Modified silicon-carbon laminated lithium battery and formation method thereof

By using a highly elastic wound three-dimensional conductive grid and polymer separator in silicon carbon laminated lithium batteries, combined with staged charging and discharging operations, the expansion and stripping problem of silicon-based negative electrode is solved, and the high-temperature circulation and high-rate performance of the battery is improved, ensuring that More uniform protective interface mask formation.

CN119050445AActive Publication Date: 2024-11-29YIBEI NEW ENERGY TECH (HUIZHOU) CO LTD

Patent Information

Application Number
CN202411385431.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-29
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

During the charging and discharging process, existing silicon-based laminated lithium batteries cause the silicon-based negative electrode to expand due to lithium ions embedded in the charging and discharging process, causing stress differences and causing peeling of the negative electrode active material, affecting battery performance and safety.

Method used

Using a highly elastic wound three-dimensional conductive grid and polymer diaphragm, through staged charging and discharging operations, combining high-temperature, high-voltage, high-current, constant current charging and low-temperature, high-voltage, high-current, constant current discharge, inhibits the expansion and peeling of silicon-carbon materials, and makes polymer diaphragm The silicon carbon material is bonded or peeled off as the temperature changes.

Benefits of technology

It effectively reduces the expansion rate and peeling phenomenon of the silicon-based negative electrode, improves the high-temperature circulation and high-rate performance of modified silicon-carbon laminated lithium batteries, ensures a more uniform protective interface film formation, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050445A_ABST
    Figure CN119050445A_ABST
Patent Text Reader

Abstract

The invention provides a modified silicon-carbon laminated lithium battery and a formation method thereof. According to the formation method, the high-elasticity winding three-dimensional conductive net is formed in the silicon-based negative plate of the modified silicon-carbon laminated lithium battery and is a polymer diaphragm; sequentially carrying out a first section of low-temperature low-voltage small-current constant-current charging operation, a second section of low-temperature medium-voltage medium-current constant-current charging operation, a third section of high-temperature high-voltage large-current constant-current charging operation and a fourth section of low-temperature high-voltage large-current constant-current discharging operation on the liquid-injected modified silicon carbon laminated lithium battery, and finally carrying out normal-temperature standing operation. According to the method, the polymer diaphragm can change along with the temperature change of the formation process, the added high-elasticity winding three-dimensional conductive net can effectively restrain the problem of expansion and stripping of the silicon-based negative electrode of the high-energy and high-rate laminated lithium battery in the formation process, the elastic modulus of the negative electrode active material layer is also increased, the expansion deformation is reduced, and the stability of the lithium battery is improved. And the cycle performance and the high-rate performance of the modified silicon-carbon laminated lithium battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of laminated lithium batteries, and in particular to a modified silicon-carbon laminated lithium battery and a formation method thereof. Background Art

[0002] Generally, the battery capacity depends on the positive electrode material. In order to maximize the positive electrode of the laminated lithium battery, the laminated lithium battery generally uses the alternating stacking process of "negative electrode-positive electrode-negative electrode" to fully utilize the positive electrode material. However, it will cause the lithium ions to be embedded only on the side corresponding to the positive electrode of the two outermost silicon-based negative electrodes, while the other side of the silicon-based negative electrode facing away from the positive electrode has no lithium ions embedded. When the laminated lithium battery is fully charged, due to the embedding of lithium ions, the volume of the side of the silicon-based negative electrode corresponding to the positive electrode expands and becomes larger, resulting in a strong stress difference between the two sides of the outermost two silicon-based negative electrodes, which leads to the phenomenon that the negative electrode active material of the silicon-based negative electrode peels off the negative electrode current collector. Especially after the pressure is fully charged, the phenomenon of the negative electrode active material peeling off the negative electrode current collector is more obvious, and the peeled negative electrode active material can easily pierce the diaphragm and cause safety problems; or the peeled negative electrode active material is free inside the battery, causing self-discharge to affect the battery performance.

