Tire
By designing a structure in which the stress relaxation layer extends from the main groove to the land on the tire, combined with specific material composition and structural parameters, the problem of stress relaxation layer peeling and insufficient wet performance is solved, achieving better durability and wet performance.
Patent Information
- Application Number
- CN202380026897.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-29
AI Technical Summary
Existing tires have deficiencies in balancing the durability performance of the stress relaxation layer and wet performance. The stress relaxation layer is easy to peel off and has poor wet performance.
A tire is designed, the stress relaxation layer of which is mainly composed of diene rubber materials and non-diene rubber materials, contains carbon, vulcanizing agents and vulcanization accelerators, and is viewed from the cross-sectional view of the main groove in the meridian direction of the tire. The bottom of the groove continuously extends to the tread of the bank, covering the edge of the bank, ensuring that the width and total width of the stress relaxation layer are within a specific range to increase the bonding area and inhibit peeling.
It effectively inhibits the peeling of the stress relaxation layer, improves the wet performance of the tire, and ensures performance in the early stages of wear.
Smart Images

Figure CN118871306A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a tire, and more particularly to a tire capable of achieving both durability performance of a stress relaxation layer and wet performance of the tire. Background Art
[0002] In recent years, tires have adopted a structure in which a stress relaxation layer is provided at the groove bottom of the main groove, mainly for the purpose of suppressing groove cracking generated at the groove bottom of the main groove. As conventional tires adopting such a structure, the techniques described in Patent Documents 1 and 2 are known.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Laid-Open No. 2-45202
[0006] Patent Document 2: Japanese Patent Publication No. 2005-523193 Summary of the invention
[0007] Problems to be solved by the invention
[0008] An object of the present invention is to provide a tire capable of achieving both the durability performance of a stress relaxation layer and the wet performance of the tire.
[0009] Technical means of solving problems
[0010] In order to achieve the above-mentioned purpose, the tire of the present invention comprises: tread rubber exposed on the tread surface; a main groove and a land portion formed on the tread surface; and a stress relief layer formed on the groove bottom surface of the main groove, characterized in that the stress relief layer is mainly composed of a diene rubber material and a non-diene rubber material, and contains carbon, a vulcanizing agent and a vulcanization accelerator, and in a cross-sectional view in the tire meridian direction, the stress relief layer continuously extends from the groove bottom of the main groove to the tread surface of the land portion on at least one side and covers the edge portion of the land portion, the width Wc of the stress relief layer on the tread surface of the land portion is in the range of 0.06≤Wc / Hg relative to the groove depth Hg of the main groove, and the total width ∑Wc of the stress relief layer on the tread surface of one land portion is in the range of ∑Wc / Wb≤0.70 relative to the ground contact width Wb of the land portion.
[0011] Effects of the Invention
[0012] In the tire of the present invention, the stress relief layer extends continuously from the groove bottom of the main groove to the tread surface of the land portion and covers the edge of the land portion, thereby increasing the bonding area of the stress relief layer to the tread rubber compared to a structure in which the stress relief layer is formed only on the groove bottom and the groove wall. As a result, the peeling of the stress relief layer when the tire rotates is suppressed. In addition, the above lower limit of the Wc / Hg ratio appropriately ensures the width Wc of the stress relief layer on the tread surface of the land portion, thereby appropriately suppressing the peeling of the stress relief layer. In addition, the above upper limit of the ∑Wc / Wb ratio ensures the exposed area of the tread rubber on the tread surface of the land portion, thereby ensuring the wet performance of the tire in the early stage of wear. As a result, there is an advantage of being able to take into account both the durability performance of the stress relief layer and the wet performance of the tire. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a cross-sectional view in the tire meridian direction showing a tire according to an embodiment of the present invention.
[0014] Figure 2 Yes means Figure 1 A top view of the tread surface of the tire.
[0015] Figure 3 Yes means Figure 2 An enlarged view of a single-sided area of the tread surface of the tire.
[0016] Figure 4 Yes means Figure 3 A cross-sectional view of the shoulder main groove.
[0017] Figure 5 Yes means Figure 3 A cross-sectional view of the shoulder main groove.
[0018] Figure 6 Yes means Figure 3 A cross-sectional view of the shoulder main groove.
[0019] Figure 7 Yes means Figure 3 A cross-sectional view of the shoulder main groove.
[0020] Figure 8 Yes means Figure 2 An explanatory diagram of a variation of the tire described above.
[0021] Fig. 9 Yes means Figure 8 A cross-sectional view of the central main groove.
[0022] Fig.10 Yes means Figure 4 An explanatory diagram of a variation of the stress relaxation layer.
[0023] Fig.11 Yes means Figure 2 An explanatory diagram of a variation of the tire described above.
[0024] Fig.12 Yes means Fig.11 An illustration of the narrow shallow groove of the shoulder land portion.
[0025] Fig.13 Yes means Fig.11 An illustration of the narrow shallow groove of the shoulder land portion.
[0026] Fig.14 Yes means Figure 4 An explanatory diagram of a variation of the stress relaxation layer.
[0027] Fig.15 This is a graph showing the results of performance tests of tires according to the embodiments of the present invention.
[0028] Fig.16 This is a graph showing the results of performance tests of tires according to the embodiments of the present invention.
[0029] Fig.17 It is an explanatory diagram showing a test tire of a comparative example. DETAILED DESCRIPTION
[0030] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings. It should be noted that the present invention is not limited to the present embodiment. In addition, the constituent elements of the present embodiment include elements that are replaceable while maintaining the identity of the invention, and the replacement is obvious. In addition, the multiple variations described in the present embodiment can be arbitrarily combined within the scope that is obvious to those skilled in the art.
[0031] [tire]
[0032] Figure 1 1 is a cross-sectional view of a tire 1 according to an embodiment of the present invention in the tire meridian direction. This figure shows a cross-sectional view of a single side region in the tire radial direction. In this embodiment, a pneumatic radial tire for a passenger car is described as an example of a tire.
[0033] In this figure, the cross section in the tire meridian direction is defined as the cross section when the tire is cut on a plane including the tire rotation axis (not shown). In addition, the tire equatorial plane CL is defined as a plane passing through the midpoint of the tire cross section width specified by JATMA and perpendicular to the tire rotation axis. In addition, the tire width direction is defined as a direction parallel to the tire rotation axis, and the tire radial direction is defined as a direction perpendicular to the tire rotation axis.
[0034] The tire 1 has an annular structure centered on the tire rotation axis, and includes: a pair of bead cores 11, 11, a pair of bead cores 12, 12, a carcass layer 13, a belt layer 14, a tread rubber 15, a pair of sidewall rubbers 16, 16, and a pair of rim cushion rubbers 17, 17 (see Figure 1 ).
[0035] A pair of bead cores 11, 11 are formed by winding one or more bead wires made of steel in a ring shape and multiple times, and are buried in the bead portion to form the core of the left and right bead portions. A pair of bead edge cores 12, 12 are respectively arranged on the tire radial outer periphery of the pair of bead cores 11, 11 to reinforce the bead portion.
[0036] The carcass layer 13 has a single-layer structure formed by a layer of carcass ply or a multi-layer structure formed by stacking multiple carcass ply layers, and is annularly erected between the left and right bead cores 11, 11 to form the skeleton of the tire. In addition, the two ends of the carcass layer 13 are rolled back in a manner to wrap the bead core 11 and the bead core 12 and are clamped on the outside in the tire width direction. In addition, the carcass ply of the carcass layer 13 is formed by coating a plurality of carcass cords made of steel or an organic fiber material (for example, aramid, nylon, polyester, rayon, etc.) with a coating rubber and rolling them, and has a cord angle of 80 [deg] or more and 100 [deg] or less (defined as the inclination angle of the length direction of the carcass cord relative to the circumferential direction of the tire).
[0037] The belt layer 14 is formed by laminating a plurality of belt plies 141 to 143 and is disposed around the outer circumference of the carcass layer 13. The belt plies 141 to 143 include a pair of cross belts 141 and 142 and a belt cover layer 143.
[0038] The pair of cross belts 141, 142 is formed by coating a plurality of belt cords made of steel or organic fiber material with coating rubber and rolling them, and has a cord angle (defined as the inclination angle of the length direction of the belt cord relative to the tire circumferential direction) of 15 [deg] or more and 55 [deg] or less in absolute value. In addition, the pair of cross belts 141, 142 has cord angles of opposite signs, so that the length directions of the belt cords are intersected and stacked (so-called cross ply structure). In addition, the pair of cross belts 141, 142 are stacked and arranged on the tire radial outside of the carcass layer 13.
[0039] The belt covering layer 143 is formed by covering a belt covering layer cord formed of steel or an organic fiber material with a covering rubber, and has a cord angle of 0 [deg] or more and 10 [deg] or less in absolute value. In addition, the belt covering layer 143 is, for example, a strip-shaped profile formed by covering one or more belt covering layer cords with a covering rubber, and is formed by spirally winding the strip-shaped profile on the outer peripheral surface of the cross belts 141 and 142 multiple times in the tire circumferential direction. In addition, the belt covering layer 143 is arranged to cover the entire area of the cross belts 141 and 142.
