Negative electrode active material for secondary battery, method for producing same, negative electrode, and secondary battery

By using composite particles of conductive polymers and Si-containing particles in secondary batteries, the problems of low conductivity and expansion and contraction of Si-containing materials are solved, higher current collection and capacity maintenance rates are achieved, and the negative electrode is significantly suppressed. swell.

CN118872093APending Publication Date: 2024-10-29PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380023380.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-28
Filing Date
2023-02-22
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Si-containing materials in secondary batteries have low electrical conductivity and expand and contract greatly with the absorption and release of lithium ions, causing the negative electrode to expand or reduce current collection.

Method used

Composite particles containing conductive polymers and Si-containing particles are used as the negative electrode active material. Multiple Si-containing particles are connected through conductive polymers to form a good electronic conduction network, and the Si-containing particles are covered with conductive polymers to limit them. Contact with electrolyte inhibits side reactions and controls particle size distribution and sulfur content.

Benefits of technology

It significantly suppresses the expansion of the negative electrode, improves the current collection and capacity maintenance rate of the negative electrode, reduces the internal resistance and the volume of by-products, and enhances the performance stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118872093A_ABST
    Figure CN118872093A_ABST
Patent Text Reader

Abstract

A negative electrode active material for a secondary battery, the negative electrode active material containing composite particles containing a conductive polymer and Si-containing particles, in the composite particles, a plurality of Si-containing particles are connected by the conductive polymer, the particle diameter D50 of the composite particles at a cumulative volume of 50% in the volume-based particle size distribution is 100 [mu] m or less, the composite particles containing elemental sulfur, and the particle diameter D50 of the composite particles is 100 [mu] m or less. The content of elemental sulfur in the composite particles is less than 0.05 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a negative electrode active material for a secondary battery, a method for producing the negative electrode active material, a negative electrode, and a secondary battery. Background Art

[0002] It is known that silicon (Si)-containing materials can absorb a larger amount of lithium ions per unit volume than carbon materials such as graphite, and therefore, studies have been conducted on the use of Si-containing materials as negative electrode active materials for secondary batteries.

[0003] Patent document 1 proposes an organic polymer-silicon composite particle for a negative electrode active material of a lithium secondary battery, characterized in that it is an organic polymer-silicon composite particle comprising an organic polymer matrix with free space and silicon fine particles, the aforementioned organic polymer matrix with free space is any one or more selected from polypyrrole, polyaniline or polythiophene, silicon fine particles are dispersed in the aforementioned organic polymer matrix with free space, and a metal covering layer is formed on the surface of the organic polymer-silicon composite particle.

[0004] Non-Patent Document 1 proposes a negative electrode in which a conductive organic polymer and silicon fine particles are composited on a current collector.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 5712439 (Japanese Patent Publication No. 2013-522820)

[0008] Non-patent literature

[0009] Non-patent document 1: Nat. Commun. 2013, 4, 1943 Summary of the invention

[0010] Problem that the invention aims to solve

[0011] Si-containing materials have high capacity, lower conductivity than carbon materials, and large expansion and contraction with the absorption and release of lithium ions. If the Si-containing material expands, the negative electrode expands, and if the Si-containing material shrinks, the current collection of the negative electrode decreases.

[0012] Solutions for solving problems

[0013] In view of the above situation, one scheme of the present invention relates to a negative electrode active material for a secondary battery, which contains composite particles comprising a conductive polymer and Si-containing particles, wherein a plurality of the aforementioned Si-containing particles are connected by the aforementioned conductive polymer, and a particle size D50 when the cumulative volume in the volume-based particle size distribution of the aforementioned composite particles is 50% is less than 100 μm, and the aforementioned composite particles contain sulfur element, and the content of the aforementioned sulfur element in the aforementioned composite particles is less than 0.05 mass %.

[0014] Another aspect of the present invention relates to a negative electrode for a secondary battery, comprising the negative electrode active material for a secondary battery.

[0015] Still another aspect of the present invention relates to a secondary battery comprising a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the negative electrode is the negative electrode for the secondary battery described above.

[0016] Another aspect of the present invention relates to a method for producing a negative electrode active material for a secondary battery, which comprises the following steps: a first step of mixing a monomer as a raw material of a conductive polymer, a polymerization initiator containing sulfur element, and Si-containing particles, and polymerizing the aforementioned monomer to synthesize a composite, wherein the aforementioned composite comprises a conductive polymer and Si-containing particles, and a plurality of the aforementioned Si-containing particles are connected by the aforementioned conductive polymer; a second step of crushing the aforementioned composite to obtain composite particles having a particle size D50 of less than 100 μm when the cumulative volume in the volume-based particle size distribution is 50%; and a third step of washing the aforementioned composite particles until the content of the aforementioned sulfur element in the aforementioned composite particles is less than 0.05% by mass.

[0017] Effects of the Invention

[0018] According to the present invention, expansion of a negative electrode for a secondary battery including Si-containing particles can be suppressed.

[0019] The novel features of the present invention are described in the appended claims, but the present invention, both about the configuration and content, together with other objects and features of the present invention, should be further fully understood from the following detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a longitudinal cross-sectional view showing the structure of a secondary battery according to one embodiment of the present invention. DETAILED DESCRIPTION

[0021] Hereinafter, the embodiments of the present disclosure will be described with examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values, materials, etc. are sometimes exemplified, but other numerical values, materials, etc. may also be applied as long as the effects of the present disclosure can be obtained. It should be noted that the constituent elements other than the characteristic parts of the present disclosure may also apply the constituent elements of known secondary batteries. In this specification, in the case of "a range of numerical value A to numerical value B", the range includes numerical value A and numerical value B. In addition, the present disclosure includes a combination of matters recorded in two or more claims arbitrarily selected from a plurality of claims recorded in the attached claims. That is, as long as no technical contradiction arises, matters recorded in two or more claims arbitrarily selected from a plurality of claims recorded in the attached claims can be combined.