[0003] For this reason, some scholars believe that the above problems can be solved by optimizing the formation process of silicon-based laminated lithium batteries. However, for example, Chinese patent document No. CN108258347B discloses a formation method for a silicon negative electrode soft-pack lithium-ion battery, which controls the uniform volume change of the silicon-based negative electrode during the charging and discharging process by controlling the upper limit voltage of the charge in stages, applying mechanical external pressure to the outside of the battery, and applying negative pressure to the inside of the battery. This effectively improves the wrinkling problem of the silicon-based negative electrode in the lithium-ion soft-pack battery, but does not reflect a good inhibitory effect on the expansion of the silicon-based negative electrode; for example, Chinese patent document No. CN 117080594 A discloses a formation method for a silicon negative electrode soft-pack lithium-ion battery, which adopts a full charge formation process and gradually increases the pressure, improves the utilization rate of the electrolyte, and is conducive to the formation of a more uniform, stable and dense SEI film, but does not reflect a good inhibitory effect on the expansion of the silicon-based negative electrode; and after pressurization, P3>P2, resulting in excessive pressure that damages the inside of the lithium battery and affects the cycle life of the lithium battery. It can be seen that the above-mentioned silicon-based laminated lithium battery formation process is still unable to effectively suppress the expansion and peeling problem of the silicon-based negative electrode during the formation process of the high-energy and high-rate laminated lithium battery. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a modified silicon-carbon laminated lithium battery and its formation method, wherein the polymer diaphragm can change with the temperature change of the formation process, and the added high-elasticity winding three-dimensional conductive network can effectively suppress the expansion and peeling problem of the silicon-based negative electrode in the formation process of the high-energy and high-rate laminated lithium battery, and at the same time increase the elastic modulus of the negative electrode active material layer and reduce the expansion deformation, thereby improving the high-temperature cycle performance and high-rate performance of the modified silicon-carbon laminated lithium battery.

[0005] The purpose of this disclosure is achieved through the following technical solutions:

[0006] A modified silicon-carbon laminate lithium battery comprises the following steps:

[0007] Obtaining a modified silicon-carbon laminated lithium battery filled with liquid; wherein a highly elastic winding three-dimensional conductive mesh is formed in the negative electrode active material layer of the silicon-based negative electrode sheet of the modified silicon-carbon laminated lithium battery, and the highly elastic winding three-dimensional conductive mesh is used to inhibit the expansion and peeling of the silicon-carbon material; the diaphragm of the modified silicon-carbon laminated lithium battery is a polymer diaphragm;

[0008] The modified silicon-carbon laminated lithium battery injected with liquid is subjected to a first stage of low-temperature, low-voltage, small-current constant-current charging operation to charge the modified silicon-carbon laminated lithium battery to 15% to 20% SOC;

[0009] The modified silicon-carbon laminated lithium battery that has undergone the first stage of low-temperature, low-voltage, small-current constant-current charging operation is subjected to a second stage of low-temperature, medium-voltage, medium-current constant-current charging operation, so that the modified silicon-carbon laminated lithium battery is charged to 40% to 60% SOC;

[0010] The modified silicon-carbon laminated lithium battery that has undergone the second stage of low-temperature, medium-voltage, medium-current constant-current charging operation is subjected to a third stage of high-temperature, high-voltage, large-current constant-current charging operation, so that the modified silicon-carbon laminated lithium battery is charged to 100% SOC;

[0011] The modified silicon-carbon laminated lithium battery that has undergone the third stage of high-temperature, high-pressure, high-current constant-current charging operation is subjected to a fourth stage of low-temperature, high-voltage, high-current constant-current discharging operation, so that the modified silicon-carbon laminated lithium battery is discharged to 30% to 50% DOD;

[0012] The modified silicon-carbon laminated lithium battery that has undergone the fourth stage of low-temperature, high-voltage, high-current constant-current discharge operation is subjected to a room-temperature static operation.

[0013] In one embodiment, the first stage of low-temperature, low-voltage, small-current constant-current charging operation is performed under the conditions of a pressure F1 of 1kgf / cm2 to 2kgf / cm2, a temperature of 30°C to 40°C, and a current of 0.1C to 0.2C.

