Preparation method of N-type silicon single crystal rod with high resistance uniformity

By using antimony and red phosphorus dopants and pre-treatment seed crystal cleaning technology in the Czochralski production of single crystal silicon rods, the problem of uneven resistivity of single crystal silicon rods is solved and the resistivity is stabilized. The stability and uniformity are improved, the production cost and oxygen content are reduced, and the quality and service life of single crystal silicon rods are improved.

CN118854433AInactive Publication Date: 2024-10-29INNER MONGOLIA CHANGRUI SEMICON MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411358339.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing technology, the resistivity inhomogeneity of single crystal silicon rods leads to low availability and high cost. Especially in the production of N-type single crystal silicon rods, the segregation coefficient of phosphorus as a dopant is low, making it difficult to control the doping. The impurity concentration causes the resistivity distribution range to be too large, insufficient to meet the qualified part, and affects the quality and service life.

Method used

N-type single crystal silicon rods are prepared using the Czochralski method. By adding antimony and red phosphorus dopants into the polycrystalline silicon material, according to the mass ratio of 8:1, the melting temperature and argon gas pressure are controlled to perform necking, shoulder releasing and The equal-diameter growth process, combined with the pre-treatment seed crystal cleaning method, improves the uniformity and stability of the resistivity.

Benefits of technology

It has improved the stability and uniformity of the resistivity of single crystal silicon rods, extended its service life, reduced production costs, improved quality and utilization, significantly improved the resistivity distribution of the crystal rods, and reduced argon gas costs and oxygen content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854433A_ABST
    Figure CN118854433A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of silicon single crystal rod manufacturing, in particular to a preparation method of an N-type silicon single crystal rod with high resistance uniformity. The preparation method is a czochralski method, a used doping agent is composed of antimony and red phosphorus according to the mass ratio of 8: 1, used seed crystals are pretreated through modified sorbitan laurate and microcapsule-EDTA, and the N-row single crystal silicon rod prepared through the method is good in resistance uniformity and long in minority carrier lifetime.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of single crystal silicon rod manufacturing, and in particular to a method for preparing an N-type single crystal silicon rod with high resistance uniformity. Background Art

[0002] As a semiconductor material, single crystal silicon is mainly used in the fields of photovoltaics and semiconductors. There are currently two technologies used in the actual production of single crystal silicon: the Czochralski method and the zone melting method. In the production of single crystal silicon, a certain amount of dopants are often added to meet the requirements for its electrical properties. Common dopants are: boron, phosphorus, arsenic and antimony. Due to the phenomenon of impurity segregation during crystal solidification, the later the crystal rod is, the higher the dopant concentration is, and the lower the resistivity is, resulting in the non-uniformity of the axial resistivity of the single crystal, especially for dopants with small segregation coefficients (such as phosphorus and arsenic). The axial resistivity uniformity of the single crystal is worse. Single crystal silicon with dopants has the advantages of high conversion efficiency, long service life and good resistance to harsh environments, which has attracted widespread attention. However, due to the low segregation coefficient of some dopants in silicon, it is difficult to control the doping concentration during doping, resulting in the resistivity distribution of the obtained single crystal silicon rods between 0.1-5Ω·cm, and the distribution range is too large. The qualified part that meets the resistivity between 0.8-3Ω·cm is usually less than 50%, resulting in low availability of single crystal silicon rods and high cost. Single crystal silicon rods can be divided into P-type single crystal silicon rods and N-type single crystal silicon rods according to the different dopants. At present, most of the dopants used in the production of N-type solar single crystal silicon rods are N-type phosphorus master alloys. The segregation coefficient of phosphorus in silicon crystals and silicon melts is 0.35. Affected by the segregation coefficient, the resistivity of the single crystal is short in the length of the pull-up process of the solar silicon rod, and with the increase in the number of pulled rods, the impurity concentration in the solution gradually increases, resulting in a rapid decay of the minority carrier lifetime, thereby affecting the quality of the crystal rod, reducing the use efficiency, and further increasing the production cost. Summary of the invention

[0003] In view of the deficiencies in the prior art, the present invention provides a method for preparing an N-type single crystal silicon rod with high resistance uniformity.