[0022] <Negative electrode active material>

[0023] The negative electrode active material for secondary battery of the present embodiment comprises composite particles, each of which comprises a conductive polymer and Si-containing particles. The negative electrode active material may also comprise materials other than composite particles. As materials other than composite particles, carbon materials, Si-containing materials, Sn-containing materials, etc. may be listed. The negative electrode active material may be used alone or in combination of two or more.

[0024] <Compound particles>

[0025] Composite particles are particles containing conductive polymers and Si-containing particles. The particle shape of the composite particles is not particularly limited. In the composite particles, multiple Si-containing particles are connected by conductive polymers. In other words, it can be said that multiple Si-containing particles are dispersed in the matrix of the conductive polymer. In the composite particles, for example, at least a portion of the surface of each Si-containing particle is covered with a conductive polymer, and such Si-containing particles are aggregated together with the conductive polymer to form composite particles.

[0026] The content of the composite particles in the negative electrode active material is not particularly limited and may be 100%, 5% to 50% by mass, or 5% to 30% by mass from the viewpoint of more significantly suppressing negative electrode expansion while ensuring high capacity.

[0027] The composite particles have the following properties.

[0028] First, the composite particles contain Si-containing particles, so they have high capacity, which significantly increases the capacity of the negative electrode active material or the negative electrode. In particular, when nano-silicon particles are used as Si-containing particles, the nano-silicon particles are substantially 100% (at least 90% by mass) formed by silicon alone, so composite particles with higher capacity can be obtained. It should be noted that the conductive polymer can also show capacity based on Faraday reaction or non-Faraday reaction.

[0029] Second, multiple Si-containing particles are connected by conductive polymers, thereby forming a good electronic conduction network in each composite particle, thereby improving the conductivity of the composite particles. In order to form a better electronic conduction network, it is desirable to improve the conductivity of the conductive polymer. For example, the conductivity can be significantly improved by doping the conductive polymer with a dopant.

[0030] Third, the composite particles have a free volume derived from the conductive polymer. Free volume refers to the volume of the space of the pores usually formed in the conductive polymer region. The free volume absorbs the volume change of the Si-containing particles accompanying the absorption and release of lithium ions, or the stress caused by the volume change. Therefore, the expansion of the negative electrode caused by repeated charge and discharge is suppressed, and it is easy to maintain the current collection of the negative electrode and maintain the capacity.

[0031] Fourth, by covering the Si-containing particles with a conductive polymer, the contact between the Si-containing particles and the electrolyte is appropriately limited, and the side reaction is suppressed. By suppressing the side reaction, the capacity retention rate can be maintained at a high level, and the expansion suppression effect of the negative electrode is improved by reducing the volume of the byproducts.

[0032] The content of Si-containing particles in the composite particles is, for example, 30% by mass or more, 50% by mass or more, 55% by mass or more, or 60% by mass or more. The higher the content of Si-containing particles in the composite particles, the higher the capacity of the negative electrode can be obtained. From the viewpoint of improving the effect of suppressing the expansion of the negative electrode, it is desirable that the content of Si-containing particles in the composite particles is not too high, and may be 90% by mass or less, or 80% by mass or less.

[0033] The remainder of the composite particles other than the Si-containing particles is mostly the conductive polymer, and 90 mass % to 100 mass % of the remainder may be the conductive polymer.

[0034] Since the composite particles contain conductive polymers, the powder resistivity thereof is lower than that of the composite particles containing non-conductive polymers, for example, 10 3 Ω·cm~10 7 Ω·cm. When the composite particles have such a volume resistivity, the internal resistance of the negative electrode is reduced, and the interface resistance between the negative electrode mixture layer and the current collector described later is also reduced. As a result, the current collection of the negative electrode can be maintained at a higher level, and the capacity can also be easily maintained at a higher level.

[0035] For the powder resistivity, at 204Kgf / cm 2The composite particles are measured by a four-probe method under pressure using a powder resistivity measuring apparatus (for example, Loresta SP manufactured by Mitsubishi Chemical Analytech Co., Ltd. (currently Nittoseiko Analytech Co., Ltd.)).

[0036] The particle size D50 (hereinafter referred to as "average particle size") when the cumulative volume in the volume-based particle size distribution of the composite particles is 50% can be, for example, 100 μm or less, 50 μm or less, or 30 μm or less. By having such an upper limit, the average particle size of the composite particles becomes less likely to cause local volume changes and stress concentration of Si-containing particles, or it is easier to maintain current collection. In addition, if the particle form is such, it is easy to control the content of sulfur in the composite particles to less than 0.05 mass%.

[0037] On the other hand, the average particle size of the composite particles can be, for example, 1 μm or more, 10 μm or more, or 20 μm or more. By having such a lower limit on the average particle size of the composite particles, the surface area of ​​the Si-containing particles will not be excessively increased, and the side reactions can be effectively suppressed and high capacity can be easily ensured.

[0038] The volume-based particle size distribution of the composite particles can be measured by a laser diffraction / scattering method using a particle size distribution measuring apparatus (eg, MT3000II manufactured by MICROTRAC Co., Ltd.) The measurement uses a dispersion obtained by dispersing the composite particles in pure water.

[0039] The particle size D10 at 10% cumulative volume in the volume-based particle size distribution of the composite particles may be 0.5 μm or more (eg, 0.5 μm to 50 μm). In this case, the proportion of micro-sized composite particles is small, side reactions are effectively suppressed, and high capacity is easily ensured.

[0040] The particle size D90 at 90% of the cumulative volume in the volume-based particle size distribution of the composite particles can also be 500 μm or less (e.g., 50 μm to 500 μm or 100 μm to 300 μm). In this case, the proportion of oversized composite particles is small, local volume changes and stress concentration are less likely to occur, and it is easier to maintain current collection.

[0041] <Conductive polymer>

[0042] The conductive polymer refers to an organic polymer that exhibits conductivity alone or by being doped with a dopant. Representative examples of the conductive polymer include π-conjugated polymers.