[0014] In one embodiment, the second stage low temperature, medium voltage, medium current constant current charging operation is performed under the conditions of pressure F2 of 3kgf / cm2 to 4kgf / cm2, temperature of 30℃ to 40℃, and current of 0.3C to 0.4C.

[0015] In one embodiment, the third stage high temperature, high pressure, large current constant current charging operation is performed under the conditions of pressure F3 of 6kgf / cm2 to 8kgf / cm2, temperature of 80℃ to 90℃, and current of 0.5C to 1.0C.

[0016] In one embodiment, the fourth stage of low-temperature, high-voltage, high-current constant-current discharge is carried out under the conditions of a pressure F4 of 6kgf / cm2 to 8kgf / cm2, a temperature of 30°C to 40°C, and a current of 0.5C to 1.0C.

[0017] In one embodiment, the time of the room temperature static operation is 1 hour to 4 hours.

[0018] In one embodiment, the negative electrode active material layer includes graphite, silicon-carbon material, linear single-walled carbon nanotubes, mesh carbon fibers and a highly elastic binder;

[0019] The linear single-walled carbon nanotubes, the mesh carbon fibers and the highly elastic binder are mixed to form the highly elastic winding three-dimensional conductive mesh;

[0020] The highly elastic wound three-dimensional conductive mesh is mixed with the silicon-carbon material and the graphite to obtain a negative electrode slurry; the negative electrode slurry is coated on a negative electrode current collector to form the negative electrode active material layer.

[0021] In one embodiment, the length of the linear single-walled carbon nanotube is 8 nm to 10 nm; and / or,

[0022] The length of the mesh carbon fiber is 100um to 200um; and / or,

[0023] The highly elastic binder includes at least one of PMA, PAA and SBR.

[0024] A modified silicon-carbon laminate lithium battery is prepared by the formation method of the modified silicon-carbon laminate lithium battery described in any of the above embodiments.

[0025] In one embodiment, the modified silicon-carbon laminate lithium battery includes a shell and a battery cell, the battery cell is arranged in the shell, the battery cell includes a plurality of alternately stacked silicon-based negative electrode sheets, positive electrode sheets and silicon-based negative electrode sheets, the silicon-based negative electrode sheets are separated from the positive electrode sheets by a diaphragm, and the diaphragm extends to the outer side surfaces of the silicon-based negative electrode sheets located on the outermost sides of the battery cell.

[0026] Compared with the prior art, the present invention has at least the following advantages:

[0027] 1) The first stage of low-temperature, low-voltage, small-current constant-current charging operation, the second stage of low-temperature, medium-voltage, medium-current constant-current charging operation, and the third stage of high-temperature, high-voltage, large-current constant-current charging operation are adopted to realize the slow charging operation of the modified silicon-carbon laminated lithium battery in stages, so as to avoid the problem of the silicon-carbon material expanding too fast and causing expansion and peeling due to the modified silicon-carbon laminated lithium battery being charged too fast; at the same time, when the modified silicon-carbon laminated lithium battery is fully charged to 100% SOC, it is ensured that the active materials in the modified silicon-carbon laminated lithium battery can achieve full, comprehensive and rapid reaction, that is, the modified silicon-carbon laminated lithium battery is easier to form under the condition of full charge, which is conducive to the modification. A uniform protective interface film is formed inside the modified silicon-carbon laminated lithium battery, thereby improving the high-rate performance and high-temperature cycle performance of the modified silicon-carbon laminated lithium battery; and the added fourth low-temperature, high-voltage, high-current constant-current discharge operation enables the modified silicon-carbon laminated lithium battery to discharge to 30%-50% DOD, which, on the one hand, reduces the stress difference of the silicon-based negative electrode sheets on the outermost sides of the cell of the modified silicon-carbon laminated lithium battery, and effectively reduces the phenomenon of negative electrode active material peeling off the negative electrode current collector; on the other hand, it also better ensures that the liquid retention of the modified silicon-carbon laminated lithium battery at this time is sufficient, so as to ensure that a more uniform protective interface film is formed inside the modified silicon-carbon laminated lithium battery.