[0040] The tread rubber 15 is arranged on the radial outer periphery of the carcass layer 13 and the belt layer 14 to constitute the tread portion of the tire 1. In addition, the tread rubber 15 includes a crown tread and a base tread (not shown). The crown tread is made of a rubber material having excellent ground contact characteristics and weather resistance, and is exposed on the entire outer peripheral surface of the tire to constitute the tread surface. Specifically, in order to reduce the rolling resistance of the tire and improve the wet performance of the tire, silica is blended into the crown tread. Furthermore, in order to improve the adhesion with the stress relief layer 4 described later in the crown tread blended with silica, it is preferred to blend carbon black with a particle size of not less than 20 [nm] and not more than 150 [nm] in the crown tread. The base tread is made of a rubber material having excellent heat resistance, and is sandwiched between the crown tread and the belt layer 14 (refer to Figure 1 ) constitute the basic part of the tread rubber 15.
[0041] A pair of sidewall rubbers 16, 16 are respectively arranged on the tire width direction outer side of the carcass layer 13 to form the left and right sidewall portions. A pair of rim cushion rubbers 17, 17 extend from the tire radial direction inner side of the left and right bead cores 11, 11 and the turned-back portion of the carcass layer 13 to the tire width direction outer side to form the rim fitting surface of the bead portion.
[0042] [Tread surface]
[0043] Figure 2 Yes means Figure 1 A top view of the tread surface of the tire 1. The figure shows the tread surface of a winter tire. In the figure, the tire circumference refers to the direction around the tire rotation axis. In addition, the reference numeral T is the tire ground contact end, and the dimension mark TW is the tire ground contact width.
[0044] like Figure 2 As shown, the tire 1 includes four circumferential main grooves 21 to 24 and five rows of land portions 31 to 35 on the tread surface.
[0045] The circumferential main grooves 21 to 24 are composed of a pair of shoulder main grooves 21, 24 and two central main grooves 22, 23. These circumferential main grooves 21 to 24 have an annular structure extending continuously over the entire circumference of the tire. The shoulder main grooves 21, 24 are the outermost circumferential main grooves in the tire width direction, and are each defined by the left and right areas where they are located with the tire equatorial plane CL as the boundary. The central main grooves 22, 23 are defined as circumferential main grooves that are closer to the tire equatorial plane CL than the shoulder main grooves 21, 24.
[0046] The main groove is defined as a groove having a display obligation of a wear indicator stipulated in JATMA. In addition, the circumferential main grooves 21 to 24 have a groove width of 4.0 [mm] or more and a groove depth of 6.2 [mm] or more.
[0047] The groove width is measured by the maximum value of the distance between the groove walls facing each other at the groove opening on the tread surface when the tire is mounted on a specified rim and filled with a specified internal pressure in an unloaded state. In the structure where the groove opening has a notch or chamfer, the groove width is measured with the intersection of the extension line of the tread surface and the extension line of the groove wall in the cross-sectional view in the groove width direction and parallel to the groove depth direction as the endpoint.
[0048] The groove depth is measured by the maximum value of the distance from the tread surface to the groove bottom in the unloaded state when the tire is mounted on a specified rim and filled with a specified internal pressure. In addition, if the groove bottom has a structure with local concave and convex parts or sipes, these are excluded and the groove depth is measured.
[0049] The prescribed rim refers to the "standard rim" prescribed by JATMA, the "design rim" prescribed by TRA, or the "measuring rim" prescribed by ETRTO. In addition, the prescribed internal pressure refers to the "maximum air pressure" prescribed by JATMA, the maximum value of the "tire load limits at various cold inflation pressures" prescribed by TRA, or the "inflation pressures" prescribed by ETRTO. In addition, the prescribed load refers to the "maximum load capacity" prescribed by JATMA, the maximum value of the "tire load limits at various cold inflation pressures" prescribed by TRA, or the "load capacity" prescribed by ETRTO. However, in JATMA, in the case of tires for passenger cars, the prescribed internal pressure is an air pressure of 180 [kPa], and the prescribed load is 88 [%] of the maximum load capacity under the prescribed internal pressure.
[0050] For example, in Figure 2 In the structure, the distance from the tire equatorial plane CL to the groove center line of the left and right shoulder main grooves 21, 24 (dimension marks omitted in the figure) is within the range of 19[%] to 34[%] of the tire contact width TW.
[0051] The slot centerline is defined as a virtual line connecting the midpoints of the distance between opposing slot walls.
[0052] The tire contact width TW is measured by the maximum straight-line distance in the tire axial direction on the contact surface between the tire and the flat plate when the tire is mounted on a specified rim and applied with a specified internal pressure, and is placed perpendicular to the flat plate in a stationary state and applied with a load corresponding to a specified load.
[0053] The tire ground contact edge T is defined as the maximum axial width position of the tire on the contact surface between the tire and the flat plate when the tire is mounted on a specified rim and applied with a specified internal pressure, and is placed perpendicular to the flat plate in a stationary state and applied with a load corresponding to a specified load.
[0054] The land portions 31 to 35 are composed of a pair of shoulder land portions 31, 35, a pair of intermediate land portions 32, 34, and a row of central land portions 33. These land portions 31 to 35 are divided by the circumferential main grooves 21 to 24, and constitute an annular tread extending over the entire circumference of the tire. The shoulder land portions 31, 35 are defined as land portions on the outer side of the tire width direction divided by the shoulder main grooves 21, 24. In addition, the pair of shoulder land portions 31, 35 are arranged in the left and right areas with the tire equatorial plane CL as the boundary. The intermediate land portions 32, 34 are defined as land portions on the inner side of the tire width direction divided by the shoulder main grooves 21, 24. In addition, the pair of intermediate land portions 32, 34 are arranged in the left and right areas with the tire equatorial plane CL as the boundary. The central land portion 33 is defined as a land portion closer to the tire equatorial plane CL side than the intermediate land portions 32, 34.
[0055] In addition, Figure 2 In the embodiment, the contact widths Wb1 and Wb5 of the shoulder land portions 31 and 35 are within a range of 12% to 26% relative to the tire contact width TW. In addition, the contact widths Wb2 and Wb4 of the intermediate land portions 32 and 34 are within a range of 8% to 27% relative to the tire contact width TW. In addition, the contact width Wb3 of the center land portion 33 is within a range of 10% to 23% relative to the tire contact width TW.
[0056] The ground contact width of the land portion is measured by the maximum straight-line distance in the tire axial direction on the contact surface between the land portion and the flat plate when the tire is mounted on a specified rim and applied with a specified internal pressure, and is placed perpendicular to the flat plate in a stationary state and applied with a load corresponding to a specified load.
[0057] In addition, Figure 2 In the structure of the tire 1, as described above, by providing the tire 1 with a pair of shoulder main grooves 21, 24 and two central main grooves 22, 23, a pair of shoulder land portions 31, 35, a pair of intermediate land portions 32, 34 and a single central land portion 33 are defined. However, the tire 1 is not limited thereto, and may also include a single or more than three central main grooves (omitted from the illustration). In the former structure, the central land portion is omitted, and in the latter structure, more than two rows of central land portions are defined.
[0058] In addition, Figure 2 In the structure, the central main groove 22 on one side (the left side in the figure) has a zigzag shape formed by alternately connecting long strips and short strips in the tire circumferential direction. In addition, the left and right shoulder main grooves 21, 24 have a straight line shape. However, this is not limited to this, and any circumferential main grooves 21 to 24 may have a straight line shape, or may have a zigzag shape, a wave shape, or a step shape with an amplitude in the tire width direction (illustration omitted). For example, a structure in which all circumferential main grooves 21 to 24 have a straight line shape may be adopted (illustration omitted).
[0059] In addition, Figure 2 In the structure, the left and right shoulder land portions 31, 35, the middle land portion 32 on one side (left side in the figure), and the central land portion 33 respectively have through lug grooves 311, 321, 331, 351 penetrating the land portions 31, 35, whereby these land portions 31, 32, 33, 35 are divided in the tire circumferential direction to form pattern block rows. In addition, the lug groove 311 of the middle land portion 34 on the other side has a single-side open lug groove 341, whereby the land portion 34 is formed as a rib having a tread surface continuous in the tire circumferential direction. In addition, the land portions 31 to 35 each have a plurality of sipes (the reference numerals in the figure are omitted).
[0060] The lug grooves 311 to 351 are transverse grooves extending in the tire width direction, and have a width of 1.5 [mm] or more and a depth of 3.0 [mm] or more, and open when the tire contacts the ground to function as grooves.