[0043] As π-conjugated polymers, for example, polymers with basic skeletons such as polypyrrole, polythiophene, polyaniline, polyfuran, polyacetylene, polyphenylene, polyphenylene vinylene, polyphenylene, polythiophene vinylene, etc. can be listed. These polymers also include homopolymers, copolymers of more than two monomers, and their derivatives (substitutes with substituents, etc.). For example, polyaniline includes poly (N-methylaniline) in which at least a portion of amino groups is substituted by methyl. In addition, polythiophene includes poly (3,4-ethylenedioxythiophene) and the like. However, these are only specific examples, and conductive polymers are not limited to these specific examples.

[0044] The conductive polymer may be doped with a dopant. By doping with the dopant, the conductivity of the conductive polymer becomes higher, the powder resistivity of the composite particles becomes lower, and it is easier to maintain the current collection. The dopant, for example, gives protons to the conductive polymer to generate anions. By attaching the protonated anions to the conductive polymer, the conductive polymer stably exhibits conductivity.

[0045] The content of the dopant in the composite particles is not particularly limited, and may be, for example, 0.1% by mass to 10% by mass, or 1% by mass to 5% by mass.

[0046] The dopant can be appropriately selected according to the type of the conductive polymer. The dopant may have, for example, an oxyacid group capable of releasing protons. The dopant may also be an oxyacid, an oxyacid ester, etc. capable of releasing protons. It may also be in the form of their ions (anions).

[0047] Examples of the ionic dopant include sulfate ions, nitrate ions, phosphate ions, borate ions, and halide ions (F - , Cl - Br - ,I - ), benzenesulfonate ion, naphthalenesulfonate ion, toluenesulfonate ion, methanesulfonate ion (CF3SO3 - ), perchlorate ion (ClO4 - ), tetrafluoroborate ion (BF4 - ), hexafluorophosphate ion (PF6 - ), fluorosulfate ion (FSO3 - ), bis(fluorosulfonyl)imide ion (N(FSO2)2 - ), bis(trifluoromethanesulfonyl)imide ion (N(CF3SO2)2 - ) etc. These may be used alone or in combination of two or more.

[0048] The dopant may also be a macromolecule. Examples of the macromolecule include polyvinyl sulfonic acid, polystyrene sulfonic acid, polyallyl sulfonic acid, polyacrylic acid sulfonic acid, polymethacrylic acid sulfonic acid, poly(2-acrylamide-2-methylpropane sulfonic acid), polyisoprene sulfonic acid, and polyacrylic acid. These may be homopolymers or copolymers of two or more monomers. They may also be in their ionic (anionic) state. These may be used alone or in combination of two or more.

[0049] The dopant may include phosphorus. More specifically, the dopant may include phosphoric acid, phosphonic acid, phosphoric acid ester, phosphonic acid ester, etc. When the conductive polymer includes phosphorus, it can be determined that the dopant including phosphorus is included in the conductive polymer.

[0050] Phosphate, for example, may also be phytic acid (inositol hexaphosphate). In particular, when the conductive polymer includes polyaniline, it is desirable to use phytic acid having affinity for both Si-containing particles and polyaniline as a dopant. Phytic acid acts as a dopant for the protons of the conductive polymer and hydrogen bonds with the hydroxyl groups on the Si surface. Therefore, the Si-containing particles are easily and uniformly covered by the conductive polymer.

[0051] <Polyaniline>

[0052] Polyaniline is a conductive polymer with aniline (C6H5-NH2) as a monomer. Polyaniline includes polyaniline and its derivatives as described above. For example, derivatives with alkyl groups such as methyl added to at least a portion of the benzene ring, derivatives with halogen groups etc. added to at least a portion of the benzene ring, derivatives with alkyl groups such as methyl added to at least a portion of the amino group, etc., as long as they are conductive polymers with aniline as the basic skeleton, they are also included in polyaniline in the present invention.

[0053] The structure of polyaniline includes structural units that can form a benzene (ring) type skeleton (-C6H4-NH-) (also called IP structure) and structural units that can form a quinone type skeleton (-C6H4=N-) (also called NP structure).

[0054] <Si-containing particles>

[0055] The Si-containing particles refer to a granular Si-containing material, and the particle shape is not particularly limited. Examples of the Si-containing material include Si simple substance, silicon alloy, and silicon compound.

[0056] As Si-containing particles, particles containing a lithium ion conductive phase and a silicon phase dispersed in the lithium ion conductive phase may be used. As the lithium ion conductive phase, SiO2 phase, silicate phase (eg, lithium silicate phase), carbon phase, etc. may be used.

[0057] The particles comprising SiO2 phase and silicon phase dispersed in the SiO2 phase can be made of SiO x (0.5≤x<2 (for example, 0.5≤x<1.6)). The silicon phase dispersed in the SiO2 phase is fine. In the particles containing the lithium silicate phase and the silicon phase dispersed in the lithium silicate phase, the lithium silicate phase can be represented by Li 2z SiO 2+z (0<z<1(for example, z=1 / 2)) represents.

[0058] The average particle size of the Si-containing particles is, for example, 10 nm to 500 nm, and can be 30 nm to 50 nm. Nano silicon particles having such an average particle size can also be used. Nano silicon particles are easy to obtain. When the average particle size of the Si-containing particles is within the above range, it is easy to synthesize composite particles of appropriate size, and the volume change of the composite particles is more significantly suppressed.

[0059] The average particle size of the Si-containing particles is preferably measured before the initial charge and discharge, but can also be measured after the battery is assembled and after multiple charge and discharge. In this case, it is desirable to use Si-containing particles collected from the negative electrode of a fully discharged battery for measurement.

[0060] It should be noted that the amount of charge when charging a battery in a fully discharged state (Depth of Discharge: DOD = 100%) to a fully charged state (State of Charge: SOC = 100%, DOD = 0%) is equivalent to the rated capacity of the battery. The voltage of a fully charged battery corresponds to the charge termination voltage. The voltage of a fully discharged battery corresponds to the discharge termination voltage.

[0061] The average particle size of the Si-containing particles is measured by observing a cross section of the negative electrode using a SEM or a TEM. Specifically, the average maximum diameter of any 100 Si-containing particles is calculated.