[0028] 2) Since a highly elastic wound three-dimensional conductive mesh is formed in the negative active material layer of the silicon-based negative electrode sheet, the highly elastic wound three-dimensional conductive mesh plays a restraining role at the beginning stage of the expansion of the silicon-carbon material, so as to more comprehensively restrain the expansion of the internal silicon-carbon material that restrains the negative active material layer; effectively reducing the expansion rate of the silicon-based negative electrode sheet itself; especially in conjunction with the optimized process disclosed in the present invention, the problem of expansion and peeling of the silicon-carbon material can be more effectively suppressed; and the added highly elastic wound three-dimensional conductive mesh improves the conductive properties of the silicon-based negative electrode sheet, so as to improve the conductive capacity of the negative active material layer, which is beneficial to improving the high-rate performance of the modified silicon-carbon laminated lithium battery, while also increasing the elastic modulus of the negative active material layer, reducing expansion deformation, and thus improving the high-temperature cycle performance of the modified silicon-carbon laminated lithium battery.

[0029] 3) Since the diaphragm of the modified silicon-carbon laminated lithium battery is a polymer diaphragm, the surface of the polymer diaphragm can be softened as the temperature of the formation process increases. When the modified silicon-carbon laminated lithium battery is in the third stage of high-temperature, high-voltage, high-current constant-current charging operation, the expansion rate of the silicon-carbon material is the largest at this time, so that the softened polymer diaphragm can better bond with the expanded silicon-carbon material, effectively avoiding the phenomenon of expansion and peeling of the silicon-carbon material under the condition of maximum expansion rate, and further suppressing the problem of expansion and peeling of the silicon-carbon material; and, when the modified silicon-carbon laminated lithium battery is in the fourth stage of low-temperature, high-voltage, high-current constant-current discharge operation, the polymer diaphragm will gradually harden and lose its viscosity due to the drop in temperature, which is conducive to a more comprehensive peeling of the polymer diaphragm and the silicon-carbon material, effectively avoiding the negative electrode active material layer from adhering to the polymer diaphragm and affecting the cycle performance of the modified silicon-carbon laminated lithium battery, and coordinating with the use of the high-elastic winding three-dimensional conductive mesh and the optimized process disclosed in the present invention, so as to more effectively suppress the expansion and peeling of the silicon-based negative electrode of the high-energy and high-rate laminated lithium battery in the formation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 This is a flow chart of a modified silicon-carbon laminate lithium battery according to an embodiment of the present invention;

[0032] Figure 2 This is a comparison diagram of the expansion of the modified silicon-carbon laminate lithium battery of Example 2 of the present invention and Comparative Example 14;

[0033] Figure 3 It is a charge and discharge curve diagram at different rates of Example 2 of the present invention. DETAILED DESCRIPTION

[0034] In order to facilitate the understanding of the present disclosure, the present disclosure will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present disclosure are given in the drawings. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present disclosure more thoroughly and comprehensively understood.

[0035] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.

[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present disclosure. The terms used herein in the specification of the present disclosure are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0037] The present invention provides a formation method for a modified silicon-carbon laminated lithium battery, and obtains a modified silicon-carbon laminated lithium battery filled with liquid; wherein a highly elastic winding three-dimensional conductive network is formed in the negative electrode active material layer of the silicon-based negative electrode sheet of the modified silicon-carbon laminated lithium battery, and the highly elastic winding three-dimensional conductive network is used to inhibit the expansion and peeling of the silicon-carbon material; the diaphragm of the modified silicon-carbon laminated lithium battery is a polymer diaphragm; the modified silicon-carbon laminated lithium battery filled with liquid is subjected to a first stage of low-temperature, low-voltage, small-current constant-current charging operation, so that the modified silicon-carbon laminated lithium battery is charged to 15% to 20% SOC; the modified silicon-carbon laminated lithium battery that has undergone the first stage of low-temperature, low-voltage, small-current constant-current charging operation is subjected to a second stage of low-temperature, low-voltage, small-current constant-current charging operation. The modified silicon-carbon laminated lithium battery is charged to 40% to 60% SOC by a medium-voltage medium-current constant-current charging operation; the modified silicon-carbon laminated lithium battery that has undergone the second stage of low-temperature medium-voltage medium-current constant-current charging operation is charged to 100% SOC by a third stage of high-temperature high-pressure large-current constant-current charging operation; the modified silicon-carbon laminated lithium battery that has undergone the third stage of high-temperature high-pressure large-current constant-current charging operation is discharged to 30% to 50% DOD by a fourth stage of low-temperature high-pressure large-current constant-current discharge operation; the modified silicon-carbon laminated lithium battery that has undergone the fourth stage of low-temperature high-pressure large-current constant-current discharge operation is left standing at room temperature.

