Ruthenium monatomic catalyst, preparation method thereof and application of ruthenium monatomic catalyst in water electrolysis hydrogen production
By using a ruthenium single-atom catalyst on a cobalt vanadium phosphorus nanoneedle carrier in the electrolysis of water to produce hydrogen, the problem of insufficient activity of the existing catalyst is solved, efficient electrolysis of water for hydrogen evolution is achieved, the cost is reduced and the catalytic performance is improved, demonstrating The excellent performance of ruthenium single atom catalyst in alkaline environment.
Patent Information
- Application Number
- CN202410800559.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-29
AI Technical Summary
Existing single-atom catalysts have insufficient catalytic activity in the electrolysis of water to produce hydrogen, and cannot effectively replace the precious metal platinum. They are also costly and have poor applicability.
A nanoneedle structure catalyst composed of a cobalt vanadium phosphorus nanoneedle carrier and a ruthenium single atom loaded on the vanadium phosphorus nanoneedle is used. Through a specific preparation method, the cobalt vanadium nanoneedle is grown on a nickel foam substrate and loaded with a ruthenium single atom to form ruthenium. Single atom catalyst for electrolyzing water and hydrogen evolution reaction in alkaline environment.
It achieves stable loading and efficient catalysis of ruthenium single atoms, reduces the amount of precious metals, improves catalytic performance and atomic utilization, reduces hydrogen production costs, and shows better catalytic performance than Pt/C in an alkaline environment.
Smart Images

Figure HDA0004903256300000011 
Figure HDA0004903256300000012 
Figure HDA0004903256300000013
Abstract
Description
Technical Field
[0001] The invention relates to a ruthenium single-atom catalyst and a preparation method thereof and application thereof in hydrogen production by electrolysis of water, belonging to the technical field of hydrogen production by electrolysis of water. Background Art
[0002] As a clean energy with high combustion calorific value and good renewability, hydrogen energy has attracted great attention in recent years. Hydrogen produced by coupling renewable energy (such as photovoltaic and wind power) with water electrolysis is called "green hydrogen", which can convert abundant but discrete energy into concentrated and stable chemical energy, and thus has incomparable advantages in energy storage.
[0003] Electrolyzers based on anion exchange membrane technology are considered to be an important candidate for the next generation of water electrolysis technology. They can not only achieve high electrolysis efficiency of membrane electrolyzers, but also their alkaline working environment can significantly reduce the electrolyzer's dependence on precious metals. At present, the maturity of this technology is relatively low, and the development of efficient and stable catalysts is one of the core issues that need to be solved urgently.
[0004] Research has shown that transition metal phosphides have great potential for hydrogen evolution, but to date, there is still a significant gap between their catalytic activity and that of the precious metal platinum (Pt), and it is not possible to replace precious metals for the time being. However, the cost of Pt is very high, and its reserves are relatively small, making it unsuitable for large-scale application.
[0005] In recent years, single atom catalysts (SACs) in which active metals are dispersed on supports at the atomic level have become a new frontier in the field of catalytic science and have attracted widespread research attention. Single atom catalysts can maximize the utilization of metal atoms and have the advantages of both homogeneous catalysts and heterogeneous catalysts. They not only show great potential to bridge the gap between the two, but are also used in many important energy reactions and industrial chemical synthesis. In addition, the singleness and homogeneity of their structure also help to fully understand the relationship between catalyst structure and performance, and realize the rational catalyst design for atomic-level target reactions. However, there are still many problems that need to be solved in single atom catalysts, the most critical of which is that the hydrogen evolution performance of most single atom catalysts currently developed is not comparable to that of Pt. Summary of the invention
[0006] In view of the problem of insufficient activity of existing single-atom catalysts, the present invention proposes a ruthenium single-atom catalyst and its preparation method and application in hydrogen production by electrolysis of water. The ruthenium single-atom catalyst of the present invention has excellent catalytic activity and stability in the hydrogen evolution reaction by electrolysis of water in an alkaline environment. Compared with traditional Pt / C catalysts, the catalyst can significantly reduce the amount of precious metals used, reduce costs, and improve atomic utilization.