[0004] The present invention is achieved through the following technical solutions: A method for preparing an N-type single crystal silicon rod with high resistance uniformity, the preparation method is a Czochralski method, comprising the following steps: (1) placing polysilicon material and dopants in a quartz crucible and heating and melting them into stable molten silicon in a 20 torr argon atmosphere; (2) Introducing seed crystals into stable molten silicon, followed by necking and shoulder release before entering the isodiameter growth stage; (3) During the entire stage of equal-diameter growth, the crystal pulling rate is maintained constant. At the beginning of equal-diameter growth, the argon pressure in the single crystal furnace is reduced to 0.5-0.8 torr and maintained until the growth of the CZ-pulled single crystal silicon rod is completed. The rod is cooled to obtain an N-type single crystal silicon rod.

[0005] Furthermore, the melting temperature in step (1) is 1420-1450°C.

[0006] Furthermore, the argon gas flow rate in step (1) is 70 slpm.

[0007] Furthermore, the dopant in step (1) is composed of antimony and red phosphorus in a mass ratio of 8:1.

[0008] Furthermore, the dopant in step (1) has a phosphorus concentration of 3.5×10 18 Atom / cm 3 Dopants are added to the polysilicon material.

[0009] Furthermore, the crucible temperature during the necking in step (2) is 1420-1500°C.

[0010] Furthermore, in step (2), the crucible temperature during shouldering is 1000-1100° C., the crucible rotation speed is 9-10 rpm, and the crystal rotation speed is 10-11 rpm.

[0011] Furthermore, in step (3), the crucible temperature for the equal-diameter growth is 1300-1400° C., the crucible rotation speed is 9 rpm, and the crystal rotation speed is 11 rpm.

[0012] Furthermore, the diameter of the equal-diameter region of the CZS silicon rod is 200-205 mm, and the equal-diameter length is 1300-1400 mm.

[0013] Furthermore, the entire stage of the equal-diameter growth in step (3) refers to the entire process from the beginning of equal-diameter growth of the crystal rod after the shoulder is released to the end of crystal growth.

[0014] Furthermore, the crystal pulling rate in step (3) is in the range of 1.2-2 mm / min.

[0015] Furthermore, the seed crystal in step (2) is a pretreated seed crystal, and the pretreatment method comprises the following steps: (a) Sorbitol anhydride dodecanoate and 1-amino-1-deoxy-D-galactopyranose are mixed, and a mixed catalyst of dodecylbenzenesulfonic acid and p-toluenesulfonic acid is added under stirring at 180 rpm, reacted at 30-40 mmHg and 120°C for 5-6 h, allowed to stand at 4°C for 3-4 h, filtered, and the residue is washed with anhydrous ethanol and deionized water, and vacuum dried at 50°C for 12-14 h to obtain modified sorbitol anhydride dodecanoate; (b) Dissolving hydrofluoric acid, acetic acid and citric acid in deionized water, stirring at 400-500 r / min for 10 min to obtain a mixed acid solution, slowly adding the mixed acid solution to a 3 wt % chitosan acetic acid solution, adding 2-aminoethyl stearate to a concentration of 1 wt %, stirring at 500-600 r / min for 2 h, centrifuging at 10000 rpm for 30 min, precipitating and freeze-drying at -20°C for 12 h to obtain acid sustained-release microcapsules; (c) placing the acid sustained-release microcapsules obtained in step (b) into a mixture of ethanol and acetic acid, ultrasonicating at 200W for 30 min, adding ethylenediaminetetraacetic dianhydride (EDTAD), reacting at 60-80°C for 8-10 h, washing with deionized water to pH 7.2-7.4, and drying at 60°C to obtain microcapsules-EDTA; (d) The modified sorbitan dodecanoate obtained in step (a) is mixed with deionized water, and seed crystals are placed in the mixture (the liquid is sufficient to cover the seed crystals), and the mixture is ultrasonicated at 300 W for 20 min. After the mixture is taken out, the mixture is added into microcapsule-EDTA solution (the liquid is sufficient to cover the seed crystals), and the mixture is ultrasonicated at 60° C. and 200 W for 15 min. The seed crystals are taken out and rinsed in ultrapure water for 6-8 times, each time for 30 s, and then dried with nitrogen to obtain pretreated seed crystals.

[0016] Furthermore, in step (a), the mass ratio of sorbitan dodecanoate to 1-amino-1-deoxy-D-galactopyranose is 16:9.

[0017] Furthermore, the mass ratio of dodecylbenzenesulfonic acid to p-toluenesulfonic acid in step (a) is 2-3:1.

[0018] Furthermore, the mass ratio of the mixed catalyst to sorbitan dodecanoate in step (a) is 1:100.

[0019] Furthermore, in step (b), the mass ratio of hydrofluoric acid, acetic acid and citric acid is 1:5:3.