[0038] The above-mentioned modified silicon-carbon laminate lithium battery formation method reduces the expansion rate of the silicon-based negative electrode sheet itself, and also optimizes the polymer diaphragm so that the polymer diaphragm can change with the temperature change of the formation process, that is, the polymer diaphragm softens during the third stage of high-temperature, high-voltage, high-current constant-current charging operation, so that the softened polymer diaphragm can better bond to the expanded silicon-carbon material, effectively avoiding the phenomenon of expansion and peeling of the silicon-carbon material under the condition of the maximum expansion rate, and further suppressing the problem of expansion and peeling of the silicon-carbon material; and the polymer diaphragm will slowly shrink due to the temperature drop during the fourth stage of low-temperature, high-voltage, high-current constant-current discharge operation. Slowly hardening to make the polymer lose its viscosity is conducive to a more comprehensive peeling of the polymer diaphragm and the silicon-carbon material, effectively avoiding the negative electrode active material layer from adhering to the polymer diaphragm and affecting the cycle performance of the modified silicon-carbon laminated lithium battery, so as to more effectively suppress the expansion and peeling of the silicon-based negative electrode in the formation process of the high-energy and high-rate laminated lithium battery. In addition, the added high-elastic winding three-dimensional conductive mesh not only improves the conductivity of the negative electrode active material layer, which is conducive to improving the high-rate performance of the modified silicon-carbon laminated lithium battery, but also increases the elastic modulus of the negative electrode active material layer, reduces expansion deformation, and thus improves the high-temperature cycle performance of the modified silicon-carbon laminated lithium battery.

[0039] See also Figure 1 In order to better understand the technical solution and beneficial effects of the present disclosure, the present disclosure is further described in detail below in conjunction with specific embodiments. A modified silicon-carbon laminate lithium battery of one embodiment includes some or all of the following steps:

[0040] S101. Obtain a modified silicon-carbon laminated lithium battery filled with liquid; wherein, a highly elastically wound three-dimensional conductive mesh is formed in the negative electrode active material layer of the silicon-based negative electrode sheet of the modified silicon-carbon laminated lithium battery, and the highly elastically wound three-dimensional conductive mesh is used to inhibit the expansion and peeling of the silicon-carbon material; the diaphragm of the modified silicon-carbon laminated lithium battery is a polymer diaphragm.

[0041] It is understandable that there are also some Chinese patent documents that suppress the volume expansion of silicon-based negative electrodes by optimizing the structure of silicon-based negative electrodes, thereby improving the cycle performance, safety and high-current charge and discharge capabilities of silicon-based lithium-ion batteries. For example, Chinese patent document No. CN111129427B discloses a silicon-based negative electrode and a preparation method thereof, by adding a functional coating on the active material layer, so that the polypyrrole, single-walled carbon nanotubes and carboxymethyl cellulose lithium of the functional coating can form a three-dimensional mesh conductive network to achieve a cage effect on the volume expansion of the silicon-based negative electrode, so as to suppress the volume expansion of the silicon-based negative electrode. However, since the functional coating is directly reacted and formed on the active material layer, that is, the functional coating is formed and fixed on one side of the active material layer, the functional coating will only play an inhibitory role when the active material layer expands to a greater extent, and it is impossible to achieve a better inhibitory and restraining effect on the inside of the active material layer, and there is still a probability of silicon-carbon material expansion and peeling.