[0062] At least a portion of the surface of the Si-containing particles can be covered with a conductive carbon material. In this case, the conductivity of the Si-containing particles is improved, and it is easier to maintain the current collection of the negative electrode and the capacity. For example, the Si-containing particles are mixed with a raw material of a carbon material (asphalt, tar, carbon black, etc.), calcined at a predetermined temperature, and at least a portion of the surface of the Si-containing particles is covered with a conductive carbon material.

[0063] <Sulfur>

[0064] The composite particles may contain elemental sulfur. The elemental sulfur may be derived from an oxidizing agent used as an initiator when polymerizing the conductive polymer.

[0065] As for the sulfur element, due to the concern that harmful sulfur-based gases may be generated by decomposition during charge and discharge, it is desirable that the sulfur element content in the composite particles is low. For example, it is desirable to be less than 0.05% by mass, and it may also be less than 0.01% by mass. On the other hand, a trace amount of sulfonic acid groups can be expected to promote the dissociation of lithium salts contained in the electrolyte in the conductive polymer region and improve the lithium ion conductivity. From the viewpoint of obtaining such an effect, it is desirable that the sulfur element content in the composite particles is 0.001% by mass or more.

[0066] The content of sulfur in the composite particles can be measured, for example, by inductively coupled plasma atomic emission spectrometry (ICP-AES). Specifically, a sample of the composite particles is dissolved in a heated acid solution (a mixed acid of hydrofluoric acid, nitric acid, and sulfuric acid) to fully extract the sulfur element, and the solution residue is filtered and removed. Then, the filtrate obtained is analyzed by ICP-AES to measure the spectral intensity of sulfur. Next, a standard curve is prepared using a commercially available standard solution of sulfur element, and the sulfur content is calculated.

[0067] <Nitrogen>

[0068] The composite particles may further contain nitrogen. The nitrogen may be derived from an oxidant used as an initiator when the conductive polymer is polymerized. The sulfur and nitrogen may be derived from, for example, ammonium persulfate. Ammonium persulfate is suitable as a polymerization initiator when aniline is polymerized to generate polyaniline.

[0069] <Preferred method>

[0070] As a preferred embodiment of the composite particles, the conductive polymer is polyaniline and the dopant is phytic acid. When ammonium persulfate is used to synthesize polyaniline, the composite particles may contain sulfur. When the content of sulfur in the composite particles is controlled within a desired range, it is desirable to perform a predetermined washing step.

[0071] <Method for producing composite particles>

[0072] The method for producing composite particles contained in a negative electrode active material for a secondary battery includes, for example, the following first to third steps.

[0073] (i) Step 1

[0074] The first step is a step of preparing a polymerization solution and synthesizing a composite. The polymerization solution is prepared by mixing a monomer as a raw material of a conductive polymer, a polymerization initiator containing sulfur, Si-containing particles, and a dopant. As a conductive polymer, for example, in the case of synthesizing polyaniline, aniline is used as a monomer. As a polymerization initiator containing sulfur, a peroxide is preferably used, for example, ammonium persulfate is used. As Si-containing particles, for example, nanoparticles with an average particle size of 10nm to 500nm are used.

[0075] If the initiator is dissolved in the polymerization solution, the polymerization of the monomer proceeds to generate a conductive polymer. At this time, the conductive polymer grows in a manner that covers at least a portion of the surface of the Si-containing particles. As a result, a composite structure including the conductive polymer and the Si-containing particles, and a plurality of Si-containing particles connected via the conductive polymer, can be obtained.

[0076] (ii) Second step

[0077] The second step is to pulverize the composite. A pulverizer such as a mixer, a kneader, or a mortar can be used for pulverization. By pulverizing, composite particles of a desired size, for example, a particle size D50 (average particle size) of 100 μm or less when the cumulative volume in the volume-based particle size distribution is 50% are generated. This can significantly improve the cleaning effect in the subsequent cleaning step.

[0078] (iii) Step 3

[0079] The third step is a step of washing the composite particles. It is desirable to wash until the content of sulfur in the composite particles is less than 0.05% by mass. Washing is not particularly limited, and water washing may be performed. The sulfur element originates from a polymerization initiator containing sulfur. When a large amount of residue of the polymerization initiator remains in the composite particles, side reactions are induced in the battery, so there is a tendency for the battery performance to decrease, and there is also a concern that harmful sulfur-based gases are generated as a result of decomposition. On the other hand, by reducing the content of sulfur in the composite particles to less than 0.05% by mass by washing, such disadvantages can be prevented.

[0080] Before the composite is pulverized, the composite may be washed. In this case, washing of the composite particles after pulverization may be omitted, but it is desirable to repeatedly wash the composite particles after pulverization.

[0081] <Negative electrode>

[0082] The negative electrode comprises a negative electrode mixture layer containing a negative electrode active material and a negative electrode current collector. The negative electrode mixture layer can be formed by applying a negative electrode slurry formed by dispersing the constituent components of the negative electrode mixture in a dispersion medium to the surface of the negative electrode current collector and drying it. The dried coating film can also be rolled as needed.

[0083] The negative electrode mixture may include a negative electrode active material as an essential component and a binder, a thickener, a conductive agent, etc. as an optional component. The negative electrode active material may also include the composite particles described above and materials other than the composite particles. The negative electrode active material may include, for example, carbon materials such as graphite, easily graphitizable carbon (soft carbon), and non-graphitizable carbon (hard carbon).

[0084] As the binder of the negative electrode, for example, a resin material is used. As the binder, for example, fluororesins, polyolefin resins, polyamide resins, polyimide resins, acrylic resins, vinyl resins, rubber-like materials (such as styrene butadiene copolymer (SBR)) and the like can be listed. The binder can be used alone or in combination of two or more.

[0085] Examples of the thickener include cellulose derivatives such as cellulose ethers, and examples of the cellulose derivative include carboxymethyl cellulose (CMC) and modified forms thereof, and methyl cellulose. The thickener may be used alone or in combination of two or more.

[0086] Examples of the conductive material include carbon nanotubes (CNTs), carbon fibers other than CNTs, and conductive particles (eg, carbon black and graphite).