[0020] Furthermore, in the mixed acid solution of step (b), the ratio of acetic acid to deionized water is 1-1.5 g:8 mL.

[0021] Furthermore, in step (b), the volume ratio of the mixed acid solution to the chitosan acetic acid solution is 1:3.

[0022] Furthermore, in step (c), the ratio of the acid sustained-release microcapsules to the mixed solution of ethanol and acetic acid is 1 g:10 mL.

[0023] Furthermore, in the mixed solution of ethanol and acetic acid in step (c), the volume ratio of ethanol to acetic acid is 1:1.

[0024] Furthermore, in step (c), the mass ratio of the acid sustained-release microcapsules to EDTAD is 1:0.3-0.5.

[0025] Furthermore, in step (d), the mass ratio of the modified sorbitan dodecanoate to deionized water is 1:1.

[0026] Furthermore, in the microcapsule-EDTA solution of step (d), the mass ratio of microcapsule-EDTA to deionized water is 1:1.

[0027] Compared with the prior art, the present invention has the following beneficial effects: The method of the present invention is applicable to N-type single crystal silicon rods. In the process of drawing the N-type single crystal silicon rods, the resistivity of the head and tail of the single crystal silicon rods is controlled by adding dopants. By adding new dopants, the resistivity stability of the N-type single crystal silicon rods is better, the service life is longer, and the quality is better. The present invention uses a mixed doping method of phosphorus and antimony elements, and phosphorus and antimony are mixed into polysilicon materials in a ratio of 1:8 (weight ratio). The resistivity segregation of the N-type single crystal silicon rods prepared according to this ratio is slowed down, the resistivity uniformity is better, the resistivity stability is high, and it is convenient to control the resistivity more accurately; accompanied by the high-temperature volatilization of antimony in the single crystal preparation process, the resistivity segregation is slowed down, and the single crystal has a longer length in the gear; the phosphorus antimony dopant can volatilize the metal impurities in the form of antimony compounds through the internal absorption process of impurities during the volatilization process, further improving the life of the single crystal and making the single crystal quality better. Conventional N-type single crystal silicon rods are usually forced to stop the furnace when they are pulled to 7-8 rods due to the reduction of minority carrier lifetime. After using mixed alloys, the minority carrier lifetime can be further improved, and the number of rods pulled can be increased, thereby further reducing production costs. The present invention reduces the furnace pressure, significantly improves the resistivity uniformity of the crystal rod, improves the utilization rate of N-type direct-pulled single crystal silicon, and saves argon gas costs; the resistance uniformity of the single crystal silicon prepared by the method of the present invention is significantly improved, and the oxygen content is significantly reduced. The present invention prepares sorbitan dodecanoate, introduces aminogalactose groups, enhances the hydrophilicity of the hydrophilic end, improves surface activity, exhibits higher stability, and can effectively remove impurities on the surface of single crystal silicon seed crystals. The present invention combines acetic acid, citric acid and hydrofluoric acid to improve the cleaning effect of impurities contaminated by monocrystalline silicon seed crystals, reduce the amount of hydrofluoric acid used, and make the mixed acid into microcapsules, which can reduce acid residues, avoid excessive corrosion of the surface of monocrystalline silicon seed crystals, reduce surface roughness, improve the surface quality of seed crystals, and avoid excessive corrosion of seed crystals, thereby increasing the service life of seed crystals. In addition, EDTA is grafted on the surface of microcapsules to improve chelation and effectively remove metal impurities. The pretreatment method of the present invention can make the surface cleanliness of monocrystalline silicon seed crystals high, the content of metal impurities removed is high, the surface roughness of monocrystalline silicon seed crystals is reduced, the stability after cleaning is better, the average number of times that can be introduced is increased, and the service life of monocrystalline silicon seed crystals is extended; and while ensuring that the surface dirt, metal ions and oxide layers of monocrystalline silicon seed crystals are cleaned, the bearing capacity of seed crystals during crystal pulling is improved, and the lead break rate is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1is the resistivity change rate of the single crystal silicon rods obtained in Example 1 of the present invention and Comparative Examples 1-5; Figure 2 is the oxygen content of the single crystal silicon rods obtained in Example 2 of the present invention and Comparative Examples 1-5; Figure 3 The minority carrier lifetime of the single crystal silicon rods obtained in Example 3 of the present invention and Comparative Examples 1-5; Figure 4 It is the seeding wire breakage rate of Example 1 of the present invention and Comparative Examples 1-5. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments. It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention are purchased through commercial channels.