[0042] Therefore, in the present disclosure, a highly elastically wound three-dimensional conductive mesh is formed within the negative electrode active material layer, so that the highly elastically wound three-dimensional conductive mesh plays a restraining role at the beginning stage of the expansion of the silicon-carbon material, so as to more comprehensively restrain the expansion of the internal silicon-carbon material that restrains the negative electrode active material layer; effectively reduce the expansion rate of the silicon-based negative electrode sheet itself; thereby effectively reducing the probability of expansion and peeling of the silicon-carbon material, and also reducing the side reactions of the modified silicon-carbon laminated lithium battery at high temperature, thereby improving the high temperature performance of the modified silicon-carbon laminated lithium battery while taking into account the improvement of the energy density of the modified silicon-carbon laminated lithium battery.

[0043] It should be noted that although the newly added highly elastic winding three-dimensional conductive mesh can better suppress the expansion rate of the bound silicon-based negative electrode sheet itself, due to the expansion coefficient of the silicon-carbon material expansion being about 300%, for some high-energy and high-rate laminated lithium batteries, simply optimizing the material structure of the silicon-based negative electrode still cannot effectively suppress the expansion of its silicon-carbon material. Especially when the high-energy and high-rate laminated lithium battery is fully charged, the silicon-carbon material is fully embedded with lithium to achieve the maximum expansion, and the highly elastic winding three-dimensional conductive mesh has pores, resulting in the probability that a small part of the silicon-carbon material still has the expansion and peeling off the pores of the highly elastic winding three-dimensional conductive mesh.

[0044] Therefore, in the present disclosure, by adopting a polymer diaphragm, the added polymer diaphragm can change with the temperature change of the formation process, that is, the polymer diaphragm softens during the third stage of high temperature, high pressure, large current constant current charging operation, and the softened polymer diaphragm can better bond with the expanded silicon-carbon material, effectively avoiding the expansion and peeling of the silicon-carbon material under the condition of maximum expansion rate, and further suppressing the expansion and peeling of the silicon-carbon material; and the polymer diaphragm will slowly harden due to the drop in temperature during the fourth stage of low temperature, high pressure, large current constant current discharge operation to make the polymer lose its viscosity, which is conducive to a more comprehensive peeling of the polymer diaphragm and the silicon-carbon material, effectively avoiding the negative electrode active material layer from adhering to the polymer diaphragm and affecting the cycle performance of the modified silicon-carbon laminated lithium battery, so as to more effectively suppress the expansion and peeling problem of the silicon-based negative electrode of the high-energy and high-rate laminated lithium battery during the formation process.

[0045] S102, performing the first stage of low-temperature, low-voltage, small-current constant-current charging operation on the modified silicon-carbon laminated lithium battery that has been filled with liquid, so that the modified silicon-carbon laminated lithium battery is charged to 15% to 20% SOC; so as to realize the first stage of slow charging operation of the modified silicon-carbon laminated lithium battery, so as to avoid the problem of the modified silicon-carbon laminated lithium battery expanding too fast due to over-rapid charging, thereby causing expansion and peeling, and also realize the preliminary heating of the polymer diaphragm.

[0046] S103. Perform a second stage of low-temperature, medium-voltage, medium-current constant-current charging operation on the modified silicon-carbon laminated lithium battery that has undergone the first stage of low-temperature, low-voltage, small-current constant-current charging operation, so that the modified silicon-carbon laminated lithium battery is charged to 40% to 60% SOC, so as to achieve a faster charging operation of the modified silicon-carbon laminated lithium battery in the second stage, so as to avoid the problem of the modified silicon-carbon laminated lithium battery expanding too fast due to over-rapid charging, thereby causing expansion and peeling; and also achieve secondary heating of the polymer diaphragm.