[0061] [Stress relaxation layer]
[0062] Figure 3 Yes means Figure 2 An enlarged view of a single-side area of the tread surface of the tire 1. Figure 4 and Figure 5 Yes means Figure 3 The cross-sectional view of the shoulder main groove 21. In these figures, Figure 4 An enlarged cross-sectional view of the tire width direction showing the shoulder main groove 21, Figure 5 An enlarged cross-sectional view along the tire circumferential direction of the shoulder main groove 21 is shown.
[0063] The tire 1 includes a stress relaxation layer 4 formed on the surface of the groove bottom of the main grooves 21 and 24 to suppress groove cracking. Figure 2 In the structure of the tire, the stress relief layer 4 is formed on the left and right shoulder main grooves 21 and 24, respectively, where groove cracking is likely to occur. On the other hand, the stress relief layer 4 is not formed on the central main grooves 22 and 23. However, the present invention is not limited thereto, and the stress relief layer 4 may be formed on the central main grooves 22 and 23 in addition to the shoulder main grooves 21 and 24 (see the following description). Figure 8 ).
[0064] Here, as an example, the stress relaxation layer 4 formed on the shoulder main groove 21 on one side (the left side in the figure) is described, and the shoulder main groove 24 on the other side is the same as the shoulder main groove 21 on one side, so its description is omitted.
[0065] The stress relaxation layer 4 is mainly composed of diene rubber material and non-diene rubber material, and contains carbon, vulcanizing agent and vulcanization accelerator. Diene rubber is selected from the group consisting of diene polymers including natural rubber, synthetic diene rubber (isoprene rubber (IR), butadiene rubber (BR), styrene butadiene rubber (SBR), acrylonitrile butadiene rubber (NBR), chloroprene rubber (CR), etc.). Non-diene rubber is selected from the group consisting of non-diene polymers including synthetic non-diene rubber (butyl rubber (IIR), ethylene propylene rubber (EPDM, EPM), polyurethane rubber, silicone rubber, etc.). In addition, in order to ensure weather resistance, the stress relaxation layer 4 preferably does not contain a resin component.
[0066] In addition, the stress relaxation layer 4 preferably does not contain an anti-aging agent. Such a structure is more preferred in terms of suppressing the transfer of the stress relaxation layer 4 to the mold and suppressing coloring on the stress relaxation layer 4 in a structure where a coating material of the stress relaxation layer 4 described later is applied to the unvulcanized tread rubber 15 and a vulcanization molding process is performed.
[0067] However, the stress relaxation layer 4 may also contain an antioxidant, without being limited thereto. In this case, it is preferred not to use an amine antioxidant, but to mix other antioxidants (e.g., phenols, phosphorous acids, organic thioacids, benzimidazoles, etc.) in an amount of 0.1 to 5 parts by weight relative to 100 parts by weight of the rubber component.
[0068] In addition, the modulus Mc of the stress relaxation layer 4 when stretched 100% at 100 [°C] is in the range of 0.3 [MPa] ≤ Mc ≤ 2.8 [MPa], preferably in the range of 0.4 [MPa] ≤ Mc ≤ 2.3 [MPa], more preferably in the range of 0.5 [MPa] ≤ Mc ≤ 1.8 [MPa], and further preferably in the range of 0.6 [MPa] ≤ Mc ≤ 1.5 [MPa]. The above lower limit suppresses damage to the stress relaxation layer 4 caused by foreign matter (such as pebbles, etc.) intruding into the main groove when the tire rotates, and the above upper limit suppresses uneven wear of the land portion caused by excessive modulus Mc of the stress relaxation layer 4.
[0069] In addition, the modulus Mc of the stress relaxation layer 4 when it is elongated 100% at 100 [°C] is within the range of 0.45≤Mc / Mt≤1.15, preferably within the range of 0.50≤Mc / Mt≤1.10, relative to the modulus Mt of the tread rubber 15 when it is elongated 100% at 100 [°C]. In addition, for example, in the case of a summer tire, the above Mc / Mt ratio is preferably within the range of 0.50≤Mc / Mt≤0.90, and in the case of a winter tire, the above Mc / Mt ratio is preferably within the range of 0.70≤Mc / Mt≤1.10.
[0070] The moduli Mc and Mt are measured by a tensile test at 100° C. using a dumbbell-shaped test piece in accordance with JIS K6251 (using a No. 3 dumbbell). The modulus Mt of the tread rubber 15 is the modulus of the rubber material in the portion in surface contact with the stress relaxation layer 4 .
[0071] In addition, the rubber hardness Hc of the stress relaxation layer 4 is within the range of 0≤Ht-Hc≤32, preferably within the range of 2≤Ht-Hc≤27, relative to the rubber hardness Ht of the tread rubber 15. The above lower limit ensures the rubber hardness Hc of the stress relaxation layer 4, thereby suppressing the damage of the stress relaxation layer 4 caused by foreign matter (such as pebbles, etc.) invading the main groove when the tire rotates. In addition, the above upper limit suppresses the uneven wear of the land portion caused by excessive rubber hardness Hc of the stress relaxation layer 4.
[0072] The rubber hardness Hc and Ht are measured at a temperature of 20[°C] in accordance with JIS K6253. The rubber hardness Ht of the tread rubber 15 is measured for the rubber material constituting the tread rubber 15 that is in surface contact with the stress relaxation layer 4 .
[0073] In addition, the tensile strength TBc of the stress relief layer 4 is within the range of 0.30≤TBc / TBt≤0.90 relative to the tensile strength TBt of the tread rubber 15, and preferably within the range of 0.35≤TBc / TBt≤0.88. The above lower limit ensures the tensile strength TBc of the stress relief layer 4, thereby ensuring the fracture durability of the stress relief layer 4 against deformation during tire rotation. In addition, the above upper limit suppresses the peeling of the stress relief layer caused by excessive tensile strength TBc of the stress relief layer 4. In addition, the tensile strength TBc of the stress relief layer 4 is preferably within the range of 3[MPa]≤TBt-TBc≤15[MPa] relative to the tensile strength TBt of the tread rubber 15.
[0074] The tensile strengths TBc and TBt are measured by a tensile test at room temperature (temperature 20° C.) using a dumbbell-shaped test piece in accordance with JIS K6251 (using a No. 3 dumbbell). In addition, the tensile strength TBt of the tread rubber 15 is the tensile strength of the rubber material in the portion in surface contact with the stress relaxation layer 4.
[0075] In addition, if Figure 3 and Figure 5 As shown in FIG. 1 , the stress relaxation layer 4 extends continuously in the tire circumferential direction along the main groove 21. Figure 3 and Figure 4 As shown in FIG. 1 , the stress relaxation layer 4 not only covers the bottom of the main groove 21, but also continuously extends to the groove wall and the groove opening to cover the entire area of the inner wall of the main groove 21. Figure 4 As shown, in the cross-sectional view in the tire meridian direction, the stress relaxation layer 4 is bent at the edge of the land portions 31, 32 and extends to the tread surface of the land portions 31, 32 to cover the edge of the land portions 31, 32. In addition, the stress relaxation layer 4 has an edge portion at the tread surface of the land portions 31, 32, that is, the ground contact area.
[0076] On the other hand, Figure 3 and Figure 4 As shown in FIG. 1 , the tread surface of the land portions 31 and 32 has an uncovered area (the reference numerals in the figure are omitted) that is not covered by the stress relaxation layer 4 in the central part in the width direction of the land portions 31 and 32. In this uncovered area, the tread rubber 15 is exposed to form the contact surface of the land portions 31 and 32. Figure 3 In the structure, the shoulder main groove 21 has a straight line shape, and the edge portion of the stress relaxation layer 4 has a straight line shape along the shoulder main groove 21.
[0077] In the above structure, the stress relief layer 4 continuously extends from the groove bottom of the main groove 21 to the tread surface of the land portions 31 and 32 and covers the edge portions of the land portions 31 and 32. Therefore, it is different from the structure in which the stress relief layer 4 is formed only on the groove bottom and the groove wall (refer to the structure described later). Fig.17 ), the adhesion area of the stress relief layer 4 to the tread rubber 15 is increased compared to the structure in which the stress relief layer 4 is provided only on the groove bottom and the groove wall (see the structure in which the stress relief layer 4 is provided only on the groove bottom and the groove wall). Fig.17 ), and a structure in which the stress relaxation layer covers the entire tread area of the land portion (not shown), the peeling durability of the stress relaxation layer 4 and the wet performance of the tire are effectively balanced.
[0078] In addition, Figure 3 and Figure 4 In the embodiment, the width Wc of the stress relaxation layer 4 on the tread surface of the land portions 31 and 32 is Figure 3 , the width WcA of the shoulder land portion 31 and the width WcB of the middle land portion 32 relative to the groove depth Hg (Hg1) of the main groove 21 are in the range of 0.06≤Wc / Hg, preferably in the range of 0.10≤Wc / Hg. The above lower limit appropriately ensures the width Wc of the stress relief layer 4 on the tread of the land portions 31 and 32, thereby appropriately suppressing the peeling of the stress relief layer 4. That is, the deeper the main groove 21, the greater the deformation of the main groove 21 when the tire rotates, so the greater the groove depth Hg of the main groove 21, the greater the width Wc of the stress relief layer 4 needs to be set. It should be noted that the upper limit of the Wc / Hg ratio is not particularly limited, but is subject to other conditions.