[0031] Embodiment 1: This embodiment provides a method for preparing an N-type single crystal silicon rod with high resistance uniformity, the preparation method is a Czochralski method, comprising the following steps: (1) Polycrystalline silicon material and dopant are placed in a quartz crucible. The dopant is composed of antimony and red phosphorus in a mass ratio of 8:1. The dopant has a phosphorus concentration of 3.5×10 18 Atom / cm 3 Adding dopants to polysilicon material, heating and melting at 1450° C. in an argon atmosphere of 70 slpm and 20 torr to a stable molten silicon; (2) Introducing a seed crystal into the stable molten silicon, followed by necking and shouldering, and then entering the equal diameter growth stage. The crucible temperature during necking is 1500°C, the crucible temperature during shouldering is 1100°C, the crucible speed is 10 rpm, and the crystal speed is 11 rpm; (3) During the whole stage of equal-diameter growth (the whole process from the beginning of equal-diameter growth after the shoulder release to the end of crystal growth), the crystal pulling rate was kept constant at 2 mm / min, the crucible temperature of equal-diameter growth was 1400°C, the crucible speed was 9 rpm, the crystal speed was 11 rpm, and the argon pressure in the single crystal furnace was reduced to 0.8 torr at the beginning of equal-diameter growth and maintained until the growth of the CZ-pulled single crystal silicon rod was completed. The diameter of the equal-diameter region of the CZ-pulled single crystal silicon rod was 205 mm, and the equal-diameter length was 1400 mm. After cooling, an N-type single crystal silicon rod was obtained.

[0032] The seed crystal is a pre-treated seed crystal, and the pre-treatment method comprises the following steps: (a) 16 g of sorbitan dodecanoate and 9 g of 1-amino-1-deoxy-D-galactopyranose were mixed, and a mixed catalyst of 0.12 g of dodecylbenzenesulfonic acid and 0.04 g of p-toluenesulfonic acid was added under stirring at 180 rpm, and the mixture was reacted at 40 mmHg and 120°C for 6 h, and allowed to stand at 4°C for 4 h, filtered, and the residue was washed with anhydrous ethanol and deionized water, and dried under vacuum at 50°C for 14 h to obtain modified sorbitan dodecanoate; (b) 3 g of hydrofluoric acid, 15 g of acetic acid, and 9 g of citric acid were dissolved in 80 mL of deionized water, and stirred at 500 r / min for 10 min to obtain a mixed acid solution. 100 mL of the mixed acid solution was slowly added to 300 mL of 3 wt% chitosan acetic acid solution, and 2-aminoethyl stearate was added to a concentration of 1 wt%. The mixture was stirred at 600 r / min for 2 h, centrifuged at 10,000 rpm for 30 min, and the precipitate was freeze-dried at -20 °C for 12 h to obtain acid sustained-release microcapsules. (c) 10 g of the acid sustained-release microcapsules obtained in step (b) were placed in 100 mL of a mixture of ethanol and acetic acid (v:v=1:1), ultrasonicated at 200 W for 30 min, 5 g of ethylenediaminetetraacetic dianhydride (EDTAD) was added, reacted at 80° C. for 10 h, washed with deionized water to pH 7.4, and dried at 60° C. to obtain microcapsule-EDTA; (d) The modified sorbitan dodecanoate obtained in step (a) is mixed with deionized water in a mass ratio of 1:1, a seed crystal is put into it, and ultrasonic treatment is performed at 300 W for 20 min. After taking it out, it is added into a microcapsule-EDTA solution, in which the mass ratio of microcapsule-EDTA to deionized water is 1:1, and ultrasonic treatment is performed at 60° C. and 200 W for 15 min. The seed crystal is taken out and rinsed in ultrapure water for 8 times, each time for 30 s, and blown dry with nitrogen to obtain a pretreated seed crystal.