[0007] A ruthenium single atom catalyst is a nano-needle structure catalyst composed of a cobalt vanadium phosphorus nano-needle carrier and an active component ruthenium single atom loaded on the vanadium phosphorus nano-needle carrier, wherein the substrate of the cobalt vanadium phosphorus nano-needle carrier is foamed nickel.
[0008] The chemical formula of the cobalt vanadium phosphorus nanoneedle carrier is Co x VP, where 1≤x≤5.
[0009] The preparation method of the ruthenium single atom catalyst comprises the following specific steps:
[0010] (1) dissolving cobalt salt, vanadium salt, urea and ammonium fluoride in deionized water to obtain a mixed solution;
[0011] (2) immersing a nickel foam substrate (NF) in the mixed solution and reacting the solution at a temperature of 90 to 160° C. under a closed condition for 6 to 24 hours to grow cobalt-vanadium nanoneedles on the surface of the nickel foam substrate to obtain cobalt-vanadium nanoneedles / nickel foam substrate CoV-LDH;
[0012] (3) Cobalt-vanadium nanoneedles / nickel foam substrate CoV-LDH was placed in a ruthenium salt solution for surface chemical reaction to obtain cobalt-vanadium nanoneedles / nickel foam substrate Ru loaded with single ruthenium atoms SA -CoV-LDH;
[0013] (4) Sodium hypophosphite and cobalt vanadium nanoneedles / nickel foam substrate loaded with ruthenium single atoms were prepared. SA -CoV-LDH was placed in a tube furnace, and a protective gas was introduced to calcine to obtain a ruthenium single atom catalyst Ru SA -CoVP.
[0014] In step (1), the cobalt salt is one or more of cobalt nitrate, cobalt sulfate, and cobalt chloride, the vanadium salt is one or more of vanadyl sulfate, vanadium chloride, and ammonium metavanadate, and the molar ratio of the cobalt salt to the vanadium salt is (1 to 5).1.
[0015] Preferably, the molar ratio of urea to ammonium fluoride in step (1) is 1:(1-3).
[0016] In the mixed solution of step (1), the molar concentration of the cobalt salt is 0.001-0.1 mol / L, the molar concentration of the vanadium salt is 0.001-0.1 mol / L, the molar concentration of the urea is 0.1-1 mol / L, and the molar concentration of the ammonium fluoride is 0.1-1 mol / L.
[0017] The concentration of the ruthenium salt solution in step (3) is 1-10 mmol / L, the ruthenium salt is one or more of ruthenium sulfate, ruthenium chloride, and potassium ruthenate, the temperature of the surface chemical reaction is 25-35° C., and the time is 6-8 hours.
[0018] According to the gas flow direction of the protective gas, the sodium hypophosphite in step (4) is located upstream of the cobalt vanadium nanoneedle / nickel foam substrate loaded with ruthenium single atoms.
[0019] Preferably, in step (4), the protective gas flow rate is 10 to 200 sccm, the calcination temperature is 300 to 400° C., and the calcination time is 60 to 180 min.
[0020] The application of the ruthenium single atom catalyst in catalyzing the hydrogen evolution reaction in alkaline water electrolysis: during the electrolysis process, the OH- concentration in water is 0.1 to 6 mol / L.
