that of Embodiment 1 except that the hydrochloric acid in step (4) is not recycled to step (1) and the hydrochloric acid in step (1) is commercial hydrochloric acid.

[0117] Comparative Example 1

[0118] This comparative example provides a method for leaching laterite nickel ore, which is the same as Example 1 except that in step (2), magnesium oxide is added for precipitation to remove iron instead of heating and hydrolysis.

[0119] Comparative Example 2

[0120] This comparative example provides a leaching method for laterite nickel ore, which is the same as Example 1 except that the neutralizing agent used in the neutralization of aluminum precipitation in step (3) is commercial magnesium oxide, and the secondary nickel precipitation slag and regenerated magnesium oxide are not recycled.

[0121] The nickel concentration and iron concentration in the hydrolyzate of step (2) in the above embodiments and comparative examples, the iron concentration in the feed solution after aluminum precipitation in step (3) and the total nickel recovery rate are shown in the following table:

[0122] Table 1

[0123]

[0124]

[0125] From Table 1 we can see that:

[0126] (1) The leaching method of the present invention can obtain a leachate with a high nickel content, and at the same time, the overall nickel recovery rate is increased, and the problem of the need to add a large amount of neutralizer and oxidant in the prior art is overcome; it can be seen from Examples 1 and 7 that the present invention removes iron by heating hydrolysis, and the obtained hydrolyzate can be reused in step (1) without affecting the final result; it can be seen from Examples 1 and 8-9 that the temperature of the heating hydrolysis of the present invention will affect the efficiency of iron removal, the nickel concentration and the nickel recovery rate; it can be seen from Examples 1 and 10 that in the first and second nickel precipitation processes of the present invention, the final regenerated magnesium oxide is used. Compared with the additionally added commercial magnesium oxide, it can be seen that the use of regenerated magnesium oxide as a nickel precipitation agent will not have a significant impact on the results of the present invention.

[0127] (2) It can be seen from Example 1 and Example 11 that when the hydrochloric acid obtained in step (4) is reused in step (1), a good recovery result is still obtained, and the overall process is not affected; it can be seen from Example 1 and Comparative Example 1 that Comparative Example 1 uses a conventional method to remove iron, which will generate difficult-to-filter substances, introduce impurities, and increase the reaction time. In addition, since most of the neutralizing agent is added in the form of slurry, the concentration of nickel and cobalt in the solution after iron removal will be reduced, affecting the recovery effect of the overall process and increasing the cost. The present invention can avoid the addition of the neutralizing agent by heating and hydrolysis, and at the same time increase the content of nickel and cobalt in the leachate; it can be seen from Example 1 and Comparative Example 2 that the present invention uses secondary nickel precipitation slag as a neutralizing agent, and can use the manganese oxide therein to oxidize and precipitate iron, thereby avoiding the introduction of other oxidants as much as possible, which not only reduces the cost but also improves the efficiency of the overall process.

[0128] In summary, the present invention provides a leaching method for laterite nickel ore, which can significantly reduce the solution processing volume, reduce the addition of neutralizing agent and the number of neutralization times, increase the nickel ion concentration in the solution, reduce the overall equipment investment, and reduce production costs.

[0129] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A leaching method for laterite nickel ore, characterized in that: The leaching method comprises the following steps: (1) mixing laterite nickel ore with hydrochloric acid, and then leaching to obtain leachate and leached residue; (2) heating and hydrolyzing the leaching solution of step (1) to obtain iron slag and hydrolyzate; (3) neutralizing the hydrolyzate obtained in step (2) and precipitating aluminum to obtain aluminum slag and aluminum precipitation liquid; (4) subjecting the aluminum precipitation liquid in step (3) to nickel precipitation to obtain nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid to obtain regenerated magnesium oxide and hydrochloric acid; The nickel precipitation slag is recycled for the neutralization and aluminum precipitation process in step (3).

2. The leaching method according to claim 1, characterized in that The hydrolyzate of step (2) is also added during the mixing process of step (1); Preferably, the concentration of the hydrochloric acid in step (1) is above 30%; Preferably, after the leaching in step (1), solid-liquid separation is further performed to obtain the leaching solution and leaching residue; Preferably, the leached slag in step (1) comprises silicon slag.

3. The leaching method according to claim 1 or 2, characterized in that: The leaching temperature in step (1) is 80-120° C. and the leaching time is 1-3 h; Preferably, the leaching in step (1) is carried out in a reactor.