[0033] Embodiment 2: This embodiment provides a method for preparing an N-type single crystal silicon rod with high resistance uniformity, the preparation method is a Czochralski method, comprising the following steps: (1) Polycrystalline silicon material and dopant are placed in a quartz crucible. The dopant is composed of antimony and red phosphorus in a mass ratio of 8:1. The dopant has a phosphorus concentration of 3.5×10 18 Atom / cm 3 Adding dopants to polysilicon material, heating and melting at 1420° C. in an argon atmosphere of 70 slpm and 20 torr to a stable molten silicon; (2) Introducing a seed crystal into the stable molten silicon, followed by necking and shouldering, and then entering the equal diameter growth stage. The crucible temperature during necking is 1420°C, the crucible temperature during shouldering is 1000°C, the crucible speed is 9 rpm, and the crystal speed is 10 rpm; (3) During the whole stage of equal-diameter growth (the whole process from the beginning of equal-diameter growth after the shoulder release to the end of crystal growth), the crystal pulling rate was kept constant at 1.2 mm / min, the crucible temperature of equal-diameter growth was 1300°C, the crucible speed was 9 rpm, and the crystal speed was 11 rpm. At the beginning of equal-diameter growth, the argon pressure in the single crystal furnace was reduced to 0.5 torr and maintained until the growth of the CZ-pulled single crystal silicon rod was completed. The diameter of the equal-diameter region of the CZ-pulled single crystal silicon rod was 200 mm, and the equal-diameter length was 1300 mm. After cooling, an N-type single crystal silicon rod was obtained.

[0034] The seed crystal is a pre-treated seed crystal, and the pre-treatment method comprises the following steps: (a) 48 g of sorbitan dodecanoate and 27 g of 1-amino-1-deoxy-D-galactopyranose were mixed, and a mixed catalyst of 0.32 g of dodecylbenzenesulfonic acid and 0.16 g of p-toluenesulfonic acid was added under stirring at 180 rpm, and the mixture was reacted at 30 mmHg and 120°C for 5 h, and allowed to stand at 4°C for 3 h, filtered, and the residue was washed with anhydrous ethanol and deionized water, and dried under vacuum at 50°C for 12 h to obtain modified sorbitan dodecanoate; (b) 3 g of hydrofluoric acid, 15 g of acetic acid, and 9 g of citric acid were dissolved in 120 mL of deionized water, and stirred at 400 r / min for 10 min to obtain a mixed acid solution. 100 mL of the mixed acid solution was slowly added to 300 mL of 3 wt% chitosan acetic acid solution, and 2-aminoethyl stearate was added to a concentration of 1 wt%. The mixture was stirred at 500 r / min for 2 h, centrifuged at 10,000 rpm for 30 min, and the precipitate was freeze-dried at -20 °C for 12 h to obtain acid sustained-release microcapsules. (c) 10 g of the acid sustained-release microcapsules obtained in step (b) were placed in 100 mL of a mixture of ethanol and acetic acid (v:v=1:1), ultrasonicated at 200 W for 30 min, 3 g of ethylenediaminetetraacetic dianhydride (EDTAD) was added, reacted at 60° C. for 8 h, washed with deionized water to pH 7.2, and dried at 60° C. to obtain microcapsule-EDTA; (d) The modified sorbitan dodecanoate obtained in step (a) is mixed with deionized water in a mass ratio of 1:1, a seed crystal is put into it, and ultrasonic treatment is performed at 300 W for 20 min. After taking it out, it is added into a microcapsule-EDTA solution, in which the mass ratio of microcapsule-EDTA to deionized water is 1:1, and ultrasonic treatment is performed at 60° C. and 200 W for 15 min. The seed crystal is taken out and rinsed in ultrapure water for 6 times, each time for 30 s, and blown dry with nitrogen to obtain a pretreated seed crystal.

[0035] Embodiment 3: This embodiment provides a method for preparing an N-type single crystal silicon rod with high resistance uniformity, the preparation method is a Czochralski method, comprising the following steps: (1) Polycrystalline silicon material and dopant are placed in a quartz crucible. The dopant is composed of antimony and red phosphorus in a mass ratio of 8:1. The dopant has a phosphorus concentration of 3.5×10 18 Atom / cm 3 Adding dopants to polysilicon material, heating and melting at 1440° C. in an argon atmosphere of 70 slpm and 20 torr to a stable molten silicon; (2) A seed crystal is introduced into the stable molten silicon, and then after necking and shouldering, it enters the equal diameter growth stage. The crucible temperature during necking is 1480°C, the crucible temperature during shouldering is 1050°C, the crucible speed is 9.8 rpm, and the crystal speed is 10.8 rpm; (3) During the whole stage of equal-diameter growth (the whole process from the beginning of equal-diameter growth after the shoulder release to the end of crystal growth), the crystal pulling rate was kept constant at 1.5 mm / min, the crucible temperature of equal-diameter growth was 1350°C, the crucible speed was 9 rpm, and the crystal speed was 11 rpm. At the beginning of equal-diameter growth, the argon pressure in the single crystal furnace was reduced to 0.6 torr and maintained until the growth of the CZ-pulled single crystal silicon rod was completed. The diameter of the equal-diameter region of the CZ-pulled single crystal silicon rod was 203 mm, and the equal-diameter length was 1350 mm. After cooling, an N-type single crystal silicon rod was obtained.