[0021] The beneficial effects of the present invention are:
[0022] (1) The ruthenium single-atom catalyst of the present invention realizes the stable loading of ruthenium single atoms, exposes more catalytic reaction active sites, improves the catalytic performance, and improves the utilization rate of the catalyst and reduces the cost of hydrogen production; adopts a double transition metal phosphide substrate, which has an adjustable electronic structure, variable component composition and high conductivity, which can improve the efficiency of the catalyst; adopts a non-powder-based hydrogen evolution catalyst, and the preparation process does not require the addition of conductive carbon black and binder; adopts commercial nickel foam as the substrate, which further reduces the cost of materials;
[0023] (2) Compared with Pt, the present invention uses relatively cheap ruthenium as the active site, and through the synergistic effect with the double transition metal phosphide substrate, it achieves a catalytic performance better than Pt / C in the alkaline electrocatalytic hydrogen evolution reaction, and only 66 mV overpotential is required to generate 100 mA / cm 2 Current density. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Example 1 Ru SA -SEM image of Co4VP catalyst nanoneedles, (a) Ru SA -Partial image of Co4VP catalyst nanoneedles, (b) Ru SA -Partial magnified image of Co4VP catalyst nanoneedles;
[0025] Figure 2 Example 1 Ru SA - Spherical aberration corrected transmission electron microscopy image of Co4VP catalyst;
[0026] Figure 3 Example 1 Ru SA -Linear sweep voltammetry curve of Co4VP catalyst and comparison with commercial Pt / C;
[0027] Figure 4 Example 1 Ru SA-Co4VP catalyst at 20, 50 and 100 mA cm -2 Chronopotentiographs at current density;
[0028] Figure 5 Example 1 Ru SA -Comparison of the linear sweep voltammetric curves of Co4VP catalyst in the initial state and after 5000 CV cycles during the catalytic reaction;
[0029] Figure 6 Example 2 Ru SA -Linear sweep voltammetry curve of Co5VP catalyst and comparison with commercial Pt / C;
[0030] Figure 7 Example 3 Ru SA -Linear sweep voltammetry curve of Co3VP catalyst and comparison with commercial Pt / C;
[0031] Figure 8 Example 4 Ru SA -Linear sweep voltammetry curve of Co2VP catalyst and comparison with commercial Pt / C;
[0032] Fig. 9 Example 5 Ru SA -Linear sweep voltammetry curves of Co1VP catalyst and comparison with commercial Pt / C. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0034] Example 1: The ruthenium single atom catalyst of this example is a nanoneedle structure catalyst composed of a cobalt vanadium phosphorus nanoneedle carrier and an active component ruthenium single atom loaded on the vanadium phosphorus nanoneedle carrier, wherein the substrate of the cobalt vanadium phosphorus nanoneedle carrier is nickel foam; the chemical formula of the cobalt vanadium phosphorus nanoneedle carrier is Co x VP, x = 4;
[0035] A method for preparing a ruthenium single-atom catalyst, the specific steps are as follows:
[0036] (1) Dissolving Co(NO3)2·6H2O, VCl3, urea and ammonium fluoride in deionized water to obtain a mixed solution; the molar concentration of cobalt salt in the mixed solution is 0.04 mol / L, the molar concentration of vanadium salt is 0.01 mol / L, the molar concentration of urea is 0.25 mol / L, and the molar concentration of ammonium fluoride is 0.15 mol / L;
[0037] (2) A nickel foam substrate (NF) with a size of 2 cm × 3 cm was ultrasonically cleaned with ethanol and deionized water in turn, ultrasonically activated in dilute hydrochloric acid with a concentration of 0.1 mol / L for 20 min, and then ultrasonically cleaned with deionized water to obtain an activated nickel foam substrate (NF). The activated nickel foam substrate (NF) was then immersed in the mixed solution and reacted at a temperature of 120°C under closed conditions for 12 h to grow cobalt-vanadium nanoneedles on the surface of the activated nickel foam substrate (NF). The substrate was cooled to room temperature, and then cleaned with deionized water and anhydrous ethanol in turn, and vacuum dried to obtain cobalt-vanadium nanoneedles / nickel foam substrate Co4V-LDH.