[0087] The dispersion medium used in the negative electrode slurry is not particularly limited, and examples thereof include water, alcohol, N-methyl-2-pyrrolidone (NMP), and mixed solvents thereof.

[0088] As the negative electrode current collector, for example, a metal foil can be used. The negative electrode current collector can also be porous. As the material of the negative electrode current collector, for example, stainless steel, nickel, nickel alloy, copper, copper alloy, etc. can be exemplified. The thickness of the negative electrode current collector is not particularly limited, for example, 1 to 50 μm, and can be 5 to 30 μm.

[0089] <Positive electrode>

[0090] The positive electrode contains a positive electrode active material. The positive electrode usually has a positive electrode collector and a layered positive electrode mixture (hereinafter referred to as a "positive electrode mixture layer") maintained on the positive electrode collector. The positive electrode mixture layer can be formed by applying a positive electrode slurry formed by dispersing the constituent components of the positive electrode mixture in a dispersion medium to the surface of the positive electrode collector and drying it. The dried coating film can also be rolled as needed. The positive electrode mixture can contain a positive electrode active material as an essential component and contain a binder, a thickener, etc. as an optional component.

[0091] The positive electrode active material can be any material that can be used as a positive electrode active material for a non-aqueous electrolyte secondary battery (particularly a lithium ion secondary battery), but from the viewpoint of high capacity, at least a lithium transition metal composite oxide (composite oxide N) containing nickel as a transition metal is included. The proportion of the composite oxide N in the positive electrode active material is, for example, 70% by mass or more, 90% by mass or more, or 95% by mass or more.

[0092] The composite oxide N can be, for example, a lithium transition metal composite oxide having a layered rock salt structure and comprising Ni and at least one selected from the group consisting of Co, Mn and Al. Hereinafter, a lithium transition metal composite oxide having a layered rock salt structure and comprising Ni, and at least one selected from the group consisting of Co, Mn and Al, wherein the proportion of Ni in the metal elements other than Li is 80 atomic % or more is also referred to as "composite oxide HN". The proportion of composite oxide HN in composite oxide N used as a positive electrode active material is, for example, 90 mass % or more, 95 mass % or more, or 100%. The higher the proportion of Ni, the more lithium ions can be taken out of the composite oxide HN during charging, and the more the capacity can be improved. Co, Mn and Al contribute to the stabilization of the crystal structure of composite oxide HN with a high Ni content.

[0093] The composite oxide HN is, for example, of the formula: Li α Ni (1-x1-x2-y-z) Co x1 Mn x2 Al y M z O 2+β Element M is an element other than Li, Ni, Co, Mn, Al and oxygen. Mn contributes to stabilization of the crystal structure of the composite oxide HN, and the composite oxide HN contains inexpensive Mn, which is advantageous for cost reduction. Al contributes to stabilization of the crystal structure of the composite oxide HN.

[0094] In the above formula, α, which represents the atomic ratio of lithium, is, for example, 0.95≤α≤1.05. α increases and decreases by charge and discharge. In (2+β), which represents the atomic ratio of oxygen, β satisfies -0.05≤β≤0.05.

[0095] 1-x1-x2-yz (=v) representing the atomic ratio of Ni is, for example, greater than 0.8, greater than 0.85, greater than 0.90, or greater than 0.95. In addition, v may be less than 0.98, or less than 0.95. x1 representing the atomic ratio of Co is, for example, less than 0.1 (0≤x1≤0.1), x2 representing the atomic ratio of Mn is, for example, less than 0.1 (0≤x2≤0.1), y representing the atomic ratio of Al is, for example, less than 0.1 (0≤y≤0.1), and z representing the atomic ratio of element M is, for example, 0≤z≤0.10.

[0096] The element M may be at least one selected from the group consisting of Ti, Zr, Nb, Mo, W, Fe, Zn, B, Si, Mg, Ca, Sr, Sc and Y. When at least one selected from the group consisting of Nb, Sr and Ca is contained in the composite oxide HN, it is believed that the surface structure of the composite oxide HN is stabilized, the resistance is reduced, and the dissolution of the metal is further suppressed. It is more effective when the element M is unevenly present near the particle surface of the composite oxide HN.

[0097] As the binder of the positive electrode, for example, a resin material is used. As the binder, for example, fluororesins, polyolefin resins, polyamide resins, polyimide resins, acrylic resins, vinyl resins, etc. can be listed. The binder can be used alone or in combination of two or more.

[0098] Examples of the conductive material include carbon nanotubes (CNTs), carbon fibers other than CNTs, and conductive particles (eg, carbon black and graphite).

[0099] The dispersion medium used in the positive electrode slurry is not particularly limited, and examples thereof include water, alcohol, N-methyl-2-pyrrolidone (NMP), and mixed solvents thereof.

[0100] As the positive electrode current collector, for example, a metal foil can be used. The positive electrode current collector can also be porous. As the porous current collector, for example, a mesh, a punched sheet, a porous metal mesh, etc. can be listed. As the material of the positive electrode current collector, for example, stainless steel, aluminum, aluminum alloy, titanium, etc. can be exemplified. The thickness of the positive electrode current collector is not particularly limited, for example, it is 1 to 50 μm, and can be 5 to 30 μm.

[0101] <Electrolyte>

[0102] The electrolyte may be a liquid electrolyte (electrolyte), a gel electrolyte, or a solid electrolyte. The gel electrolyte comprises a lithium salt and a matrix polymer, or comprises a lithium salt, a non-aqueous solvent, and a matrix polymer. As the matrix polymer, for example, a polymer material that absorbs a non-aqueous solvent and gels is used. As polymer materials, fluororesins, acrylic resins, polyether resins, polyethylene oxides, etc. may be cited. The solid electrolyte may be an inorganic solid electrolyte. As an inorganic solid electrolyte, for example, a well-known material in an all-solid lithium ion secondary battery (for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a halide-based solid electrolyte, etc.) is used.

[0103] For example, a liquid electrolyte (electrolyte) includes a solvent and a solute dissolved in the solvent. The solute is an electrolyte salt that undergoes ion dissociation in the electrolyte. The solute may include, for example, a lithium salt. The components of the electrolyte other than the solvent and the solute are additives. Various additives may be included in the electrolyte.