[0036] The seed crystal is a pre-treated seed crystal, and the pre-treatment method comprises the following steps: (a) 56 g of sorbitan dodecanoate and 31.5 g of 1-amino-1-deoxy-D-galactopyranose were mixed, and a mixed catalyst of 0.4 g of dodecylbenzenesulfonic acid and 0.16 g of toluenesulfonic acid was added under stirring at 180 rpm, and the mixture was reacted at 35 mmHg and 120°C for 5.5 h, and allowed to stand at 4°C for 3.5 h. The mixture was filtered, and the residue was washed with anhydrous ethanol and deionized water, and dried under vacuum at 50°C for 13 h to obtain modified sorbitan dodecanoate; (b) Dissolve 3 g of hydrofluoric acid, 15 g of acetic acid, and 9 g of citric acid in 100 mL of deionized water, stir at 450 r / min for 10 min to obtain a mixed acid solution, slowly add 100 mL of the mixed acid solution into 300 mL of 3 wt% chitosan acetic acid solution, add 2-aminoethyl stearate to a concentration of 1 wt%, stir at 550 r / min for 2 h, centrifuge at 10,000 rpm for 30 min, precipitate and freeze-dry at -20 °C for 12 h to obtain acid sustained-release microcapsules; (c) 10 g of the acid sustained-release microcapsules obtained in step (b) were placed in 100 mL of a mixture of ethanol and acetic acid (v:v=1:1), ultrasonicated at 200 W for 30 min, 4 g of ethylenediaminetetraacetic dianhydride (EDTAD) was added, reacted at 70 ° C for 9 h, washed with deionized water to pH 7.3, and dried at 60 ° C to obtain microcapsule-EDTA; (d) The modified sorbitan dodecanoate obtained in step (a) is mixed with deionized water in a mass ratio of 1:1, a seed crystal is put into it, and ultrasonic treatment is performed at 300 W for 20 min. After taking it out, it is added into a microcapsule-EDTA solution, in which the mass ratio of microcapsule-EDTA to deionized water is 1:1, and ultrasonic treatment is performed at 60° C. and 200 W for 15 min. The seed crystal is taken out and rinsed in ultrapure water for 7 times, each time for 30 s, and blown dry with nitrogen to obtain a pretreated seed crystal.

[0037] The difference between Comparative Example 1 and Example 1 is that only phosphorus is doped as a dopant.

[0038] The difference between Comparative Example 2 and Example 1 is that only antimony is doped as a dopant.

[0039] The only difference between Comparative Example 3 and Example 1 is that no microcapsule-EDTA is added, and hydrofluoric acid, acetic acid and citric acid are directly added in the same amount as the amount of acid provided by the microcapsules.

[0040] The difference between Comparative Example 4 and Example 1 is that sorbitan dodecanoate is used instead of modified sorbitan dodecanoate.

[0041] The only difference between Comparative Example 5 and Example 1 is that the furnace pressure is not reduced and is kept unchanged.

[0042] Experimental Example 1: According to the methods of Example 1 and Comparative Examples 1-5, N-type single crystal silicon rods were prepared. Starting from the equal diameter position, a four-probe resistivity tester was used to measure the axial resistivity change rate of the single crystal silicon rod and the radial resistivity change rate of the head. The axial resistivity uniformity (%) and radial resistance uniformity (%) were calculated. The calculation formula is resistance uniformity (%) = [(highest resistivity - lowest resistivity) / lowest resistivity] × 100%. The results are as follows Figure 1 As shown, the resistivity distribution uniformity of Example 1 is good, which is better than that of Comparative Examples 1-5, indicating that the preparation method of an N-type single crystal silicon rod of the present invention can effectively improve the resistance uniformity of the single crystal silicon rod.

[0043] Experimental Example 2: The surface roughness of the pretreated seed crystals prepared in Examples 1-3 and Comparative Examples 3-4 was tested using a surface roughness instrument. The surface roughness was tested at 4 points and a middle point evenly distributed 10 mm from the edge of the pretreated seed crystal surface. The surface roughness after cleaning was measured by taking the average value of the 5 points. The surface roughness can reflect whether there are traces of corrosion pits on the surface of the sample after cleaning, and determine the smoothness of the sample surface. Metal impurity removal test: The single crystal silicon seed crystal samples before and after cleaning were tested using an X-ray diffraction (XRD) to detect the amount of metal impurities removed (mg / g). The results are shown in Table 1.