[0038] (3) Cobalt vanadium nanoneedles / nickel foam substrate Co4V-LDH was placed in a RuCl3 solution with a concentration of 4.8 mmol / L and subjected to surface chemical reaction at 25°C for 8 h. The excess RuCl3 solution was then removed by washing with deionized water and anhydrous ethanol, and vacuum dried to obtain cobalt vanadium nanoneedles / nickel foam substrate Ru loaded with single ruthenium atoms. SA -Co4V-LDH;
[0039] (4) Sodium hypophosphite and cobalt vanadium nanoneedles / nickel foam substrate loaded with ruthenium single atoms were prepared. SA -Co4V-LDH was placed at both ends of the ceramic boat, and then the ceramic boat was placed in a tube furnace to evacuate the air, and then high-purity argon gas (gas flow rate 80sccm) was introduced, and the temperature was uniformly increased to 350°C at a heating rate of 5.5°C / min, and calcined at 350°C for 120min, and then cooled to room temperature to obtain a ruthenium single atom catalyst Ru SA -Co4VP; according to the gas flow direction of high-purity argon, the sodium hypophosphite is located upstream of the cobalt vanadium nanoneedle / nickel foam substrate loaded with ruthenium single atoms;
[0040] This embodiment Ru SA -SEM image of Co4VP catalyst nanoneedles Figure 1 , (a) is Ru SA -Partial image of Co4VP catalyst nanoneedles, (b) Ru SA -Local magnified image of Co4VP catalyst nanoneedles; RuS nanoneedles are evenly distributed on the nickel foam substrate A -Co4VP;
[0041] This embodiment Ru SA -Spherical aberration corrected transmission electron microscopy image of Co4VP catalyst is shown in Figure 2 , the bright spots (single ruthenium atoms) are evenly distributed on the surface of the carrier Co4VP, and the catalyst is a single atom catalyst;
[0042] In this embodiment Ru SA-Co4VP catalyst was used as the working electrode, graphite electrode as the counter electrode, and Ag / AgCl as the reference electrode, and alkaline electrocatalytic hydrogen evolution was carried out in a potassium hydroxide solution system with a concentration of 1 mol / L;
[0043] Activity test: Linear sweep voltammetry (LSV) curve test was carried out in the voltage range of -0.8 to -1.7 V vs Ag / AgCl; Ru SA -Linear sweep voltammetry curve of Co4VP catalyst and comparison with commercial Pt / C are shown in Figure 3 , this embodiment Ru SA -Co4VP catalyst at -100mA / cm 2 The overpotential of hydrogen evolution at the current density is 66 mV;
[0044] Stability test: Perform chronopotentiometry and set the current density to 10 mA cm -2 , 20mA cm -2 , 50mA cm -2 , test time 150h, record the voltage curve under constant current density for 150h Figure 4 ,from Figure 4 It can be seen that in this embodiment Ru SA -Co4VP catalyst has good performance at current densities of 10, 20, 30 and 50 mA / cm 2 When , the potential increase of continuous electrocatalysis is negligible, indicating that it can be applied in various working conditions;
[0045] Cyclic stability test: CV cycle test, Ru SA -The LSV comparison curves of the initial state of the Co4VP catalyst during the catalytic reaction and after 5000 CV cycles are shown in Figure 5 ,from Figure 5 It can be seen that in this embodiment Ru SA The LSV curve of the -Co4VP catalyst after 5000 CV cycles almost overlaps with the initial curve, proving that Ru SA -Co4VP electrocatalyst has excellent durability.
[0046] Example 2: The ruthenium single atom catalyst of this example is a nanoneedle structure catalyst composed of a cobalt vanadium phosphorus nanoneedle carrier and an active component ruthenium single atom loaded on the vanadium phosphorus nanoneedle carrier, wherein the substrate of the cobalt vanadium phosphorus nanoneedle carrier is nickel foam; the chemical formula of the cobalt vanadium phosphorus nanoneedle carrier is Co x VP, x = 5;
[0047] A method for preparing a ruthenium single-atom catalyst, the specific steps are as follows:
[0048] (1) Dissolving Co(NO3)2·6H2O, VCl3, urea and ammonium fluoride in deionized water to obtain a mixed solution; the molar concentration of cobalt salt in the mixed solution is 0.05 mol / L, the molar concentration of vanadium salt is 0.01 mol / L, the molar concentration of urea is 0.25 mol / L, and the molar concentration of ammonium fluoride is 0.15 mol / L;