[0104] The solvent uses an aqueous solvent or a non-aqueous solvent. As the non-aqueous solvent, for example, cyclic carbonates, chain carbonates, cyclic carboxylates, chain carboxylates, etc. are used. As cyclic carbonates, propylene carbonate (PC), ethylene carbonate (EC), vinylene carbonate (VC), etc. can be listed. As chain carbonates, diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), etc. can be listed. In addition, as cyclic carboxylates, γ-butyrolactone (GBL), γ-valerolactone (GVL), etc. can be listed. As chain carboxylates, methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), ethyl propionate (EP), etc. can be listed. The non-aqueous solvent can be used alone or in combination of two or more.

[0105] As the lithium salt, for example, a lithium salt containing chloric acid (LiClO4, LiAlCl4, LiB 10 Cl 10 etc.), lithium salts of fluorinated acids (LiPF6, LiPF2O2, LiBF4, LiSbF6, LiAsF6, LiCF3SO3, LiCF3CO2, etc.), lithium salts of fluorinated imides (LiN(FSO2)2, LiN(CF3SO2)2, LiN(CF3SO2)(C4F9SO2), LiN(C2F5SO2)2, etc.), lithium halides (LiCl, LiBr, LiI, etc.), etc. The lithium salts may be used alone or in combination of two or more.

[0106] The concentration of the lithium salt in the electrolyte may be 1 mol / liter or more and 2 mol / liter or less, or 1 mol / liter or more and 1.5 mol / liter or less. However, the concentration of the lithium salt is not limited to the above.

[0107] <Separator>

[0108] It is desirable to sandwich a separator between the positive electrode and the negative electrode. The separator has high ion permeability and has appropriate mechanical strength and insulation. As the separator, a microporous film, a woven fabric, a non-woven fabric, etc. can be used. As the material of the separator, polyolefins such as polypropylene and polyethylene are preferred.

[0109] <Secondary battery>

[0110] As an example of the structure of a secondary battery, an electrode group formed by winding a positive electrode and a negative electrode with a separator and being contained in an outer shell together with an electrolyte can be cited. However, it is not limited to this, and electrode groups of other forms can also be applied. For example, it can also be a stacked electrode group obtained by stacking a positive electrode and a negative electrode with a separator. The form of the secondary battery is also not limited, for example, it can be a cylindrical, square, coin-shaped, button-shaped, laminated type, etc. Secondary batteries include lithium-ion secondary batteries containing electrolytes, non-aqueous electrolyte secondary batteries such as solid batteries containing gel electrolytes or solid electrolytes.

[0111] Below, refer to Figure 1 The structure of the secondary battery will be described. Figure 1 1 is a longitudinal cross-sectional view of a cylindrical secondary battery 10 as an example of the present embodiment. However, the present disclosure is not limited to the following configuration.

[0112] The secondary battery 10 includes: an electrode group 18, an electrolyte (not shown), and a bottomed cylindrical battery can 22 that accommodates these. The sealing body 11 is tightly fixed to the opening of the battery can 22 by means of a gasket 21. As a result, the interior of the battery is sealed. The sealing body 11 includes: a valve body 12, a metal plate 13, and an annular insulating member 14 sandwiched between the valve body 12 and the metal plate 13. The valve body 12 and the metal plate 13 are connected to each other at their respective center parts. The positive electrode lead 15a derived from the positive electrode 15 is connected to the metal plate 13. As a result, the valve body 12 functions as an external terminal of the positive electrode. The negative electrode lead 16a derived from the negative electrode plate 16 is connected to the bottom inner surface of the battery can 22. An annular groove 22a is formed near the open end of the battery can 22. A first insulating plate 23 is arranged between one end surface of the electrode group 18 and the annular groove 22a. A second insulating plate 24 is disposed between the other end surface of the electrode group 18 and the bottom of the battery can 22. The electrode group 18 is formed by winding the positive electrode 15 and the negative electrode 16 with the separator 17 interposed therebetween.

[0113] The present disclosure will be specifically described below based on Examples and Comparative Examples, but the present disclosure is not limited to the following Examples.

[0114] 《Example 1》

[0115] [Synthesis of composite particles]

[0116] 2 g of nano silicon particles (average particle size 40 nm) were dispersed in 60 mL of aqueous solution A containing 100 mM aniline and 30 mM phytic acid. Next, 20 mL of aqueous solution B containing 125 mM ammonium persulfate was injected into the aqueous solution A containing the nano silicon particles, and the mixture was stirred at room temperature for 3 days to polymerize the aniline, thereby obtaining a composite A1.

[0117] After the composite A1 is separated by suction filtration, it is thoroughly washed with distilled water. The washed composite is vacuum dried at 60°C. After the dried composite A1 is crushed in a mortar, it is passed through a sieve with a mesh size of 75 μm. The crushed composite A1 (composite particles A1) is put into 500 mL of pure water and washed with water for 5 hours while stirring. Then, the composite particles A1 are separated by suction filtration and vacuum dried at 60°C.

[0118] (Particle size distribution)

[0119] The volume-based particle size distribution of the composite particles was measured by a laser diffraction scattering method. The composite particles A1 had a D50 of 29 μm, a D10 of 1.9 μm, and a D90 of 122 μm.

[0120] (ICP-AES analysis)

[0121] The content of silicon nanoparticles in composite particle A1 was measured by ICP-AES and found to be 67% by mass. The conductive polymer was estimated to be about 33% by mass. The content of sulfur element derived from ammonium persulfate in composite particle A1 was measured by ICP-AES and found to be 0.03% by mass.

[0122] (Volume resistivity)

[0123] At 204Kgf / cm 2 The volume resistivity of the composite particles A1 was measured by a four-probe method using a powder resistivity measuring device (Loresta SP manufactured by Nittoseiko Analytech Co., Ltd.) under pressure, and the result was 1.6×10 6 Ω·cm.