[0079] The width Wc of the stress relief layer 4 on the tread surface of the land portions 31 and 32 is measured as the distance in the tire width direction from the edge of the land portions 31 and 32 to the edge of the stress relief layer 4 in the cross-sectional view in the tire meridian direction. Fig. 9 ), the width Wc of the stress relaxation layer 4 is measured with the intersection of the extension line of the groove wall of the main groove and the extension line of the tread of the land portion as the endpoint.
[0080] In addition, Figure 3 and Figure 4In the embodiment, the total width ΣWc of the stress relaxation layer 4 on the tread of one land portion 31, 32 is within the range of ΣWc / Wb≤0.70, preferably within the range of ΣWc / Wb≤0.68, relative to the ground contact width Wb (Wb1, Wb2) of the land portions 31, 32. Therefore, it is ensured that the exposed width (dimension marks in the figure are omitted) of the tread rubber 15 on the tread of the land portions 31, 32 is 30 [%] or more relative to the ground contact width Wb of the land portions 31, 32. Since the above upper limit ensures the exposed area of the tread rubber 15 on the tread of the land portions 31, 32, the wet performance of the tire in the early stage of wear is ensured. It should be noted that the lower limit of the ΣWc / Wb ratio is not particularly limited, but is subject to other conditions.
[0081] For example, in Figure 3 In the structure of, since the central main groove 22 does not have the stress relief layer 4, the total width ∑Wc of the stress relief layer 4 on the tread surface of the shoulder land portion 31 is WcA, and the total width ∑Wc of the stress relief layer 4 on the tread surface of the intermediate land portion 32 is WcB. On the other hand, in the structure where the stress relief layer 4 is formed on the central main grooves 22 and 23 in addition to the shoulder main grooves 21 and 24 (see Figure 2 and the following Figure 8 ), the width Wc of the stress relief layer 4 exists respectively at the left middle land portion 32, the central land portion 33 and the left and right edge portions of the middle land portion 34 on the right side of the figure, so the total width ∑Wc of the stress relief layer 4 on each land portion 32 to 34 is set to satisfy the above conditions.
[0082] In addition, Figure 4 , the width Wc (WcA, WcB) of the stress relaxation layer 4 on the tread surface of the land portions 31, 32 is relative to the ground contact width Wb (Wb1, Wb2) of the land portions 31, 32. Figure 2 ) is in the range of 0.02≤Wc / Wb≤0.50, preferably in the range of 0.03≤Wc / Wb≤0.35. In addition, in the structure where the edge of the land portion 31, 32 has a straight shape, the Wc / Wb ratio is preferably set in the range of 0.02≤Wc / Wb≤0.12. The above lower limit appropriately ensures the width Wc of the stress relaxation layer 4 on the tread surface of the land portion 31, 32, and the above upper limit ensures the exposed area of the tread rubber 15 on the tread surface of the land portion 31, 32. For example, Figure 3 In the structure of FIG. 1 , since the edge portions of the land portions 31 and 32 have a straight line shape, the width Wc of the stress relaxation layer 4 is equal to the width Wc of the stress relaxation layer 4 described later. Figure 8The structure is set to be relatively narrow. Additionally, since the shoulder circumferential land portions 31 and the intermediate circumferential land portions 32 only have the stress relaxation layer 4 at the edge portions on the side of the main shoulder groove 21, the ratio ∑Wc / Wb of the total width of the stress relaxation layer 4 is set to be small. Thereby, a relatively large exposed area of the tread rubber 15 is ensured.
[0083] In addition, in Figure 4 , the width Wc (WcA, WcB) of the stress relaxation layer 4 on the tread surface of the circumferential land portions 31, 32 with respect to the thickness Gc1 of the stress relaxation layer 4 at the bottom of the main groove 21 is in the range of 2.0 ≤ Wc / Gc1 ≤ 70, preferably in the range of 2.3 ≤ Wc / Gc1 ≤ 65. Additionally, the thickness Gc1 of the stress relaxation layer 4 at the bottom of the main groove 21 is in the range of 0.030 [mm] ≤ Gc1 ≤ 0.400 [mm], preferably in the range of 0.040 [mm] ≤ Gc1 ≤ 0.380 [mm]. Thereby, the thickness Gc1 of the stress relaxation layer 4 at the bottom of the main groove 21 is optimized, and thus the peeling of the stress relaxation layer 4 during tire rotation is suppressed.
[0084] The thickness Gc1 of the stress relaxation layer 4 at the bottom of the main groove 21 is measured on the groove center line (not shown) of the main groove 21.
[0085] In addition, in Figure 4 , the minimum value Gc2_min of the thickness Gc2 (Gc2A, Gc2B) of the stress relaxation layer 4 in the specified region of the groove wall of the main groove 21 is thinner than the thickness Gc1 of the stress relaxation layer 4 at the bottom of the main groove 21 (Gc2_min < Gc1). In such a structure, the stress relaxation layer 4 has a thin wall portion on the groove wall of the main groove 21, thereby suppressing the peeling of the stress relaxation layer 4 at the bottom of the main groove 21. Additionally, the ratio Gc2_min / Gc1 is in the range of Gc2_min / Gc1 ≤ 0.60, preferably in the range of Gc2_min / Gc1 ≤ 0.40. Additionally, the minimum value Gc2_min of the thickness Gc2 of the stress relaxation layer 4 is preferably 0.003 [mm] or more.
[0086] The thickness Gc2 (Gc2A, Gc2B) of the stress relaxation layer 4 on the groove wall of the main groove 21 is measured in the region from 40 [%] to 60 [%] of the groove depth Hg1 from the bottom of the main groove 21.
[0087] In addition, in Figure 4In this case, the minimum value Gc2_min of the thickness Gc2 (Gc2A, Gc2B) of the stress relaxation layer 4 on the groove wall of the main groove 21 is thinner than the thickness Gc3 of the stress relaxation layer 4 on the tread surfaces of the annular shoulders 31 and 32 (Gc2_min < Gc3). In such a structure, since the stress relaxation layer 4 has a thin-walled portion on the groove wall of the main groove 21, when wear occurs, the situation where the entire stress relaxation layer 4 peels off from the groove wall of the main groove 21 to the groove bottom is suppressed during the process of the portion of the stress relaxation layer 4 exposed on the tread surfaces of the annular shoulders 31 and 32 being worn away. In addition, the ratio Gc2_min / Gc3 is in the range of Gc2_min / Gc3 ≤ 0.60, preferably in the range of Gc2_min / Gc3 ≤ 0.40.
[0088] In addition, in Figure 4 this case, the thickness Gc3 (Gc3A, Gc3B) of the stress relaxation layer 4 on the tread surfaces of the annular shoulders 31 and 32 is in the range of 0.030 [mm] ≤ Gc3 ≤ 0.400 [mm], preferably in the range of 0.040 [mm] ≤ Gc3 ≤ 0.380 [mm]. Thereby, the deterioration of the performance of the tread surface due to the stress relaxation layer 4 coming into contact with the ground is suppressed.
[0089] Regarding the thickness Gc3 of the stress relaxation layer 4 on the tread surfaces of the annular shoulders 31 and 32, the maximum value of the thickness of the portion of the stress relaxation layer 4 exposed on the tread surfaces of the annular shoulders 31 and 32 is measured.
[0090] In addition, in Figure 4 this case, the left and right groove wall angles θgA, θgB [deg] of the main groove 21 have a relationship of 2.0×(Wg + Hg) - 35.0 ≤ θgA + θgB ≤ 4.5×(Wg + Hg) - 22.5 with respect to the groove width Wg (Wg1) [mm] and the groove depth Hg (Hg1) [mm] of the main groove 21, preferably having a relationship of 2.5×(Wg + Hg) - 40.0 ≤ θgA + θgB ≤ 4.0×(Wg + Hg) - 25.0. Thereby, the adhesiveness of the stress relaxation layer 4 on the groove bottom of the main groove 21 is improved, and the peeling of the stress relaxation layer 4 is effectively suppressed.
[0091] Regarding the groove wall angles θgA, θgB of the main groove 21, the angles formed between the groove wall surface of the main groove 21 and the groove depth direction are measured in the cross-sectional view in the tire meridian direction in the unloaded state where the tire is mounted on a specified rim and a specified internal pressure is applied.