[0049] (2) A nickel foam substrate (NF) with a size of 2 cm × 3 cm was ultrasonically cleaned with ethanol and deionized water in turn, ultrasonically activated in dilute hydrochloric acid with a concentration of 0.15 mol / L for 25 min, and then ultrasonically cleaned with deionized water to obtain an activated nickel foam substrate (NF). The activated nickel foam substrate (NF) was then immersed in the mixed solution and reacted at a temperature of 120 ° C under closed conditions for 12 h to grow cobalt vanadium nanoneedles on the surface of the activated nickel foam substrate (NF). The substrate was cooled to room temperature, and then cleaned with deionized water and anhydrous ethanol in turn, and vacuum dried to obtain cobalt vanadium nanoneedles / nickel foam substrate Co5V_LDH;
[0050] (3) Cobalt-vanadium nanoneedles / nickel foam substrate Co5V-LDH was placed in a RuCl3 solution with a concentration of 4.8 mmol / L and subjected to surface chemical reaction at 30°C for 7 h. The excess RuCl3 solution was then removed by washing with deionized water and anhydrous ethanol, and vacuum dried to obtain cobalt-vanadium nanoneedles / nickel foam substrate Ru loaded with single ruthenium atoms. SA -Co5V-LDH;
[0051] (4) Sodium hypophosphite and cobalt vanadium nanoneedles / nickel foam substrate loaded with ruthenium single atoms were prepared. SA -Co5V-LDH was placed at both ends of the ceramic boat, and then the ceramic boat was placed in a tube furnace to evacuate the air, and then high-purity nitrogen (gas flow rate 50sccm) was introduced, and the temperature was uniformly increased to 300°C at a heating rate of 5°C / min, and calcined at 300°C for 180min, and then cooled to room temperature to obtain a ruthenium single atom catalyst Ru SA -Co5VP; according to the gas flow direction of high-purity argon, the sodium hypophosphite is located upstream of the cobalt vanadium nanoneedle / foam nickel substrate loaded with ruthenium single atoms;
[0052] In this embodiment, RuS A -Co5VP catalyst was used as the working electrode, graphite electrode as the counter electrode, and Ag / AgCl as the reference electrode, and alkaline electrocatalytic hydrogen evolution was carried out in a potassium hydroxide solution system with a concentration of 1 mol / L;
[0053] Activity test: Linear sweep voltammetry (LSV) curve test was performed in the voltage range of -0.8 to -1.7 V vs Ag / AgCl; SA -Co5VP electrocatalyst at -100mA / cm 2The overpotential of hydrogen evolution at this current density is 81 mV.
[0054] Example 3: The ruthenium single atom catalyst of this example is a nanoneedle structure catalyst composed of a cobalt vanadium phosphorus nanoneedle carrier and an active component ruthenium single atom loaded on the vanadium phosphorus nanoneedle carrier, wherein the substrate of the cobalt vanadium phosphorus nanoneedle carrier is nickel foam; the chemical formula of the cobalt vanadium phosphorus nanoneedle carrier is Co x VP, x = 3;
[0055] A method for preparing a ruthenium single-atom catalyst, the specific steps are as follows:
[0056] (1) Dissolving Co(NO3)2·6H2O, VCl3, urea and ammonium fluoride in deionized water to obtain a mixed solution; the molar concentration of cobalt salt in the mixed solution is 0.03 mol / L, the molar concentration of vanadium salt is 0.01 mol / L, the molar concentration of urea is 0.25 mol / L, and the molar concentration of ammonium fluoride is 0.15 mol / L;
[0057] (2) A nickel foam substrate (NF) with a size of 2 cm × 3 cm was ultrasonically cleaned with ethanol and deionized water in turn, ultrasonically activated in dilute hydrochloric acid with a concentration of 0.18 mol / L for 15 min, and then ultrasonically cleaned with deionized water to obtain an activated nickel foam substrate (NF). The activated nickel foam substrate (NF) was then immersed in the mixed solution and reacted at a temperature of 120 ° C under closed conditions for 12 h to grow cobalt vanadium nanoneedles on the surface of the activated nickel foam substrate (NF). The substrate was cooled to room temperature, and then cleaned with deionized water and anhydrous ethanol in turn, and vacuum dried to obtain cobalt vanadium nanoneedles / nickel foam substrate Co3V-LDH.