[0047] S104, performing a third stage of high temperature, high pressure, large current constant current charging operation on the modified silicon-carbon laminated lithium battery that has undergone the second stage of low temperature, medium pressure, medium current constant current charging operation, so that the modified silicon-carbon laminated lithium battery is charged to 100% SOC, so as to achieve a faster charging operation of the modified silicon-carbon laminated lithium battery in the third stage, so as to avoid the problem of the modified silicon-carbon laminated lithium battery expanding too fast due to over-rapid charging, thereby causing expansion and peeling.

[0048] It can be understood that when the modified silicon-carbon laminated lithium battery is fully charged to 100% SOC, it ensures that the active materials in the modified silicon-carbon laminated lithium battery can achieve full, comprehensive and rapid reaction, that is, the modified silicon-carbon laminated lithium battery is easier to form under fully charged conditions, especially with the first stage of low temperature, low voltage, small current constant current charging operation, the second stage of low temperature, medium voltage, medium current constant current charging operation and the third stage of high temperature, high voltage and large current constant current charging operation, which is conducive to the formation of a uniform protective interface film inside the modified silicon-carbon laminated lithium battery, thereby improving the high rate performance and high temperature cycle performance of the modified silicon-carbon laminated lithium battery.

[0049] It can also be understood that when the modified silicon-carbon laminate lithium battery is fully charged to 100% SOC, the expansion rate of the silicon-carbon material is the largest at this time, and the polymer surface of the polymer membrane can be softened, so that the softened polymer membrane can better bond to the expanded silicon-carbon material, effectively avoiding the phenomenon of expansion and peeling of the silicon-carbon material under the condition of maximum expansion rate, and further suppressing the problem of expansion and peeling of the silicon-carbon material.

[0050] S105, performing a fourth stage of low temperature, high pressure, high current constant current discharge operation on the modified silicon-carbon laminated lithium battery that has undergone the third stage of high temperature, high pressure, high current constant current charge operation, so that the modified silicon-carbon laminated lithium battery is discharged to 30% to 50% DOD.

[0051] It can be understood that when the modified silicon-carbon laminated lithium battery is in the fourth stage of low-temperature, high-voltage, high-current constant-current discharge operation, the modified silicon-carbon laminated lithium battery is discharged to 30% to 50% DOD. On the one hand, it reduces the stress difference of the silicon-based negative electrode sheets on the outermost sides of the cell of the modified silicon-carbon laminated lithium battery, and effectively reduces the phenomenon of negative electrode active material peeling off the negative electrode current collector; on the other hand, it also better ensures that the liquid retention of the modified silicon-carbon laminated lithium battery is sufficient at this time, so as to ensure that a more uniform protective interface film is formed inside the modified silicon-carbon laminated lithium battery; on the other hand, due to the drop in temperature, the polymer diaphragm It will slowly harden and lose its stickiness, which is conducive to a more comprehensive peeling of the polymer diaphragm and the silicon-carbon material, effectively avoiding the negative electrode active material layer from adhering to the polymer diaphragm and affecting the cycle performance of the modified silicon-carbon laminated lithium battery, so as to more effectively inhibit the expansion and peeling of the silicon-based negative electrode in the formation process of the high-energy and high-rate laminated lithium battery; on the other hand, it also achieves a faster cooling of the modified silicon-carbon laminated lithium battery, effectively avoiding the problem of decomposition and damage of the protective interface film or volatilization of the organic solvent in the electrolyte caused by the modified silicon-carbon laminated lithium battery being exposed to high temperature for a long time.

[0052] S106. The modified silicon-carbon laminated lithium battery that has undergone the fourth stage of low-temperature, high-voltage, and high-current constant-current discharge operation is allowed to stand at room temperature so that the electrolyte can well infiltrate the battery cells of the modified silicon-carbon laminated lithium battery, which is beneficial to the normal discharge of the modified silicon-carbon laminated lithium battery, thereby ensuring that the silicon-carbon material can shrink well at room temperature, effectively avoiding the appearance of many wrinkles in the modified silicon-carbon laminated lithium battery; and at the same time, it is also beneficial to form a denser and more uniform protective interface film inside the modified silicon-carbon laminated lithium battery.