[0124] (FT-IR analysis)

[0125] FT-IR analysis of the conductive polymer (polyaniline) in the composite particles A1 confirmed the absorption of stretching and vibration attributable to the quinone structure due to proton doping, as well as the absorption attributable to the stretching of the aromatic ring and the absorption attributable to the stretching of NH.

[0126] [Production of negative electrode]

[0127] Composite particles A1, sodium salt of carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber (SBR), polyacrylic acid (PAA), and single-layer carbon nanotubes (SWCNT) were mixed in a mass ratio of composite particles A1: CMC-Na: SBR: PAA: SWCNT = 100: 5: 5: 0.5, water was added, and a mixer (manufactured by PRIMIX Corporation, TKHIVIS MIX) was used to stir and prepare a negative electrode slurry. Next, the negative electrode slurry was applied to one side of a copper foil (negative electrode collector), and after the coating was dried, it was rolled to obtain a single-sided copper foil having a density of 0.7 g / cm 3 It should be noted that the thickness TA1 was measured at 5 locations on the negative electrode mixture layer. 0-1 ~TA1 0-5 .

[0128] The negative electrode was cut into a 20 mm × 20 mm shape with a 5 mm × 5 mm protrusion, and the negative electrode mixture layer of the protrusion was peeled off to expose the copper foil. Then, the negative electrode tab lead was connected to the exposed part of the negative electrode current collector, and a predetermined area around the negative electrode tab lead was covered with an insulating film.

[0129] (Resistance of composite layer)

[0130] The volume resistivity of the negative electrode mixture layer was measured using an electrode resistance measurement system (RM2610 manufactured by Hioki Electric Co., Ltd.) and found to be 8.3 Ω·cm.

[0131] (Interface resistance)

[0132] The interface resistance was measured by an electrode resistance measurement system (RM2610 manufactured by Hioki Electric Co., Ltd.) and the result was 0.35 Ω·cm 2 .

[0133] [Fabrication of Counter Electrode]

[0134] A counter electrode was prepared by attaching a lithium metal foil having a thickness of 300 μm to one surface of a copper foil.

[0135] The counter electrode is cut into the same shape as the negative electrode, and the lithium metal foil of the protruding part is peeled off to expose the copper foil. Then, the counter electrode tab lead is connected to the exposed part of the copper foil in the same way as the negative electrode, and a predetermined area around the counter electrode tab lead is covered with an insulating film.

[0136] [Preparation of non-aqueous electrolyte]

[0137] A non-aqueous electrolyte was prepared by adding 1.3 mol / L of lithium hexafluorophosphate (LiPF6) to a mixed solvent obtained by mixing ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a volume ratio of EC:EMC:DMC=4:1:15.

[0138] [Production of Evaluation Battery Cells]

[0139] A battery cell with a designed capacity of 25 mAh of negative electrode regulation was manufactured using the above-mentioned negative electrode and counter electrode. The negative electrode and counter electrode were placed opposite each other in a manner that the negative electrode mixture layer overlapped with the lithium metal foil through two polyethylene separators (thickness 15 μm) with an aramid coating to form a plate assembly. Next, the Al laminate film (thickness 100 μm) cut into a rectangular shape was folded in half, and the ends of the long sides were heat-sealed to form a tube. Then, the manufactured plate assembly was placed into the tube from one side of the short side, and the end face of the Al laminate film was heat-sealed together with the position of the insulating film of each tab lead. Next, 0.3 cm of non-aqueous electrolyte was injected from the short side of the tube that was not heat-sealed. 3 After the injection, the battery was left to stand for 3 minutes under a reduced pressure of 0.02 MPa, and then returned to atmospheric pressure. This operation was repeated twice to impregnate the negative electrode mixture layer with the non-aqueous electrolyte. Finally, the end face of the Al laminate film on the injection side was heat-sealed to obtain the evaluation battery cell A1. The evaluation battery cell was made in a dry air atmosphere with a dew point below -60°C.

[0140] [evaluate]

[0141] The battery cell for evaluation was clamped by a pair of 10×5 cm stainless steel (thickness 6 mm) clamps and fixed under pressure at 1 MPa.

[0142] <First cycle>

[0143] In a thermostatic chamber at 25°C, the negative electrode was charged with lithium at a constant current of 0.1C (1C is the current value for discharging the designed capacity within 1 hour) until the cell voltage reached 0.005V, and then paused for 20 minutes. Next, the negative electrode was charged with lithium at a constant current of 0.01C until the cell voltage reached 0.005V, and then paused for 20 minutes. Furthermore, the negative electrode was charged with lithium at a constant current of 0.001C until the cell voltage reached 0.005V, and then paused for 20 minutes.

[0144] Next, lithium was discharged from the negative electrode at a constant current of 0.1C until the cell voltage reached 1.0V, and then the battery was paused for 20 minutes. Next, lithium was discharged from the negative electrode at a constant current of 0.01C until the cell voltage reached 1.0V, and then the battery was paused for 20 minutes. Furthermore, lithium was discharged from the negative electrode at a constant current of 0.001C until the cell voltage reached 1.0V, and then the battery was paused for 20 minutes.

[0145] <Second cycle>

[0146] The negative electrode was charged with lithium at a constant current of 0.1C until the cell voltage reached 0.005V, and then the battery was paused for 20 minutes. Next, the negative electrode was charged with lithium at a constant current of 0.01C until the cell voltage reached 0.005V, and then the battery was paused for 20 minutes. Furthermore, the negative electrode was charged with lithium at a constant current of 0.001C until the cell voltage reached 0.005V, and then the battery was paused for 20 minutes.

[0147] Next, the battery cell was removed and the thickness TA1 was measured at five locations of the negative electrode mixture layer. 1-1 ~TA1 1-5 , based on the initial thickness TA1 0-n And expansion thickness TA1 1-n (n = 1, 2, 3, 4, 5) Calculate the expansion rate = TA1 1-n / TA1 0-n . Find the average of their expansion rates, and the result is 1.43.