[0058] (3) Cobalt vanadium nanoneedles / nickel foam substrate Co3V-LDH was placed in a RuCl3 solution with a concentration of 4.8 mmol / L and subjected to surface chemical reaction at 35°C for 6 h. The excess RuCl3 solution was then removed by washing with deionized water and anhydrous ethanol, and vacuum dried to obtain cobalt vanadium nanoneedles / nickel foam substrate Ru loaded with single ruthenium atoms. SA -Co3V-LDH;
[0059] (4) Sodium hypophosphite and cobalt vanadium nanoneedles / nickel foam substrate loaded with ruthenium single atoms were prepared. SA -Co3V-LDH was placed at both ends of the ceramic boat, and then the ceramic boat was placed in a tube furnace to evacuate the air, and then high-purity argon gas (gas flow rate 120sccm) was introduced, and the temperature was uniformly increased to 380°C at a heating rate of 6°C / min, and calcined at 380°C for 100min, and then cooled to room temperature to obtain a ruthenium single atom catalyst Ru SA -Co3VP; according to the gas flow direction of high-purity argon, the sodium hypophosphite is located upstream of the cobalt vanadium nanoneedle / foam nickel substrate loaded with ruthenium single atoms;
[0060] In this embodiment Ru SA -Co3VP catalyst was used as the working electrode, graphite electrode as the counter electrode, and Ag / AgCl as the reference electrode, and alkaline electrocatalytic hydrogen evolution was carried out in a potassium hydroxide solution system with a concentration of 1 mol / L;
[0061] Activity test: Linear sweep voltammetry (LSV) curve test was performed in the voltage range of -0.8 to -1.7 V vs Ag / AgCl; SA -Co3VP electrocatalyst at -100mA / cm 2 The overpotential of hydrogen evolution at this current density is 71 mV.
[0062] Example 4: The ruthenium single atom catalyst of this example is a nanoneedle structure catalyst composed of a cobalt vanadium phosphorus nanoneedle carrier and a ruthenium single atom as an active component loaded on the vanadium phosphorus nanoneedle carrier. The substrate of the cobalt vanadium phosphorus nanoneedle carrier is nickel foam. The chemical formula of the cobalt vanadium phosphorus nanoneedle carrier is Co x VP, x = 2;
[0063] A method for preparing a ruthenium single-atom catalyst, the specific steps are as follows:
[0064] (1) Dissolving Co(NO3)2·6H2O, VCl3, urea and ammonium fluoride in deionized water to obtain a mixed solution; the molar concentration of cobalt salt in the mixed solution is 0.02 mol / L, the molar concentration of vanadium salt is 0.01 mol / L, the molar concentration of urea is 0.25 mol / L, and the molar concentration of ammonium fluoride is 0.15 mol / L;
[0065] (2) A nickel foam substrate (NF) with a size of 2 cm × 3 cm was ultrasonically cleaned with ethanol and deionized water in turn, ultrasonically activated in dilute hydrochloric acid with a concentration of 0.1 mol / L for 20 min, and then ultrasonically cleaned with deionized water to obtain an activated nickel foam substrate (NF). The activated nickel foam substrate (NF) was then immersed in the mixed solution and reacted at a temperature of 120°C under closed conditions for 12 h to grow cobalt-vanadium nanoneedles on the surface of the activated nickel foam substrate (NF). The substrate was cooled to room temperature, and then cleaned with deionized water and anhydrous ethanol in turn, and vacuum dried to obtain cobalt-vanadium nanoneedles / nickel foam substrate Co2V-LDH.