[0092] In addition, in Figure 4Among the curvature radii RgA and RgB [mm] of the connection between the groove bottom of the main groove 21 and the left and right groove walls, the smaller curvature radius Rg_min satisfies the following formula (1) with respect to the groove width Wg (Wg1) [mm], the groove depth Hg (Hg1) [mm] and the left and right groove wall angles θgA and θgB [deg] of the main groove 21. Thus, the distribution of the thickness of the stress relaxation layer 4 on the groove bottom of the main groove 21 is optimized, thereby effectively suppressing the peeling of the stress relaxation layer 4.
[0093] [Formula 1]
[0094]
[0095] The curvature radii RgA and Rg of the connection between the groove bottom and the left and right groove walls of the main groove 21 are measured in a cross-sectional view in the tire meridian direction in an unloaded state with the B tire mounted on a predetermined rim and a predetermined internal pressure applied.
[0096] In addition, Figure 4 , the thickness Gc1 [mm] of the stress relief layer 4 on the groove bottom of the main groove 21 is in the range of 0.055×e^(-0.452×UG)≤Gc1≤0.070×e^(-0.620×UG)+0.150 relative to the groove bottom thickness UG [mm] of the tread rubber 15, and preferably in the range of 0.065×e^(-0.368×UG)≤Gc1≤0.070×e^(-0.551×UG)+0.125.
[0097] The groove bottom thickness UG of the tread rubber 15 is measured from the groove bottom of the main groove 21 to the outermost layer of the belt layer 14 (at Figure 4 Specifically, a virtual line (not shown) connecting the radially outer end points of the belt cords constituting the outermost layer 143 of the belt layer 14 is drawn, and the distance from the groove bottom of the main groove 21 to the virtual line is measured.
[0098] In addition, if Figure 5 As shown, the stress relaxation layer 4 extends in the tire circumferential direction along the main groove 21 and has a uniform thickness Gc1. In addition, the stress relaxation layer 4 is arranged to cover the entire surface of the wear indicator 5. As such, when the main groove 21 has a convex portion or a concave portion at the groove bottom, it is preferred that the stress relaxation layer 4 is arranged to cover the entire convex portion or the concave portion.
[0099] In addition, the convex or concave portion formed at the groove bottom is preferably composed of a straight line and / or a curve having a curvature radius of 10 [mm] or more in the cross-sectional view in the tire circumferential direction. This suppresses the deformation of the convex or concave portion when the tire rotates, thereby suppressing the peeling of the stress relief layer 4. Figure 5In the structure, the curvature radius Ri1 of the connection portion between the side wall of the wear indicator 5 and the groove bottom of the main groove 21 and the curvature radius Ri2 of the connection portion between the side wall of the wear indicator 5 and the top are set to be 10 [mm] or more. In addition, as in a snow platform (not shown), when the height of the convex portion from the groove bottom is 1 / 3 or more of the groove depth Hg1 of the main groove 21, at least the curvature radius Ri1 of the connection portion between the side wall of the convex portion and the groove bottom of the main groove 21 satisfies the above conditions.
[0100] Figure 6 Yes means Figure 3 The cross-sectional view of the shoulder main groove 21. This figure shows the cross-sectional view of the shoulder main groove 21 at the opening position of the lug grooves 311, 321.
[0101] like Figure 6 As shown, at the intersection of the main groove 21 and the transverse grooves 311, 321, the stress relief layer 4 extends continuously from the groove bottom of the main groove 21 to the groove bottom of the transverse grooves 311, 321, and terminates at the groove bottom of the transverse grooves 311, 321. In addition, the width Wc' (Wc'A, Wc'B) of the stress relief layer 4 on the groove bottom of the transverse grooves 311, 321 is in the range of 0.06≤Wc' / Hg≤1.00 relative to the groove depth Hg (Hg1) of the main groove 21, preferably in the range of 0.10≤Wc' / Hg≤0.90. In this way, by extending the stress relief layer 4 continuously from the groove bottom of the main groove 21 to the groove bottom of the transverse grooves 311, 321, the peeling of the stress relief layer 4 on the groove bottom of the main groove 21 can be effectively suppressed. For example, in Figure 6 In the structure, the groove depths H11 and H21 of the transverse grooves 311 and 321 are shallower than the groove depth Hg1 of the main groove 21. Therefore, a height difference is generated between the groove bottom of the main groove 21 and the groove bottom of the transverse grooves 311 and 321. Moreover, the stress relief layer 4 is formed in a manner covering the edge portion having the height difference. Thus, peeling of the stress relief layer 4 is effectively suppressed.
[0102] The width Wc′ (Wc′A, Wc′B) of the stress relaxation layer 4 on the groove bottom of the lug grooves 311 , 321 is defined as the extension distance on the groove bottom of the lug grooves 311 , 321 in the tire width direction.
[0103] Figure 7 Yes means Figure 3 The cross-sectional view of the shoulder main groove 21. This figure shows the cross-sectional view of the shoulder main groove 21 at the opening position of the sipe 6.
[0104] exist Figure 3In the structure, the land portions 31 and 32 have a plurality of sipes 6, and a portion of the sipes 6 opens at the main groove 21. In such a structure, since a portion of the stress relief layer 4 is divided along the tire circumferential direction by the opening of the sipes 6, the stress generated on the stress relief layer 4 during tire rotation is dispersed, and the peeling of the stress relief layer 4 is suppressed. Figure 7 In the embodiment, the opening depth Hs (HsA, HsB) of the sipe 6 relative to the groove depth Hg (Hg1) of the main groove 21 is preferably within the range of 0.10≤Hs / Hg≤0.80. The above lower limit ensures the inhibitory effect of the sipe 6 on the peeling of the stress relaxation layer 4, and the above upper limit inhibits the groove cracking that occurs starting from the sipe 6. In addition, the interval Ds (not shown in the figure. See FIG. 1 ) between adjacent sipes 6 and 6 in the tire circumferential direction is 0.10≤Hs / Hg≤0.80. Figure 3 ) preferably has a relationship of Ds≤Hg with respect to the groove depth Hg of the main groove 21.
[0105] The sipes 6 are grooves formed on the tread surface of the tire, and are closed when the tire contacts the ground by having a maximum width of less than 1.5 [mm] and a maximum depth of more than 1.5 [mm] (size marks omitted in the figure). When the tire contacts the ground, the sipes 6 absorb and remove the water film on the icy road surface, thereby improving the closeness of the tread surface of the block 5 to the icy road surface (so-called adhesive friction). As a result, the tire's performance on ice is improved.
[0106] The sipe width is measured as the opening width of the sipe on the tread surface in a no-load state in which the tire is mounted on a predetermined rim and filled with a predetermined internal pressure.
[0107] The sipe depth is measured as the distance from the tread surface to the bottom of the sipe when the tire is mounted on a specified rim and filled with a specified internal pressure in an unloaded state. In addition, if the sipe has a structure with a local bottom raised portion or a concave-convex portion at the sipe bottom, these are excluded when measuring the sipe depth.
[0108] The opening depth Hs (HsA, HsB) of the sipe 6 is measured by the extension length of the opening of the sipe 6 on the groove wall of the main groove 21 in the groove depth direction.
[0109] [Example of variation]
[0110] Figure 8 Yes means Figure 2 Explanatory diagram of a modified example of the tire 1. This figure shows an enlarged view of the central area of the tread surface. Fig. 9 Yes means Figure 8 The cross-sectional view of the central main groove 23 is shown in FIG. Figure 3 and Figure 4The same components as those described above are denoted by the same reference numerals, and description thereof will be omitted.
[0111] exist Figure 2 In the structure, as described above, the stress relaxation layer 4 is formed on the left and right shoulder main grooves 21 and 24, respectively, but is not formed on the central main grooves 22 and 23. However, this is not limited to this. Figure 8 As shown, the stress relaxation layer 4 may be formed in the center main grooves 22 , 23 in addition to being formed in the left and right shoulder main grooves 21 , 24 .
[0112] exist Figure 8 In the structure, the stress relief layer 4 is formed on the left and right central main grooves 22 and 23, respectively. In addition, the central main groove 22 on the left side of the figure has a serrated shape with an amplitude in the tire width direction, and the stress relief layer 4 is arranged to cover the entire central main groove 22. In addition, the width Wc (WcA_min, WcA_max, WcB_min, WcB_max) of the stress relief layer 4 on the tread of the land portions 32 and 33 is within the range of 0.06≤Wc / Hg≤1.00 relative to the groove depth Hg (illustration omitted) of the central main groove 22. In addition, the width Wc (WcA_min, WcA_max, WcB_min, WcB_max) of the stress relief layer 4 on the tread of the land portions 32 and 33 is within the range of 0.06≤Wc / Hg≤1.00 relative to the ground contact width Wb (Wb2, Wb3. Refer to Figure 2 ) is in the range of 0.02≤Wc / Wb≤0.50.
[0113] In addition, the stress relaxation layer 4 is formed in three or more main grooves (for example, Figure 8 In the structure of the variation example (4 main grooves 21 to 24), the total width ∑Wb of the stress relief layer 4 on the tire contact surface is within the range of ∑Wc / TW≤0.20 relative to the tire contact width TW, preferably within the range of ∑Wc / TW≤0.18. Thus, the exposed area of the tread rubber 15 on the tire contact surface is ensured, thereby ensuring the wet performance of the tire.
