Alkaline electrolyzed water hydrogen production diaphragm, electrode module and electrolysis device

By reinforcing the filling or laminating of the edge area of ​​the alkaline electrolytic water hydrogen production separator, and using materials such as silicone rubber, the problem of rupture caused by shear force at the edge of the separator is solved and safety is improved.

CN118854366APending Publication Date: 2024-10-29CARBON HARMONY TECH (SHANGHAI) CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411072554.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The surface inorganic-organic coating of the alkaline electrolysis water hydrogen production separator is prone to cracking when the edge is subjected to shear force, leading to serious safety issues.

Method used

The edge area of ​​the separator is filled or bonded with a reinforced structure, including reinforced filling structure, reinforced layer structure and reinforced bonding structure. Materials such as silicone rubber and epoxy resin are used for edge strengthening to reduce porosity and improve edge strength.

Benefits of technology

It effectively reduces the probability of coating rupture, inhibits gas leakage, and improves the safety of using alkaline electrolyzed water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854366A_ABST
    Figure CN118854366A_ABST
Patent Text Reader

Abstract

The invention discloses an alkaline electrolytic water hydrogen production diaphragm, an electrode module and an electrolysis device.The diaphragm comprises a supporting layer and hydrophilic porous coatings formed on the two sides of the supporting layer, and a reinforcing structure is further formed in at least partial area of the edge of the diaphragm; the reinforcing structure is at least any one of the following structures: a reinforcing filling structure: filling the edge of the diaphragm with a reinforcing filling material so as to reduce the porosity of the hydrophilic porous coating; a strengthening layer structure: forming a layer shape at the edge of the diaphragm by using curing resin, and then curing; and strengthening the attaching structure: attaching a strengthening piece formed by a strengthening raw material to the edge of the diaphragm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrolytic hydrogen production, and in particular relates to an alkaline water electrolysis hydrogen production diaphragm, an electrode module and an electrolysis device. Background Art

[0002] In the production of hydrogen by alkaline water electrolysis, the diaphragm, as a core component, plays an important role in ion conduction and isolating the hydrogen and oxygen produced by the cathode and anode respectively. This type of alkaline water electrolysis hydrogen production diaphragm is usually composed of a middle support layer and an inorganic-organic slurry coating on both sides. After being installed in the alkaline electrolyzer, the edge of the diaphragm usually needs to be pressed tightly due to the need for edge sealing. Therefore, the edge of the diaphragm is often subjected to a high shear force, causing the inorganic-organic coating on the surface to rupture, further causing serious safety issues such as cross-talk.

[0003] Therefore, in order to solve the above technical problems, it is necessary to provide an alkaline water electrolysis hydrogen production diaphragm, an electrode module and an electrolysis device.

[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0005] The object of the present invention is to provide a diaphragm, an electrode module and an electrolysis device for producing hydrogen by alkaline water electrolysis.

[0006] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:

[0007] The alkaline water electrolysis hydrogen production diaphragm comprises a support layer and a hydrophilic porous coating formed on both sides of the support layer, and at least a part of the edge of the diaphragm is also formed with a reinforcement structure, and the reinforcement structure is at least any one of the following: a reinforcement filling structure: the edge of the diaphragm is filled with a reinforcement filling material to reduce the porosity of the hydrophilic porous coating;

[0008] Strengthening layer structure: the cured resin forms a layer at the edge of the diaphragm, and then solidifies (the solidification here may include the solidification of the monomer of the body structure under the solidification conditions, or the solution of the chain resin forms a solid after drying, or the molten resin forms a solid after cooling);

[0009] Reinforced bonding structure: The reinforcement formed by the reinforcing raw material is bonded to the edge of the diaphragm. The reinforcement layer structure can also be used in conjunction with the reinforced bonding structure, that is, the cured resin forms a layered cured structure at the edge of the diaphragm, and the reinforcement can be bonded to the outside; of course, the reinforced filling structure can also be used in combination with the reinforced bonding structure.