[0066] (3) Cobalt-vanadium nanoneedles / nickel foam substrate Co2V-LDH was placed in a RuCl3 solution with a concentration of 4.8 mmol / L and subjected to surface chemical reaction at 25°C for 6 h. The excess RuCl3 solution was then removed by washing with deionized water and anhydrous ethanol, and vacuum dried to obtain cobalt-vanadium nanoneedles / nickel foam substrate Ru loaded with single ruthenium atoms. SA -Co2V-LDH;
[0067] (4) Sodium hypophosphite and cobalt vanadium nanoneedles / nickel foam substrate loaded with ruthenium single atoms were prepared. SA -Co2V-LDH was placed at both ends of the ceramic boat, and then the ceramic boat was placed in a tube furnace to evacuate the air, and then high-purity argon gas (gas flow rate 150sccm) was introduced, and the temperature was uniformly increased to 350℃ at a heating rate of 6℃ / min, and calcined at 350℃ for 140min, and then cooled to room temperature to obtain a ruthenium single atom catalyst Ru SA -Co2VP; according to the gas flow direction of high-purity argon, the sodium hypophosphite is located upstream of the cobalt vanadium nanoneedle / foam nickel substrate loaded with ruthenium single atoms;
[0068] In this embodiment Ru SA -Co2VP catalyst was used as the working electrode, graphite electrode as the counter electrode, and Ag / AgCl as the reference electrode, and alkaline electrocatalytic hydrogen evolution was carried out in a potassium hydroxide solution system with a concentration of 1 mol / L;
[0069] Activity test: Linear sweep voltammetry (LSV) curve test was performed in the voltage range of -0.8 to -1.7 V vs Ag / AgCl; SA -Co2VP electrocatalyst at -100mA / cm 2 The overpotential of hydrogen evolution at this current density is 69 mV.
[0070] Example 5: The ruthenium single atom catalyst of this example is a nanoneedle structure catalyst composed of a cobalt vanadium phosphorus nanoneedle carrier and an active component ruthenium single atom loaded on the vanadium phosphorus nanoneedle carrier, wherein the substrate of the cobalt vanadium phosphorus nanoneedle carrier is nickel foam; the chemical formula of the cobalt vanadium phosphorus nanoneedle carrier is CoxVP, where x=1;
[0071] A method for preparing a ruthenium single-atom catalyst, the specific steps are as follows:
[0072] (1) Dissolving Co(NO3)2·6H2O, VCl3, urea and ammonium fluoride in deionized water to obtain a mixed solution; the molar concentration of cobalt salt in the mixed solution is 0.01 mol / L, the molar concentration of vanadium salt is 0.01 mol / L, the molar concentration of urea is 0.25 mol / L, and the molar concentration of ammonium fluoride is 0.15 mol / L;
[0073] (2) A nickel foam substrate (NF) with a size of 2 cm × 3 cm was ultrasonically cleaned with ethanol and deionized water in turn, ultrasonically activated in dilute hydrochloric acid with a concentration of 0.15 mol / L for 25 min, and then ultrasonically cleaned with deionized water to obtain an activated nickel foam substrate (NF). The activated nickel foam substrate (NF) was then immersed in the mixed solution and reacted at a temperature of 120°C under closed conditions for 12 h to grow cobalt-vanadium nanoneedles on the surface of the activated nickel foam substrate (NF). The substrate was cooled to room temperature, and then cleaned with deionized water and anhydrous ethanol in turn, and vacuum dried to obtain cobalt-vanadium nanoneedles / nickel foam substrate Co1V-LDH.
[0074] (3) Cobalt-vanadium nanoneedles / nickel foam substrate Co1V-LDH was placed in a RuCl3 solution with a concentration of 4.8 mmol / L and subjected to surface chemical reaction at 25°C for 6 h. The excess RuCl3 solution was then removed by washing with deionized water and anhydrous ethanol, and vacuum dried to obtain cobalt-vanadium nanoneedles / nickel foam substrate Ru loaded with single ruthenium atoms. SA -Co1V-LDH;
[0075] (4) Sodium hypophosphite and cobalt vanadium nanoneedles / nickel foam substrate loaded with ruthenium single atoms were prepared. SA -Co1V-LDH was placed at both ends of the ceramic boat, and then the ceramic boat was placed in a tube furnace to evacuate the air, and then high-purity helium (gas flow rate 180sccm) was introduced, and the temperature was uniformly increased to 400°C at a heating rate of 5.5°C / min, and calcined at 400°C for 80min, and then cooled to room temperature to obtain a ruthenium single atom catalyst Ru SA -Co1VP; according to the gas flow direction of high-purity argon, the sodium hypophosphite is located upstream of the cobalt vanadium nanoneedle / nickel foam substrate loaded with ruthenium single atoms;
[0076] In this embodiment Ru SA -Co1VP catalyst was used as the working electrode, graphite electrode as the counter electrode, and Ag / AgCl as the reference electrode, and alkaline electrocatalytic hydrogen evolution was carried out in a potassium hydroxide solution system with a concentration of 1 mol / L;
[0077] Activity test: Linear sweep voltammetry (LSV) curve test was performed in the voltage range of -0.8 to -1.7 V vs Ag / AgCl; SA -Co1VP electrocatalyst at -100mA / cm 2 The overpotential of hydrogen evolution at this current density is 80 mV.