[0044] Table 1 Seed crystal surface roughness test

[0045] The results in Table 1 show that the surface roughness of the seed crystals after pretreatment in Examples 1-3 is the smallest, which is smaller than that in Comparative Examples 3-4. The amount of metal impurities removed from the seed crystals after pretreatment in Examples 1-3 is the highest, which is higher than that in Comparative Examples 3-4, indicating that the surface cleanliness of the seed crystals after pretreatment using the method of the present invention is higher, the surface finish is better, and the amount of metal impurities removed is higher.

[0046] Experimental Example 3: The number of times the single crystal silicon seed crystals pretreated in Examples 1-3 and Comparative Examples 3-4 can be placed when pulling single crystal silicon is actually tested. The number of times can be used to indicate the effect of different cleaning methods on the service life of the single crystal silicon seed crystal. If the single crystal silicon seed crystal turns black or colorful when pulling single crystal silicon, it cannot be used for seeding. The results are shown in Table 2.

[0047] Table 2 Results of average number of seed crystal placements

[0048] The results in Table 2 show that the seed crystals of Examples 1-3 can be drawn and released 4.21-4.25 times on average when pulling a single crystal silicon rod, while Comparative Examples 3-4 can be drawn and released 3.21-3.35 times. This shows that the method of the present invention has a better effect than the method of Comparative Examples 3-4, can increase the average number of seed crystal draws and releases, increase the service life of the single crystal silicon seed crystal, reduce crystal breakage, and improve the quality of crystal pulling.

[0049] Experimental Example 4: The 200 mm front diameter portion (single crystal silicon rod head) of the single crystal silicon rod prepared by the methods of Example 2 and Comparative Examples 1-5 was characterized and tested. The oxygen content of the single crystal silicon rod head was measured by a Fourier transform infrared tester. The results are as follows: Figure 2 shown.

[0050] Figure 2 The results show that the oxygen content of the head of the single crystal silicon rod prepared by the method of Example 2 is lower than that of Comparative Examples 1-5, indicating that the preparation method of the N-type single crystal silicon rod of the present invention can reduce the oxygen content of the head of the single crystal silicon rod, thereby improving its photoelectric conversion efficiency and improving the quality of the single crystal silicon rod.

[0051] Experimental Example 5: The first 200 mm of the equal diameter portion of the single crystal silicon rods (the heads of the single crystal silicon rods) prepared by the methods of Example 3 and Comparative Examples 1-5 were characterized and tested, and the minority carrier lifetime of the heads of the single crystal silicon rods was measured using a Sinton Instrument minority carrier lifetime tester. The results are shown in FIG. Figure 3 shown.

[0052] Figure 3The results show that the minority carrier lifetime at the head of the single crystal silicon rod prepared by the method of Example 3 is higher than that of Examples 1-5, indicating that the preparation method of the N-type single crystal silicon rod of the present invention can increase the minority carrier lifetime at the head of the single crystal silicon rod, improve the quality of the single crystal silicon rod, thereby increasing the number of pulled rods and further reducing production costs.

[0053] Experimental Example 6: The method of Example 1 and Comparative Examples 1-5 was used to prepare single crystal silicon rods, and the seeding breakage rate was counted. The results are as follows: Figure 4 As shown, the seeding breakage rate of Example 1 is significantly lower than that of Comparative Examples 1-5, indicating that the preparation method of the present invention can effectively reduce the seeding breakage rate, reduce the cost, and improve the qualified rate when preparing single crystal silicon rods.