[0010] In one or more embodiments of the present invention, the curing resin is selected from one or more of the following: silicone rubber, epoxy resin, fluororubber, phenolic curing resin, urea-formaldehyde resin, furan resin glue, polysulfide rubber, chloroprene rubber, ultraviolet curing UV glue, polylactic acid, ethylene / vinyl acetate copolymer EVA.

[0011] In one or more embodiments of the present invention, the strengthening material is selected from one or more of the following: polyethersulfone, polyphenylenesulfone, polysulfone, polyetheretherketone, polypropylene, polytetrafluoroethylene, polytetrafluorovinylidene, polyperfluoroethylenepropylene, ethylene-tetrafluoroethylene copolymer, polyethylene terephthalate, polyethylene naphthalate, polyimide, polyetherimide, polyurethane, polyurethane polyphenylene ether, polyethylene, polyvinyl chloride, polycarbonate, nylon, ABS plastic, metal sheet material. The metal sheet material can be selected from stainless steel sheet, copper sheet, etc.

[0012] In one or more embodiments of the present invention, the reinforcing filling material is selected from one or more of the following: polyethersulfone, polyphenylene sulfone, polysulfone, polyetheretherketone, polypropylene, polytetrafluoroethylene, polytetrafluorovinylidene, polyperfluoroethylene propylene, ethylene-tetrafluoroethylene copolymer, polyethylene terephthalate, polyethylene naphthalate, polyimide, polyetherimide, polyurethane, polyurethane polyphenylene ether, polyethylene, polyvinyl chloride, polycarbonate, nylon, ABS plastic, silicone rubber, epoxy resin, fluororubber, phenolic curing resin, urea-formaldehyde resin, furan resin glue, polysulfide rubber, chloroprene rubber, and ultraviolet curing UV glue.

[0013] In one or more embodiments of the present invention, the porosity of the edge of the diaphragm filled with the reinforcing filling material after filling is reduced by 5% or more compared to the original porosity.

[0014] In one or more embodiments of the present invention, the reinforcing filling material is filled by: immersing the edge of the membrane to be reinforced in a solution containing the reinforcing filling material, and then curing it.

[0015] In one or more embodiments of the present invention, the concentration of the reinforcing filler material in the solution is 5-100 wt %.

[0016] In one or more embodiments of the present invention, the solvent in the solution is selected from: water, ethanol, methanol, isopropanol, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetonitrile, pyridine, phenol, ester solvents, carboxylic acid solvents, ether solvents, aliphatic hydrocarbon solvents, aromatic hydrocarbon solvents, halogenated hydrocarbon solvents. The preferred solvent is dimethyl sulfoxide.

[0017] In one or more embodiments of the invention, the difference between the thickness of the reinforcement structure and the thickness at the center of the diaphragm is less than 5 mm.

[0018] In one or more embodiments of the present invention, the electrode module includes an anode electrode, a cathode electrode and at least one alkaline water electrolysis hydrogen production membrane formed therebetween. When the alkaline water electrolysis hydrogen production membrane is multi-layered, it is in a stacked state.

[0019] In one or more embodiments of the present invention, the electrolysis device at least includes an electrolysis tank having an electrolysis chamber, and an electrode module disposed in the electrolysis chamber.

[0020] Compared with the prior art, the alkaline water electrolysis hydrogen production diaphragm, electrode module and electrolysis device of the present invention, through the edge strengthening method, covers the outer surface of the edge area prone to problems with another layer of material, or strengthens the edge part, thereby improving the safety of the alkaline water electrolysis process. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 A schematic diagram of a product structure of an embodiment of the present invention;

[0023] Figure 2 The electrochemical performance and hydrogen in oxygen performance diagram of a product according to an embodiment of the present invention;

[0024] Figure 3 A schematic structural diagram of a reinforcement structure of a product according to an embodiment of the present invention;

[0025] Figure 4 A schematic structural diagram of a reinforcement structure of a product according to an embodiment of the present invention; DETAILED DESCRIPTION