[0078] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A ruthenium single atom catalyst, characterized in that: The invention discloses a nano-needle structure catalyst composed of a cobalt-vanadium-phosphorus nano-needle carrier and a single atom of ruthenium, an active component, loaded on the vanadium-phosphorus nano-needle carrier. The substrate of the cobalt-vanadium-phosphorus nano-needle carrier is nickel foam.
2. The ruthenium single atom catalyst according to claim 1, characterized in that: The chemical formula of the cobalt vanadium phosphorus nanoneedle is Co x VP, where 1≤x≤5.
3. The method for preparing the ruthenium single atom catalyst according to claim 1 or 2, characterized in that: The specific steps are as follows: (1) dissolving cobalt salt, vanadium salt, urea and ammonium fluoride in deionized water to obtain a mixed solution; (2) immersing the nickel foam substrate in the mixed solution, reacting for 6 to 24 hours at a temperature of 90 to 160° C. under a closed condition, so that cobalt vanadium nanoneedles grow on the surface of the nickel foam substrate to obtain cobalt vanadium nanoneedles / nickel foam substrate; (3) placing the cobalt-vanadium nanoneedle / nickel foam substrate in a ruthenium salt solution for surface chemical reaction to obtain a cobalt-vanadium nanoneedle / nickel foam substrate loaded with ruthenium single atoms; (4) placing sodium hypophosphite and the cobalt vanadium nanoneedle / nickel foam substrate loaded with ruthenium single atoms in a tubular furnace, introducing a protective gas, and calcining to obtain a ruthenium single atom catalyst Ru SA -CoVP.
4. The method for preparing the ruthenium single atom catalyst according to claim 3, characterized in that: The cobalt salt in step (1) is one or more of cobalt nitrate, cobalt sulfate, and cobalt chloride, the vanadium salt is one or more of vanadyl sulfate, vanadium chloride, and ammonium metavanadate, and the molar ratio of the cobalt salt to the vanadium salt is (1-5):
1.
5. The method for preparing the ruthenium single atom catalyst according to claim 4, characterized in that: The molar ratio of urea to ammonium fluoride in step (1) is 1:(1-3).
6. The method for preparing the ruthenium single atom catalyst according to claim 5, characterized in that: In the mixed solution of step (1), the molar concentration of the cobalt salt is 0.001-0.1 mol / L, the molar concentration of the vanadium salt is 0.001-0.1 mol / L, the molar concentration of the urea is 0.1-1 mol / L, and the molar concentration of the ammonium fluoride is 0.1-1 mol / L.
7. The method for preparing the ruthenium single atom catalyst according to claim 3, characterized in that: The concentration of the ruthenium salt solution in step (3) is 1 to 10 mmol / L, the ruthenium salt is one or more of ruthenium sulfate, ruthenium chloride, and potassium ruthenate, the temperature of the surface chemical reaction is 25 to 35° C., and the time is 6 to 8 hours.
8. The method for preparing the ruthenium single atom catalyst according to claim 3, characterized in that: According to the gas flow direction of the protective gas, the sodium hypophosphite in step (4) is located upstream of the cobalt vanadium nanoneedle / nickel foam substrate loaded with ruthenium single atoms.
9. The method for preparing the ruthenium single atom catalyst according to claim 3, characterized in that: In step (4), the protective gas flow rate is 10 to 200 sccm, the calcination temperature is 300 to 400° C., and the calcination time is 60 to 180 min.
10. Use of the ruthenium single atom catalyst according to any one of claims 1 to 2 in catalyzing hydrogen evolution reaction in alkaline water electrolysis.
Citation Information
Cited By
HER electrocatalyst with porous heterostructure and preparation method thereof
CN119530872A