[0114] In addition, Figure 8 In the structure, the middle land portion 34 on the right side of the figure has a plurality of chamfered portions 342 at the edge portion on the central main groove 23 side. Fig. 9 As shown, the stress relaxation layer 4 is arranged to extend from the groove bottom of the central main groove 23 to the tread surface of the intermediate land portion 34 and to cover the chamfered portion 342 of the intermediate land portion 34. In this way, even in a structure where the land portion 34 has the chamfered portion 342, by extending the stress relaxation layer 4 to the tread surface of the land portion 34 and exposing it, the peeling of the stress relaxation layer 4 can be appropriately suppressed.
[0115] In addition, Figure 2In the structure, the left and right shoulder main grooves 21 and 24 have a straight shape, and thus the edges of the left and right land portions 31 and 32 have a straight shape. On the other hand, the central main groove 22 on the left side of the figure has a sawtooth shape, and thus the edges of the land portions 32 and 33 divided by the central main groove 22 have a sawtooth shape. Figure 8 As shown, the middle land portion 34 divided by the central main groove 23 on the right side of the figure has a plurality of chamfered portions 342 at the edge portion on the central main groove 23 side, so that the edge portion of the middle land portion 34 has a sawtooth shape.
[0116] In contrast, Figure 3 and Figure 8 As shown, regardless of the shape of the edge of the land portions 31 to 35 on the main grooves 21 to 24 side, the stress relaxation layer 4 is formed in a linear region surrounding the entire edge of the main grooves 21 to 24 and the land portions 31 to 35 .
[0117] As mentioned above Figure 3 and Figure 8 As shown, in the structure in which the stress relaxation layer 4 is formed in the linear region, the forming process of the stress relaxation layer 4 can be facilitated. Specifically, in the above structure, the coating material of the stress relaxation layer 4 is applied to the region surrounding the predetermined position of the unvulcanized tread rubber 15, that is, the formation position of the main grooves 21 to 24, and then the vulcanization molding process is performed to form the main grooves 21 to 24. Therefore, the coating process of the coating material becomes easier than the process of coating the coating material of the stress relaxation layer on the vulcanized tread rubber.
[0118] However, the present invention is not limited thereto, and the coating material of the stress relaxation layer may also be applied to the tread rubber after vulcanization molding. Figure 8 In the embodiment, the stress relaxation layer 4 may be formed in a zigzag region along the zigzag shape of the central main groove 22 (not shown).
[0119] Fig.10 Yes means Figure 4 FIG. 4 is an explanatory diagram of a variation of the stress relaxation layer 4. Figure 4 The same components as those described above are denoted by the same reference numerals, and description thereof will be omitted.
[0120] exist Figure 4 In the structure, the stress relaxation layer 4 extends from the groove bottom of the main groove 21 to the treads of the left and right land portions 31 and 32 and covers the edge portions of the left and right land portions 31 and 32. Therefore, the left and right edge portions of the stress relaxation layer 4 are respectively located on the treads of the left and right land portions 31 and 32. Such a structure is more preferable in that the peeling of the stress relaxation layer 4 can be effectively suppressed.
[0121] In contrast, Fig.10 In the structure of , the edge of the stress relaxation layer 4 on one side extends from the groove bottom of the main groove 21 to the tread surface of the shoulder land portion 31, and the edge of the other side does not exceed the edge of the middle land portion 32 and ends on the groove wall of the main groove 21. In this case, the width WcB of the stress relaxation layer 4 on the middle land portion 32 side is 0. Even with such a structure, the effect of suppressing the peeling of the stress relaxation layer 4 can be obtained.
[0122] Fig.11 Yes means Figure 2 Explanatory diagram of a modified example of the tire 1. This diagram shows one block of the shoulder land portion 31. Fig.12 and Fig.13 Yes means Fig.11 The narrow shallow groove 7 of the shoulder land portion 31 is illustrated in these figures. Fig.12 2 is a cross-sectional view showing the tire width direction of the shoulder land portion 31. Fig.13 31 is a cross-sectional view showing the tire circumferential direction of the shoulder land portion 31. Figure 2 to Figure 4 The same components as those described above are denoted by the same reference numerals, and description thereof will be omitted.
[0123] exist Fig.11 In the structure, the land portion 31 (32-35) has a plurality of narrow shallow grooves 7 on the ground contact surface. In such a structure, when the tire contacts the ground, the narrow shallow grooves 7 absorb and remove the water film between the icy road surface and the tread surface, thereby improving the tire's braking performance on ice.
[0124] The narrow shallow groove 7 has a groove width W7 of 0.1 [mm] or more and 0.6 [mm] or less and a groove depth H7 of 0.1 [mm] or more and 0.5 [mm] or less (see Fig.13 ). Therefore, the narrow shallow groove 7 is shallower than the sipe pattern 6. In addition, the plurality of narrow shallow grooves 7 are arranged on the entire surface of the land portions 31 to 33. In addition, the plurality of narrow shallow grooves 7 are arranged in the entire area of the contact surface of the land portion 33. In addition, the plurality of narrow shallow grooves 7 are spaced apart by a pitch length P7 of 0.8 [mm] or more and 2.0 [mm] or less (refer to Fig.13 ) are configured in parallel.
[0125] The groove width W7 of the narrow shallow groove 7 is measured as the maximum value of the distance between the opposing groove walls at the groove opening on the tread surface in an unloaded state when the tire is mounted on a predetermined rim and filled with a predetermined internal pressure.
[0126] The groove depth H7 of the narrow shallow groove 7 is measured as the maximum value of the distance from the tread surface to the groove bottom in an unloaded state in which the tire is mounted on a predetermined rim and filled with a predetermined internal pressure.
[0127] The pitch length P7 of the narrow shallow grooves 7 is defined as the arrangement interval between adjacent narrow shallow grooves 7 , 7 .
[0128] For example, in Fig.11 In the structure, the narrow shallow groove 7 has a straight line shape and has an inclination angle θ7 of 40 [deg] or more and 90 [deg] or less relative to the tire circumferential direction. In addition, the narrow shallow groove 7 penetrates the land portion 31 and opens at the main groove 21. However, this is not limited to this, and the narrow shallow groove 7 may also have an arc shape or a wave shape (not shown). In addition, the narrow shallow groove 7 may also have a closed structure that does not penetrate the land portion 31 (not shown).
[0129] In addition, if Fig.12 and Fig.13 As shown, the stress relief layer 4 extends to the tread surface of the land portion 31 having the narrow shallow groove 7 and covers the edge of the land portion 31. In addition, the stress relief layer 4 is formed by entering the groove of the narrow shallow groove 7. Specifically, the coating material of the stress relief layer 4 is applied to the predetermined position of the unvulcanized tread rubber 15, that is, the formation position of the main groove 21, and then the vulcanization molding process is performed to form the main groove 21 and the narrow shallow groove 7. In such a structure, the contact area between the stress relief layer 4 and the tread rubber 15 is increased by the narrow shallow groove 7, thereby improving the adhesion of the stress relief layer 4 to the tread rubber 15. As a result, the peeling of the stress relief layer 4 is effectively suppressed.
[0130] In addition, Fig.12 and Fig.13 The thickness Gc3 of the stress relaxation layer 4 on the tread surface of the land portion 31 is preferably within the range of 0.20≤Gc3 / H7≤2.00 relative to the groove depth H7 of the narrow shallow groove 7. Thus, the adhesion of the stress relaxation layer 4 to the tread rubber 15 is ensured.
[0131] In addition, the color of the stress relaxation layer 4 is preferably the same as or similar to the color of the tread rubber 15. Specifically, the difference in brightness between the two is preferably 0.4 or less. This improves the appearance of the tire product.
[0132] Fig.14 Yes means Figure 4 FIG. 4 is an explanatory diagram of a variation of the stress relaxation layer 4. Figure 4 The same components as those described above are denoted by the same reference numerals, and description thereof will be omitted.
[0133] exist Figure 4In the structure, the outer surface of the stress relief layer 4 on the tread of the land portions 31 and 32 is flush with the exposed surface of the tread rubber 15. Therefore, on the tread of the land portions 31 and 32, the exposed surface of the tread rubber 15 and the outer surface of the stress relief layer 4 are smoothly connected without a height difference. Since the tread of the land portions 31 and 32 is flat, such a structure is more preferable from the perspective of improving the appearance of the tire. In addition, since the ground contact pressure of the tread of the land portions 31 and 32 is uniform from the time of a new tire to the initial stage of wear, the rolling resistance of the tire is reduced, and the tread of the land portions 31 and 32 can also be kept smooth after the stress relief layer 4 is worn away. As described above, the above structure is achieved by applying the coating material of the stress relief layer 4 to the area surrounding the predetermined position of the unvulcanized tread rubber 15, that is, the formation position of the main grooves 21 to 24, and then performing a vulcanization molding process to form the main grooves 21 to 24. Specifically, the stress relaxation layer 4 is formed flush with the exposed surface of the tread rubber 15 by making the conventional tire molding die have a flat shape on the tread surface of the land portions 31 , 32 .