[0026] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0027] In the alkaline water electrolysis hydrogen production diaphragm, electrode module and electrolysis device in one embodiment of the present invention, the main diaphragm is composed of a support layer and a hydrophilic porous coating on both sides. The support layer can be polyphenylene sulfide, nylon, polyethylene terephthalate, polypropylene, polyphenyl sulfone, polyether sulfone, polyether ether ketone, etc., preferably polyphenylene sulfide and nylon, etc. The raw materials of the porous coating can include inorganic hydrophilic particles, polymer resins and other additives, wherein the inorganic hydrophilic particles are selected from one or more of zirconium oxide, barium sulfate, hydrotalcite, titanium dioxide, and magnesium hydroxide. Various additives may include conventional additives such as tougheners, plasticizers, and antioxidants, which are not limited here. The mass ratio of polymer resins (such as polysulfone (PSU), polyether sulfone (PES), polyphenyl sulfone (PPS), polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyethylene oxide (PEO), polymethyl methacrylate (PMMA), etc.) and inorganic hydrophilic particles in the porous coating is in the range of 1:5-1:1.

[0028] In the implementation of the scheme of the present invention, since alkaline water electrolysis is usually used under high-concentration alkaline conditions and reaction conditions below 120 degrees, there are certain requirements for the reinforcement material of the edge area. It is required that the reinforcement area should not have significant size shrinkage and decomposition under high-temperature strong alkali immersion. And it is significantly different from the packaging of proton exchange membrane water electrolysis hydrogen production.

[0029] In the scheme of the present invention, strengthening the edge area through the reinforced structure can: 1. reduce the probability of coating rupture after being subjected to shear force by improving the strength of the edge area; 2. through the wrapping of the edge strengthening layer, even in the case of coating rupture, it can still suppress the phenomenon of gas and liquid cross-talk, thereby improving safety.

[0030] like Figure 1 As shown, the diaphragm 1 of the present invention may include a support layer 1-2 and a hydrophilic porous coating 1-1 formed on both sides of the support layer. A reinforcing structure 2 is also formed on the edge of the diaphragm 1. Since the support layer 1-2 is a porous support layer, its pores are often relatively large, and its main part is also covered by a porous hydrophilic layer. Figure 1 The middle dividing line may be schematic, and does not necessarily mean that there is a significant result dividing line. Further, the thickness of the reinforcing structure 2 is not more than 1000 μm, preferably not more than 500 μm. Too high thickness of the edge reinforcement area will make it relatively difficult to match with the alkaline electrolytic cell. This reinforcement height range is consistent with the difference in compression between the edge side and the center part in the tank.

[0031] The implementation of this structure can be achieved through the following scheme:

[0032] The edge area strengthening method in method 1 can be divided into two types: method a1 can form a strengthening layer by curing the resin rubber; method a2 can further use rubber glue to stick the strengthening bonding layer on the edge. Figure 3 The strengthening layer or strengthening bonding layer 2-1 to 2-4 shown is formed on the edge area of ​​the diaphragm 1. In method a1, the resin rubber is selected from: silicone rubber, epoxy resin, fluororubber, phenolic curing resin, urea-formaldehyde resin, furan resin glue, polysulfide rubber, chloroprene rubber, ultraviolet curing UV glue, preferably polysulfide rubber, chloroprene rubber, fluororubber, EPDM rubber. The rubber curing temperature can be selected from room temperature to 200 degrees. Specifically, the resin can be scraped onto the edge area of ​​the composite diaphragm with a scraper or a Meyer rod, or sprayed onto the edge area of ​​the composite diaphragm with a dilute solution, and then cured by heating in an oven, or by infrared lamp baking or ultraviolet lamp curing to obtain a strengthening layer.