[0148] Comparative Example 1

[0149] Instead of composite particles A1, a general silicon-containing material having no pores in the particles, namely SiO x The evaluation battery cell B1 was prepared in the same manner as in Example 1 except that the particles (x=1) (nano-Si was dispersed in the matrix of the SiO2 matrix phase) were used for evaluation. 0-n (n=1, 2, 3, 4, 5) and expansion thickness TB1 1-n (n = 1, 2, 3, 4, 5) Calculate the expansion ratio = TB1 1-n / TB1 0-n The average value is 1.95.

[0150] Comparative Example 2

[0151] Composite A1 was synthesized in the same manner as in Example 1, separated by suction filtration, and then vacuum dried at 60°C without washing with distilled water. The dried composite (hereinafter, composite B2) was crushed in a mortar. The content of sulfur element derived from ammonium persulfate in the crushed composite B2 (composite particles B2) was measured by ICP-AES, and the result was 0.71% by mass.

[0152] 《Example 2》

[0153] After separating the composite A1 by suction filtration, it was thoroughly washed with distilled water. The washed composite A1 was put into 500 mL of pure water, and then washed for 5 hours while stirring. Then, the composite A1 was separated by suction filtration and vacuum dried at 60°C. The dried composite A1 was crushed in a mortar and passed through a sieve with a mesh of 75 μm. The content of sulfur element derived from ammonium persulfate in the crushed composite (hereinafter referred to as composite particles A2) was measured by ICP-AES, and the result was 0.05% by mass.

[0154] 《Example 3》

[0155] Composite A1 was synthesized in the same manner as in Example 1, separated by suction filtration, and then vacuum dried at 60°C without washing with distilled water. The dried composite (hereinafter, composite B2) was crushed in a mortar and passed through a sieve with a mesh of 75 μm. The crushed composite B2 (composite particles B2) was put into 500 mL of pure water, and then washed with water for 5 hours while stirring. Then, the composite particles (hereinafter referred to as composite particles A3) were separated by suction filtration and vacuum dried at 60°C. The content of sulfur element derived from ammonium persulfate in composite particles A3 was measured by ICP-AES, and the result was 0.03% by mass.

[0156] The results are summarized in Table 1.

[0157] [Table 1]

[0158]

[0159] As shown in Table 1, the case where the composite particles A1 were used was different from the case where SiO x In addition, it is known that the sulfur content can be significantly reduced by washing the composite after pulverization.

[0160] Industrial Applicability

[0161] The secondary battery including the negative electrode active material of the present disclosure is suitable for use as a main power source for mobile communication devices, portable electronic devices, etc., a vehicle-mounted power source, etc., but the use is not limited thereto.

[0162] The present invention has been described with respect to the presently preferred embodiments, but such disclosure is not to be construed in a limiting sense. Various modifications and changes should be apparent to those skilled in the art in the art of the present invention upon reading the above disclosure. Therefore, the appended claims should be construed as including all modifications and changes without departing from the spirit and scope of the present invention.

[0163] Description of Reference Numerals

[0164] 10: secondary battery, 11: sealing body, 12: valve body, 13: metal plate, 14: insulating member, 15: positive electrode, 15a: positive electrode lead, 16: negative electrode, 16a: negative electrode lead, 17: separator, 18: electrode group, 21: gasket, 22: battery can, 22a: groove part, 23: first insulating plate, 24: second insulating plate, 16: negative electrode.

Claims

1. A negative electrode active material for a secondary battery, comprising composite particles comprising a conductive polymer and Si-containing particles, In the composite particles, a plurality of the Si-containing particles are connected via the conductive polymer. The composite particles have a particle size D50 at a cumulative volume of 50% in a volume-based particle size distribution of 100 μm or less, The composite particles contain sulfur. The content of the sulfur element in the composite particles is less than 0.05 mass %.

2. The negative electrode active material for a secondary battery according to claim 1, wherein The composite particles have a free volume.

3. The negative electrode active material for a secondary battery according to claim 1 or 2, wherein The composite particles further contain nitrogen.

4. The negative electrode active material for a secondary battery according to any one of claims 1 to 3, wherein The conductive polymer includes polyaniline.

5. The negative electrode active material for a secondary battery according to any one of claims 1 to 4, wherein The composite particles have a particle size D10 of 0.5 μm to 50 μm when the cumulative volume is 10% in a volume-based particle size distribution, and a particle size D90 of 50 μm to 500 μm when the cumulative volume is 90%.

6. The negative electrode active material for a secondary battery according to any one of claims 1 to 5, wherein The powder resistivity of the composite particles is 10 3 Ω·cm~10 7 Ω·cm.

7. The negative electrode active material for a secondary battery according to any one of claims 1 to 6, wherein The average particle size of the Si-containing particles is 10 nm to 500 nm.

8. The negative electrode active material for a secondary battery according to any one of claims 1 to 7, wherein The content of the Si-containing particles in the composite particles is 30% by mass to 90% by mass.

9. The negative electrode active material for a secondary battery according to any one of claims 1 to 8, wherein At least a portion of the surface of the Si-containing particles is covered with a conductive carbon material. 10 . A negative electrode for a secondary battery, comprising the negative electrode active material for a secondary battery according to claim 1 .

11. A secondary battery comprising a positive electrode, a negative electrode and a non-aqueous electrolyte, The negative electrode is the negative electrode for a secondary battery according to claim 10 .

12. A method for producing a negative electrode active material for a secondary battery, comprising the following steps: In the first step, a monomer as a raw material of a conductive polymer, a polymerization initiator containing sulfur, and Si-containing particles are mixed to polymerize the monomer, thereby synthesizing a composite body, wherein the composite body includes a conductive polymer and Si-containing particles, and a plurality of the Si-containing particles are connected via the conductive polymer; A second step of pulverizing the composite to obtain composite particles having a particle size D50 of 100 μm or less when the cumulative volume in the volume-based particle size distribution is 50%; and In a third step, the composite particles are washed until the content of the sulfur element in the composite particles is less than 0.05 mass %.

Citation Information

Patent Citations

  • Organic polymer-silicon composite particles, methods for producing the same, and negative electrode and lithium secondary battery containing the same

    JP2013522820A