[0134] In contrast, Fig.14 In the structure, the outer surface of the tread rubber 15, that is, the exposed surface of the tread rubber 15 and the surface in contact with the stress relief layer 4 is flat on the tread surface of the land portions 31 and 32, and the stress relief layer 4 is laminated on the surface of the flat tread rubber 15. Therefore, the stress relief layer 4 is raised relative to the exposed surface of the tread rubber 15 at the edge of the land portions 31 and 32. The above structure is formed by, for example, applying a coating material of the stress relief layer 4 to the tread rubber after vulcanization molding. Therefore, Figure 4 Compared with the structure of , the degree of freedom in construction of the stress relaxation layer 4 is higher, so the stress relaxation layer 4 can be formed on tires having various groove shapes.
[0135] Figure 4 and Fig.14 The embodiment can be appropriately selected by considering the balance of various tire performances such as groove crack resistance, wet performance, and low rolling resistance performance, as well as the physical properties of the tread rubber 15 and the combination with the tread pattern of the tire.
[0136] [Effect]
[0137] As described above, the tire 1 includes a tread rubber 15 exposed on the tread surface, main grooves 21 to 24 and land portions 31 to 35 formed on the tread surface, and a land portion 31 to 35 formed in the main grooves (in the Figure 2 In the figure, the stress relaxation layer 4 (see Figure 2In addition, the stress relief layer 4 is mainly composed of diene rubber material and non-diene rubber material, and contains carbon, a vulcanizing agent and a vulcanization accelerator. In addition, in the cross-sectional view in the tire meridian direction, the stress relief layer 4 extends continuously from the groove bottom of the main groove 21 to the land portion on at least one side (in Figure 4 The tread of the left and right land portions 31 and 32 covers the edge of the land portions 31 and 32 (see Figure 4 ). In addition, the width Wc of the stress relaxation layer 4 on the tread of the land portions 31 and 32 is within the range of 0.06≤Wc / Hg relative to the groove depth Hg (Hg1) of the main groove 21. In addition, the total width ΣWc (in Figure 3 In the shoulder land portion 31, ΣWc=WcA, and in the middle land portion 32, ΣWc=WcB) the ground contact width Wb (Wb1, Wb2) with respect to the land portions 31, 32 is in the range of ΣWc / Wb≤0.70.
[0138] In such a structure, since the stress relief layer 4 continuously extends from the groove bottom of the main groove 21 to the tread surface of the land portions 31 and 32 and covers the edge portions of the land portions 31 and 32, the bonding area of the stress relief layer 4 to the tread rubber 15 is increased compared with a structure (not shown) in which the stress relief layer 4 is formed only on the groove bottom and the groove wall. As a result, the stress relief layer 4 is prevented from peeling off when the tire rotates. In addition, the above lower limit of the Wc / Hg ratio appropriately ensures the width Wc of the stress relief layer 4 on the tread surface of the land portions 31 and 32, thereby appropriately preventing the stress relief layer 4 from peeling off. That is, the deeper the main groove 21 is, the greater the deformation amount of the main groove 21 is when the tire rotates, so the lower limit of the width Wc of the stress relief layer 4 can be optimized relative to the groove depth Hg of the main groove 21. The upper limit of the ΣWc / Wb ratio ensures the exposed area of the tread rubber 15 on the tread surface of the land portions 31 and 32, thereby ensuring the wet performance of the tire in the early stage of wear. This has the advantage of being able to achieve both the durability of the stress relaxation layer 4 and the wet performance of the tire.
[0139] In addition, in the tire 1, the modulus Mc of the stress relaxation layer 4 when it is elongated 100% at 100 [°C] is within the range of 0.45 ≤ Mc / Mt ≤ 1.15 relative to the modulus Mt of the tread rubber 15 when it is elongated 100% at 100 [°C]. By setting the above lower limit, there is an advantage that the modulus Mc of the stress relaxation layer 4 is ensured, and damage to the stress relaxation layer 4 caused by foreign matter (such as pebbles, etc.) intruding into the main groove during tire rotation is suppressed. In addition, by setting the above upper limit, there is an advantage that uneven wear of the land portion caused by excessively large modulus Mc of the stress relaxation layer 4 is suppressed.
[0140] In addition, in the tire 1, the rubber hardness Hc of the stress relaxation layer 4 is within the range of 0≤Ht-Hc≤32 relative to the rubber hardness Ht of the tread rubber 15. By setting the above lower limit, there is an advantage that the rubber hardness Hc of the stress relaxation layer 4 is ensured, and the damage of the stress relaxation layer 4 caused by foreign matter (such as pebbles, etc.) intruding into the main groove when the tire rotates is suppressed. In addition, by setting the above upper limit, there is an advantage that the partial wear of the land portion caused by the excessive rubber hardness Hc of the stress relaxation layer 4 is suppressed.
[0141] In addition, in the tire 1, the tensile strength TBc of the stress relaxation layer 4 is within the range of 0.30≤TBc / TBt≤0.90 relative to the tensile strength TBt of the tread rubber 15. By setting the above lower limit, there is an advantage of ensuring the tensile strength TBc of the stress relaxation layer 4, thereby ensuring the fracture durability of the stress relaxation layer 4 against deformation during tire rotation. In addition, by setting the above upper limit, there is an advantage of suppressing the stress relaxation layer from peeling due to excessive tensile strength TBc of the stress relaxation layer 4.
[0142] In the tire 1, the width Wc (WcA, WcB) of the stress relaxation layer 4 on the tread surface of the land portions 31, 32 is within the range of 0.02≤Wc / Wb≤0.50 with respect to the ground contact width Wb (Wb1, Wb2) of the land portions 31, 32 (see Figure 3 and Figure 4 By setting the lower limit, the width Wc of the stress relaxation layer 4 on the tread of the land portions 31 and 32 can be appropriately ensured, and by setting the upper limit, the exposed area of the tread rubber 15 on the tread of the land portions 31 and 32 can be ensured.
[0143] In the tire 1, the width Wc (WcA, WcB) of the stress relaxation layer 4 on the tread surface of the land portions 31, 32 is within the range of 2.0≤Wc / Gc1≤70 relative to the thickness Gc1 of the stress relaxation layer 4 on the groove bottom of the main groove 21 (refer to Figure 4 By setting the lower limit, the width Wc of the stress relaxation layer 4 on the tread of the land portions 31 and 32 can be appropriately ensured, and by setting the upper limit, the exposed area of the tread rubber 15 on the tread of the land portions 31 and 32 can be ensured.
[0144] In the tire 1, the thickness Gc1 of the stress relaxation layer 4 on the groove bottom of the main groove 21 (see Figure 4 ) is in the range of 0.030 [mm] ≤ Gc1 ≤ 0.400 [mm]. This has the advantage of optimizing the thickness Gc1 of the stress relaxation layer 4 and suppressing the stress relaxation layer 4 from peeling off when the tire is rotating.
[0145] In addition, in the tire 1, the minimum value Gc2_min of the thickness Gc2 (Gc2A, Gc2B) of the stress relaxation layer 4 in a predetermined region of the groove wall of the main groove 21 (defined as a region from the groove bottom of the main groove 21 to 40[%] or more and 60[%] or less of the groove depth Hg1) is thinner than the thickness Gc1 of the stress relaxation layer 4 on the groove bottom of the main groove 21 (refer to Figure 4 In such a structure, the stress relaxation layer 4 has a thin-walled portion in a predetermined region of the groove wall of the main groove 21 , thereby having an advantage of suppressing peeling of the stress relaxation layer 4 on the groove bottom of the main groove 21 .
[0146] In the tire 1, the minimum value Gc2_min of the thickness Gc2 (Gc2A, Gc2B) of the stress relaxation layer 4 on the groove wall of the main groove 21 is thinner than the thickness Gc3 of the stress relaxation layer 4 on the tread surface of the land portions 31, 32 (see Figure 4 In such a structure, since the stress relaxation layer 4 has a thin-walled portion on the groove wall of the main groove 21, it has the advantage that when the portion of the stress relaxation layer 4 exposed on the tread surface of the land portions 31 and 32 is worn away during wear, the stress relaxation layer 4 as a whole is prevented from peeling off from the groove wall of the main groove 21 to the groove bottom.
[0147] In the tire 1, the left and right groove wall angles θgA and θgB [deg] of the main groove 21 have a relationship of 2.0×(Wg+Hg)-35.0≤θgA+θgB≤4.5×(Wg+Hg)-22.5 with respect to the groove width Wg (Wg1) and the groove depth Hg of the main groove 21 (see Figure 4 ). This has the advantage of improving the adhesiveness of the stress relaxation layer 4 on the groove bottom of the main groove 21 and effectively suppressing the peeling of the stress relaxation layer 4.