[0033] In method a2, the material of the reinforcing bonding layer is selected from: polyethersulfone, polyphenylene sulfone, polysulfone, polyetheretherketone, polypropylene, polytetrafluoroethylene, polytetrafluorovinylidene fluorocarbon, polyperfluoroethylene propylene, ethylene-tetrafluoroethylene copolymer, polyethylene terephthalate, polyethylene naphthalate, polyimide, polyetherimide, polyurethane, polyurethane polyphenylene ether, polyethylene, polyvinyl chloride, polycarbonate, nylon, ABS plastic, stainless steel metal sheet, preferably polyethersulfone, polyphenylene sulfone, polysulfone, polyetheretherketone, polypropylene, polytetrafluoroethylene, polyperfluoroethylene propylene, polytetrafluorovinylidene fluorocarbon, metal sheet, etc.

[0034] Of course, the strengthening laminating layer in method a2 can also be glued to the outside of the strengthening layer obtained in method a1; under suitable conditions, the stainless steel sheet of the strengthening laminating layer can be laminated together with the vulcanized rubber of method a1 during vulcanization molding. Of course, the stainless steel sheet here can also be replaced by a nylon film, nylon sheet, aluminum sheet, copper sheet, polytetrafluoroethylene sheet, polypropylene sheet, etc., or a combination of one or more.

[0035] Method 2

[0036] like Figure 4 The reinforced filling material shown fills the edge area of ​​the diaphragm 1 by infiltration or the like to form reinforced filling structures 3-1, 3-2, thereby enhancing the pressure resistance of the edge coating itself, and the edge changes from the original high-porosity porous state to a lower-porosity state, thereby reducing the compressibility of the edge area and making it less likely to cause the coating to rupture.

[0037] The reinforcing filling material is selected from polymer resins including polyethersulfone, polyphenylene sulfone, polysulfone, polyetheretherketone, polypropylene, polytetrafluoroethylene, polytetrafluorovinylidene, polyperfluoroethylene propylene, ethylene-tetrafluoroethylene copolymer, polyethylene terephthalate, polyethylene naphthalate, polyimide, polyetherimide, polyurethane, polyurethane polyphenylene ether, polyethylene, polyvinyl chloride, polycarbonate, nylon, ABS plastic, epoxy resin, silicone rubber solution, phenolic curing resin, silicone rubber, epoxy resin, fluororubber, phenolic curing resin, urea-formaldehyde resin, furan resin glue, polysulfide rubber, chloroprene rubber, and ultraviolet curing UV glue.

[0038] The method comprises soaking at least one edge region of the membrane in a polymer resin solution, and then drying and curing to obtain a composite diaphragm with a reinforced edge region, wherein the resin solution concentration can be 5-100wt%. The solution temperature is 10-150°C, and the soaking time is not more than 10h. After the membrane edge is soaked in the solution, it is pulled out and the excess resin solution on the surface is removed and then dried and cured. The drying and curing conditions can be drying at 140-200 degrees for 4-12 hours, depending on the curing material.

[0039] Embodiment 1:

[0040] In this embodiment, a 500 μm thick liquid silicone rubber (DY 35-4088) coating was applied to the edge area of ​​the diaphragm by scraping, and then baked under an infrared lamp at 140 degrees for 30 minutes. Then, a 50 μm thick silicone rubber coating was applied to the edge area of ​​the other side, and then baked under an infrared lamp at 140 degrees for 30 minutes to cure. Then, the electrochemical properties and hydrogen in oxygen properties were tested. Figure 2 shown.

[0041] Example 2: The silicone rubber in Example 1 is replaced equally with liquid polysulfide rubber (JLY-115), and the coating thickness is 20 μm.

[0042] Example 3: A 80 μm thick Teflon tape is directly attached to the edge area of ​​a 500 μm thick diaphragm.

[0043] Example 4: A thin layer of 10 μm neoprene adhesive was applied to the edge area of ​​a 500 μm thick diaphragm, and then a 50 μm thick 316 stainless steel sheet was adhered thereto.