[0054] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

Claims

1. A method for preparing an N-type single crystal silicon rod with high resistance uniformity, characterized in that: The preparation method is a Czochralski method, comprising the following steps: (1) placing polysilicon material and dopants in a quartz crucible and heating and melting them into stable molten silicon in a 20 torr argon atmosphere; (2) Introducing seed crystals into stable molten silicon, followed by necking and shoulder release before entering the isodiameter growth stage; (3) During the entire stage of equal-diameter growth, the crystal pulling rate is kept constant, and at the beginning of equal-diameter growth, the argon pressure in the single crystal furnace is reduced to 0.5-0.8 torr, and maintained until the growth of the CZ-pulled single crystal silicon rod is completed, and then cooled to obtain an N-type single crystal silicon rod; The seed crystal in step (2) is a pretreated seed crystal, and the pretreatment method comprises the following steps: (a) Sorbitol anhydride dodecanoate and 1-amino-1-deoxy-D-galactopyranose are mixed, and a mixed catalyst of dodecylbenzenesulfonic acid and p-toluenesulfonic acid is added under stirring, reacted at 30-40 mmHg and 120° C., allowed to stand at 4° C., filtered, the residue is washed, and vacuum dried to obtain modified sorbitol anhydride dodecanoate; (b) dissolving hydrofluoric acid, acetic acid and citric acid in deionized water, stirring to obtain a mixed acid solution, adding the mixed acid solution to a 3 wt % chitosan acetic acid solution, adding 2-aminoethyl stearate to a concentration of 1 wt %, stirring, centrifuging, and freeze-drying to obtain acid sustained-release microcapsules; (c) placing the acid sustained-release microcapsules obtained in step (b) into a mixture of ethanol and acetic acid, sonicating, adding EDTAD, reacting, washing, and drying to obtain microcapsules-EDTA; (d) The modified sorbitan dodecanoate obtained in step (a) is mixed with deionized water, and seed crystals are added thereto, ultrasonicated, taken out and added to microcapsule-EDTA solution, ultrasonicated, the seed crystals are taken out, rinsed in ultrapure water, and blown dry with nitrogen to obtain pretreated seed crystals.

2. The method for preparing an N-type single crystal silicon rod with high resistance uniformity according to claim 1, characterized in that: Step (1) The melting temperature is 1420-1450°C; the argon flow rate is 70 slpm; the dopant is antimony and red phosphorus in a mass ratio of 8:1; the dopant is phosphorus concentration 3.5×10 18 Atom / cm 3 Dopants are added to the polysilicon material.

3. The method for preparing an N-type single crystal silicon rod with high resistance uniformity according to claim 2, characterized in that: In step (2), the crucible temperature during necking is 1420-1500° C.; the crucible temperature during shouldering is 1000-1100° C., the crucible speed is 9-10 rpm, and the crystal speed is 10-11 rpm.

4. The method for preparing an N-type single crystal silicon rod with high resistance uniformity according to claim 3, characterized in that: In step (3), the crucible temperature of the equal-diameter growth is 1300-1400°C, the crucible speed is 9 rpm, and the crystal speed is 11 rpm; the diameter of the equal-diameter region of the CZS silicon rod is 200-205 mm, and the equal-diameter length is 1300-1400 mm; the full stage of the equal-diameter growth refers to the entire process from the beginning of the equal-diameter growth of the crystal rod after the shoulder is released to the end of the crystal growth; the crystal pulling rate ranges from 1.2-2 mm / min.

5. The method for preparing an N-type single crystal silicon rod with high resistance uniformity according to claim 4, characterized in that: In step (a), the mass ratio of sorbitan dodecanoate to 1-amino-1-deoxy-D-galactopyranose is 16:9; the mass ratio of dodecylbenzenesulfonic acid to p-toluenesulfonic acid is 2-3:1; and the mass ratio of the mixed catalyst to sorbitan dodecanoate is 1:

100.

6. The method for preparing an N-type single crystal silicon rod with high resistance uniformity according to claim 5, characterized in that: In step (b), the mass ratio of hydrofluoric acid, acetic acid and citric acid is 1:5:3; in the mixed acid solution, the dosage ratio of acetic acid to deionized water is 1-1.5 g:8 mL; and the volume ratio of the mixed acid solution to the chitosan acetic acid solution is 1:

3.

7. The method for preparing an N-type single crystal silicon rod with high resistance uniformity according to claim 6, characterized in that: In step (c), the dosage ratio of the acid sustained-release microcapsules to the mixed solution of ethanol and acetic acid is 1 g:10 mL; the volume ratio of ethanol to acetic acid in the mixed solution of ethanol and acetic acid is 1:1; and the mass ratio of the acid sustained-release microcapsules to EDTAD is 1:0.3-0.

5.

8. The method for preparing an N-type single crystal silicon rod with high resistance uniformity according to claim 7, characterized in that: The mass ratio of the modified sorbitan dodecanoate to deionized water in step (d) is 1:1; the mass ratio of microcapsule-EDTA to deionized water in the microcapsule-EDTA solution is 1:1.

Citation Information

Patent Citations

  • Method for controlling resistivity of N-type single crystal by utilizing antimony volatilization

    CN117344375A

  • Cleaning method of monocrystalline silicon seed crystal

    CN118497891A

  • New light-sensitive colour-former containing compositions for use in the manufacture of photographic materials

    GB839896A