[0148] In addition, in the tire 1, the smaller curvature radius Rg_min of the curvature radii RgA and RgB [mm] of the connection between the groove bottom and the left and right groove walls of the main groove 21 satisfies the following formula (1) with respect to the groove width Wg [mm], the groove depth Hg [mm], and the left and right groove wall angles θgA and θgB [deg] of the main groove 21. This has the advantage of optimizing the distribution of the thickness of the stress relaxation layer 4 on the groove bottom of the main groove 21 and effectively suppressing the peeling of the stress relaxation layer 4.
[0149] [Formula 1]
[0150]
[0151] In the tire 1, the thickness Gc1 [mm] of the stress relaxation layer 4 on the groove bottom of the main groove 21 is within the range of 0.055×e^(-0.452×UG)≤Gc1≤0.070×e^(-0.620×UG)+0.150 relative to the groove bottom thickness UG [mm] of the tread rubber 15 (refer to Figure 4 The above lower limit suppresses the peeling of the stress relaxation layer 4 when the tire rotates, and the above upper limit ensures the durability of the stress relaxation layer 4.
[0152] [Applicable objects]
[0153] In addition, in this embodiment, as described above, a pneumatic tire is described as an example of a tire. However, it is not limited to this, and the structure described in this embodiment can also be arbitrarily applied to other tires within a range that is obvious to those skilled in the art. Other tires include, for example, airless tires, solid tires, etc.
[0154] Example
[0155] Fig.15 and Fig.16 Graphs showing the results of performance tests of the tire 1 according to the embodiment of the present invention. Fig.17 It is an explanatory diagram showing a test tire of a comparative example.
[0156] In this performance test, various test tires were evaluated for (1) the durability of the stress relaxation layer and (2) the wet performance of the tire. In addition, a test tire with a tire size of 225 / 65R17 was assembled on a rim with a rim size of 17×6.5J, and an internal pressure of 230 [kPa] and a prescribed load of 6.0 [kN] were applied to the test tire.
[0157] (1) In the evaluation of the durability of the stress relaxation layer, an indoor drum tester with a drum diameter of 1707 [mm] was used to measure the travel distance before the stress relaxation layer at the bottom of the groove peeled off at a travel speed of 120 [km / h]. Then, based on the measurement results, an index evaluation was performed with the comparative example as the reference (100). The larger the numerical value of the evaluation, the more preferred it is.
[0158] (2) In the evaluation of the wet performance of tires, the test tires are mounted on all wheels of a front-wheel drive vehicle with a displacement of 2000cc. In addition, the test vehicle is driven on a wet road surface with a water depth of 2 [mm], and the braking distance from an initial speed of 80 [km / h] to a complete stop is measured. Then, based on the measurement results, an index evaluation is implemented with the comparative example as a reference (100). The larger the numerical value of the evaluation, the better the braking performance on the wet road surface, and the more preferred it is. In addition, if the evaluation is above 98, it can be considered that the wet performance is appropriately ensured.
[0159] The test tires of the embodiment were Figure 1 to Figure 5 The structure is based on the premise that the left and right shoulder main grooves 21, 24 have a stress relief layer 4, and the left and right central main grooves 22, 23 do not have a stress relief layer 4. In addition, the groove width Wg1 of the shoulder main groove 21 on the left side of the figure is Wg1 = 7.0 [mm], and the groove depth is Hg1 = 8.8 [mm]. In addition, the tire ground contact width TW is TW = 180 [mm], and the ground contact widths Wb1 and Wb2 of the shoulder land portion 31 and the middle land portion 32 on the left side of the figure are Wb1 = 32 [mm] and Wb2 = 44 [mm]. In addition, the modulus Mt of the crown tread of the tread rubber 15 when it is elongated 100% at 100 [℃] is 1.1 [MPa], the rubber hardness Ht is 52, and the tensile strength TBt is 13.5 [MPa].
[0160] The comparative test tire is the test tire of Example 1, in which the stress relaxation layer 4 is terminated at the opening of the main grooves 21, 22, and the widths WcA and WcB of the stress relaxation layer 4 on the tread surface of the land portions 31, 32 are set to 0 (see Fig.16 ).
[0161] As shown in the test results, it is understood that the test tire of the example achieves both the durability performance of the stress relaxation layer and the wet performance of the tire.
[0162] Description of Reference Numerals
[0163] 1: Tire; 11: Bead core; 12: Bead core; 13: Carcass layer; 14: Belt layer; 141, 142: Cross belt; 143: Belt cover layer; 15: Tread rubber; 16: Sidewall rubber; 17: Rim cushion rubber; 21, 24: Shoulder main groove; 22, 23: Central main groove; 31, 35: Shoulder land; 32, 34: Intermediate land; 33: Central land; 311, 321, 331, 341, 351: Transverse groove; 342: Chamfer; 4: Stress relief layer; 5: Wear indicator; 5: Pattern block; 6: Sipe pattern; 7: Narrow shallow groove
Claims
1. A tire comprising: a tread rubber exposed on a tread surface; a main groove and a land portion formed on the tread surface; and a stress relaxation layer formed on a groove bottom surface of the main groove, characterized in that: The stress relief layer is mainly composed of diene rubber material and non-diene rubber material, and contains carbon, a vulcanizing agent and a vulcanization accelerator. From the perspective of a cross-section in the meridian direction of the tire, the stress relief layer continuously extends from the groove bottom of the main groove to the tread of the land portion on at least one side and covers the edge of the land portion. The width Wc of the stress relief layer on the tread of the land portion is in the range of 0.06≤Wc / Hg relative to the groove depth Hg of the main groove, and the total width ∑Wc of the stress relief layer on the tread of one land portion is in the range of ∑Wc / Wb≤0.70 relative to the ground contact width Wb of the land portion.
2. The tire according to claim 1, wherein: A modulus Mc of the stress relaxation layer when elongated 100% at 100[°C] relative to a modulus Mt of the tread rubber when elongated 100% at 100[°C] is in the range of 0.45≤Mc / Mt≤1.
15.
3. The tire according to claim 1 or 2, wherein: The rubber hardness Hc of the stress relaxation layer is within a range of 0≤Ht−Hc≤32 relative to the rubber hardness Ht of the tread rubber.
4. The tire according to any one of claims 1 to 3, wherein: The tensile strength TBc of the stress relaxation layer relative to the tensile strength TBt of the tread rubber is in the range of 0.30≤TBc / TBt≤0.
90.
5. The tire according to any one of claims 1 to 4, wherein: A width Wc of the stress relaxation layer on the tread surface of the land portion is within a range of 0.02≤Wc / Wb≤0.50 relative to a ground contact width Wb of the land portion.
6. The tire according to any one of claims 1 to 5, wherein: A width Wc of the stress relaxation layer on the tread surface of the land portion is within a range of 2.0≤Wc / Gc1≤70 relative to a thickness Gc1 of the stress relaxation layer on the groove bottom of the main groove.
7. The tire according to any one of claims 1 to 6, wherein: The thickness Gc1 of the stress relaxation layer on the groove bottom of the main groove is in the range of 0.030 [mm] ≤ Gc1 ≤ 0.400 [mm].
8. The tire according to any one of claims 1 to 7, wherein: A minimum value Gc2_min of the thickness Gc2 of the stress relaxation layer in a predetermined region of the groove wall of the main groove is thinner than a thickness Gc1 of the stress relaxation layer on the groove bottom of the main groove.
9. The tire according to any one of claims 1 to 8, wherein: A minimum value Gc2_min of the thickness Gc2 of the stress relaxation layer in a predetermined region of the groove wall of the main groove is thinner than a thickness Gc3 of the stress relaxation layer on the tread surface of the land portion.
10. The tire according to any one of claims 1 to 9, wherein: The left and right groove wall angles θgA and θgB [deg] of the main groove have a relationship of 2.0×(Wg+Hg)-35.0≤θgA+θgB≤4.5×(Wg+Hg)-22.5 with respect to the groove width Wg [mm] and the groove depth Hg [mm] of the main groove.
11. The tire according to any one of claims 1 to 10, wherein: The minimum value Rg_min [mm] of the curvature radius RgA, RgB of the connection portion between the groove bottom and the left and right groove walls of the main groove satisfies the following conditions relative to the groove width Wg [mm], groove depth Hg [mm] and left and right groove wall angles θgA, θgB [deg] of the main groove. [Formula 1] 12. The tire according to any one of claims 1 to 11, wherein: The thickness Gc1 [mm] of the stress relaxation layer at the groove bottom of the main groove is within the range of 0.055×e^(-0.452×UG)≤Gc1≤0.070×e^(-0.620×UG)+0.150 relative to the groove bottom thickness UG [mm] of the tread rubber.