[0044] Example 5: The edge area of ​​the 500 μm thick diaphragm was immersed in a DMSO solution of 50 wt.% (the same below) PSF (BASF, E3010) for 5 hours, then taken out, heated to 140 degrees and dried for 4 hours to solidify. The initial porosity was 55%, and the porosity after filling was 10%.

[0045] Example 6: 50% of the PSF solution in Example 5 was replaced with an epoxy resin solution (16 g of bisphenol S epoxy resin (epoxy equivalent 200), 5 g of diaminodiphenylmethane curing agent, and 40 ml of NMP solvent). The initial porosity was 55%, and the porosity after filling was 5%.

[0046] Example 7

[0047] In this embodiment, the edge area of ​​the 500 μm thick diaphragm is coated with a coating of ultraviolet curing UV glue (Loctite AA3106 UV glue) with a thickness of about 30 μm, and then the press-fit test is performed after curing by ultraviolet light.

[0048] Example 8

[0049] In this embodiment, the 500 μm thick edge area of ​​the diaphragm is immersed in 107 liquid silicone rubber for 10 hours, taken out, and the excess liquid silicone on the surface is scraped off and then dried and solidified.

[0050] Example 9

[0051] The chloroprene rubber in Example 4 was replaced equally with EVA hot melt adhesive.

[0052] Example 10

[0053] The stainless steel sheet in Example 4 was replaced with a 50 μm polyethylene naphthalate film.

[0054] Embodiment 11

[0055] The 50% PSF solution in Example 5 was replaced by a 25% DMF solution of polyimide.

[0056] Example 12

[0057] On the basis of Example 10, a 50 μm stainless steel sheet was attached using a chloroprene rubber adhesive.

[0058] Example 13

[0059] In this embodiment, a 500 μm thick square diaphragm (taking the edges of different sides of the square diaphragm as an example of strengthening them separately) is coated with a 50 μm thick liquid silicone rubber (DY 35-4088) coating on one edge area by scraping, and then baked at 140 degrees for 30 minutes by infrared lamp. Then, a 50 μm thick silicone rubber coating is also coated on the edge area of ​​the other side of the same side, and then cured by infrared lamp baking at 140 degrees for 30 minutes. The side is protected by masking tape, and after the excess tape is cut off, 80 μm thick Teflon tape is bonded to both sides of the next edge area. The side is protected by masking tape, and after the excess tape is cut off, the next edge area is immersed in a 50wt. (same below)% PSF (BASF, E3010) DMSO solution for 5 hours, then taken out, heated to 140 degrees, dried for 4 hours, and cured. The initial porosity is 55%, and the porosity after filling is 10%. This side was protected with masking tape, and after the excess tape was cut off, a thin layer of 10 μm neoprene adhesive was applied to the surface of the next edge area, and then a 50 μm thick 316 stainless steel sheet was adhered.

[0060] Comparative Example 1: The 500 μm thick separator does not require any treatment.

[0061] Press-fit test method: Install the composite diaphragm into a 2*2 alkaline water electrolysis test tank, press-fit with a pressure of 0.5 tons, and observe the deformation of the edge area and the center area, as well as whether there is obvious coating rupture. Both sides are Raney nickel electrodes, and the electrochemical performance test is carried out at a flow rate of 20ml / min. The tank pressure data is obtained on the electrochemical workstation, and the hydrogen in oxygen data is obtained by gas chromatography. The test results are shown in the following table.

[0062]

[0063]

[0064] It should be noted that the electrolytic performance mainly depends on the ion conduction of the membrane and the diaphragm, and the edge enhancement part improved by the technical solution of the invention is also shielded and ineffective under the prior art, so it does not affect the ion conduction of the main part of the diaphragm, and therefore the electrolytic performance will not be affected.

[0065] In the solutions of the present invention including but not limited to the above-mentioned embodiments, different edge positions of the same diaphragm can be strengthened by using the same reinforcement structure. Of course, different edge positions of the same diaphragm can also be strengthened by using different reinforcement structures.