4. The leaching method according to any one of claims 1 to 3, characterized in that: The heating and hydrolysis in step (2) is carried out at a temperature of 130-180° C. and a time of 2-5 h; Preferably, 20-50% of the hydrolyzate in step (2) is recycled to the leaching process in step (1).

5. The leaching method according to any one of claims 1 to 4, characterized in that: In the hydrolyzate of step (2), the concentration of nickel is 3-10 g / L, and the concentration of iron is less than 20 g / L; Preferably, after the heating and hydrolysis in step (2), solid-liquid separation is also performed to obtain the iron slag and the hydrolyzate.

6. The leaching method according to any one of claims 1 to 5, characterized in that: The temperature of neutralizing the aluminum precipitation in step (3) is 40-80°C and the time is 2-5h; Preferably, after the neutralization of aluminum precipitation in step (3), solid-liquid separation is also performed to obtain the aluminum slag and aluminum precipitation liquid.

7. The leaching method according to any one of claims 1 to 6, characterized in that: The regenerated magnesium oxide in step (4) is reused in the neutralization and aluminum precipitation process in step (3); Preferably, the nickel deposition in step (4) comprises a primary nickel deposition and a secondary nickel deposition performed sequentially; Preferably, the secondary nickel precipitation obtains secondary nickel precipitation slag and the nickel precipitation liquid of step (4), and the secondary nickel precipitation slag is used as a neutralizing agent back to the neutralization aluminum precipitation process of step (3); Preferably, the primary nickel precipitation slag obtained by the primary nickel precipitation includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate.

8. The leaching method according to claim 7, characterized in that The nickel precipitation agent used in the first nickel precipitation comprises the regenerated magnesium oxide described in step (4); Preferably, the nickel deposition agent used in the secondary nickel deposition comprises the regenerated magnesium oxide described in step (4).

9. The leaching method according to any one of claims 1 to 8, characterized in that: The hydrochloric acid in step (4) is reused in the leaching process in step (1); Preferably, the pyrolysis temperature in step (4) is 600-800° C. and the time is 1-3 h.

10. The leaching method according to any one of claims 1 to 9, characterized in that: The leaching method comprises the following steps: (1) mixing laterite nickel ore, hydrochloric acid and the hydrolyzate of step (2), and then leaching at a temperature of 80-120° C. for 1-3 hours, and performing solid-liquid separation after the leaching to obtain a leachate and silicon slag; (2) heating the leaching solution of step (1) at a temperature of 130-180° C. for 2-5 hours, and then performing solid-liquid separation to obtain iron slag and hydrolyzed solution, wherein 20-50% of the hydrolyzed solution is reused in the leaching process of step (1); In the hydrolyzate, the concentration of nickel is 3-10 g / L, and the concentration of iron is less than 20 g / L; (3) neutralizing the remaining hydrolyzate of step (2) at a temperature of 40-80° C. for 2-5 hours to precipitate aluminum, and then performing solid-liquid separation to obtain aluminum slag and aluminum precipitate liquid; (4) subjecting the aluminum precipitation liquid in step (3) to primary nickel precipitation and secondary nickel precipitation in sequence to obtain primary nickel precipitation slag, secondary nickel precipitation slag and nickel precipitation liquid, and pyrolyzing the nickel precipitation liquid to obtain regenerated magnesium oxide and hydrochloric acid; The secondary nickel precipitation slag is used as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the primary nickel precipitation slag includes nickel-cobalt slag, and the nickel-cobalt slag is refined to obtain battery-grade nickel sulfate; The regenerated magnesium oxide is reused as a nickel precipitation agent in the primary nickel precipitation process and the secondary nickel precipitation process, and is also reused as a neutralizing agent in the neutralization aluminum precipitation process in step (3); the hydrochloric acid obtained by pyrolysis is reused in the leaching process in step (1).

Citation Information

Patent Citations

  • Method for processing nickel cobalt extracted from laterite-nickel ore by chloride cycle desiliconisation ferrous process

    CN101328548A

  • Method for comprehensive exploitation of low-ore grade laterite nickel mine

    CN101403035A

  • Comprehensive method for processing laterite nickel ore to produce electrolytic nickel through full wet method

    CN102329955A

  • Method for recovering hydrochloric acid and metal oxides from metal chloride solution

    CN105776140A

  • Method for extracting nickel-cobalt from laterite nickel ore by utilizing hydrochloric acid leaching

    CN109457111A