[0066] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

[0067] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. An alkaline water electrolysis hydrogen production membrane, comprising a support layer and a hydrophilic porous coating formed on both sides of the support layer, characterized in that: At least a portion of the edge of the diaphragm is also formed with a reinforcement structure, and the reinforcement structure is at least any one of the following: Reinforced filling structure: using a reinforced filling material to fill the edge of the diaphragm to reduce the porosity of the hydrophilic porous coating; Strengthening layer structure: forming a layer at the edge of the diaphragm with a curing resin and then curing; Reinforced bonding structure: A reinforcement member formed of a reinforcing raw material is bonded to the edge of the diaphragm.

2. The alkaline water electrolysis hydrogen production diaphragm according to claim 1, characterized in that: The curing resin is selected from one or more of the following: silicone rubber, epoxy resin, fluororubber, phenolic curing resin, urea-formaldehyde resin, furan resin glue, polysulfide rubber, chloroprene rubber, ultraviolet curing UV glue, polylactic acid, ethylene / vinyl acetate copolymer EVA.

3. The alkaline water electrolysis hydrogen production diaphragm according to claim 1, characterized in that: The reinforcing raw material is selected from one or more of the following: polyethersulfone, polyphenylenesulfone, polysulfone, polyetheretherketone, polypropylene, polytetrafluoroethylene, polytetrafluorovinylidene, polyperfluoroethylenepropylene, ethylene-tetrafluoroethylene copolymer, polyethylene terephthalate, polyethylene naphthalate, polyimide, polyetherimide, polyurethane, polyurethane polyphenylene ether, polyethylene, polyvinyl chloride, polycarbonate, nylon, ABS plastic, and metal sheet material.

4. The alkaline water electrolysis hydrogen production diaphragm according to claim 1, characterized in that: The reinforcing filling material is selected from one or more of the following: polyethersulfone, polyphenylenesulfone, polysulfone, polyetheretherketone, polypropylene, polytetrafluoroethylene, polytetrafluorovinylidene, polyperfluoroethylene propylene, ethylene-tetrafluoroethylene copolymer, polyethylene terephthalate, polyethylene naphthalate, polyimide, polyetherimide, polyurethane, polyurethane polyphenylene ether, polyethylene, polyvinyl chloride, polycarbonate, nylon, ABS plastic, silicone rubber, epoxy resin, fluororubber, phenolic curing resin, urea-formaldehyde resin, furan resin glue, polysulfide rubber, chloroprene rubber, and ultraviolet curing UV glue.

5. The alkaline water electrolysis hydrogen production diaphragm according to claim 4, characterized in that: The porosity of the edge of the diaphragm filled with the reinforcing filling material after filling is reduced by 5% or more compared with the original porosity.

6. The alkaline water electrolysis hydrogen production diaphragm according to claim 5, characterized in that: The reinforcing filling material is filled by immersing the edge of the diaphragm to be reinforced in a solution containing the reinforcing filling material and then curing it.

7. The alkaline water electrolysis hydrogen production diaphragm according to claim 6, characterized in that: The concentration of the reinforcing filler material in the solution is 5-100 wt %.

8. The alkaline water electrolysis hydrogen production diaphragm according to claim 1, characterized in that: The difference between the thickness of the reinforcement structure and the thickness at the center of the diaphragm is less than 5 mm.

9. An electrode module, comprising an anode electrode, a cathode electrode and at least one layer of an alkaline water electrolysis hydrogen production membrane according to any one of claims 1 to 8 formed therebetween, wherein the alkaline water electrolysis hydrogen production membrane is in a stacked state when it is multi-layered.

10. An electrolysis device comprising at least an electrolysis tank having an electrolysis chamber, and the electrode module according to claim 9 arranged in the electrolysis chamber.

Citation Information

Cited By

  • PET (Polyethylene Terephthalate) coating film for lithium battery diaphragm and preparation method of PET coating film

    CN121108851A

  • Integrated membrane electrode assembly and preparation method therefor, and alkaline electrolyzer

    WO2026222856A1