[0053] The above-mentioned formation method of the modified silicon-carbon laminated lithium battery adopts a first stage of low-temperature, low-voltage, small-current constant-current charging operation, a second stage of low-temperature, medium-voltage, medium-current constant-current charging operation, and a third stage of high-temperature, high-voltage, large-current constant-current charging operation to realize the modified silicon-carbon laminated lithium battery in stages and slowly charge the battery, so as to avoid the problem of the silicon-carbon material expanding too fast and causing expansion and peeling due to the modified silicon-carbon laminated lithium battery being charged too fast; at the same time, when the modified silicon-carbon laminated lithium battery is fully charged to 100% SOC, it is ensured that the active materials in the modified silicon-carbon laminated lithium battery can achieve a full, comprehensive and rapid reaction, that is, the modified silicon-carbon laminated lithium battery is more likely to react under fully charged conditions. Easy formation is conducive to the formation of a uniform protective interface film inside the modified silicon-carbon laminated lithium battery, thereby improving the high-rate performance and high-temperature cycle performance of the modified silicon-carbon laminated lithium battery; and the added fourth stage of low-temperature, high-voltage, and high-current constant-current discharge operation enables the modified silicon-carbon laminated lithium battery to discharge to 30% to 50% DOD, which, on the one hand, reduces the stress difference between the silicon-based negative electrode sheets on the outermost sides of the cell of the modified silicon-carbon laminated lithium battery, and effectively reduces the phenomenon of negative electrode active material peeling off the negative electrode current collector; on the other hand, it also better ensures that the liquid retention of the modified silicon-carbon laminated lithium battery at this time is sufficient, so as to ensure the formation of a more uniform protective interface film inside the modified silicon-carbon laminated lithium battery.

[0054] It can be understood that since a highly elastic three-dimensional conductive mesh is formed in the negative active material layer of the silicon-based negative electrode sheet, the highly elastic three-dimensional conductive mesh plays a restraining role at the beginning stage of the expansion of the silicon-carbon material, so as to more comprehensively restrain the expansion of the internal silicon-carbon material that restrains the negative active material layer; effectively reducing the expansion rate of the silicon-based negative electrode sheet itself; especially in conjunction with the optimized process of the present disclosure, the problem of expansion and peeling of the silicon-carbon material can be more effectively suppressed; and the added highly elastic three-dimensional conductive mesh improves the conductive properties of the silicon-based negative electrode sheet, so as to improve the conductive capacity of the negative active material layer, which is beneficial to improving the high-rate performance of the modified silicon-carbon laminated lithium battery, and at the same time increases the elastic modulus of the negative active material layer, reduces expansion deformation, and thus improves the high-temperature cycle performance of the modified silicon-carbon laminated lithium battery. For details, please refer to Figure 3 .

[0055] It can also be understood that, since the diaphragm of the modified silicon-carbon laminated lithium battery is a polymer diaphragm, the surface of the polymer diaphragm can be softened as the temperature of the formation process increases. When the modified silicon-carbon laminated lithium battery is in the third stage of high-temperature, high-pressure, high-current constant-current charging operation, the expansion rate of the silicon-carbon material at this time is the largest, so that the softened polymer diaphragm can better bond the expanded silicon-carbon material, effectively avoiding the phenomenon of expansion and peeling of the silicon-carbon material under the condition of the maximum expansion rate, and further suppressing the problem of expansion and peeling of the silicon-carbon material; and when the modified silicon-carbon laminated lithium battery is In the fourth stage of low-temperature, high-voltage, high-current constant-current discharge operation, the polymer diaphragm will gradually harden and lose its viscosity due to the drop in temperature, which is conducive to a more comprehensive peeling of the polymer diaphragm and the silicon-carbon material, effectively avoiding the negative electrode active material layer from adhering to the polymer diaphragm and affecting the cycle performance of the modified silicon-carbon laminated lithium battery. In conjunction with the use of the highly elastic winding three-dimensional conductive mesh and the optimized process disclosed in the present invention, the expansion and peeling problem of the silicon-based negative electrode of the high-energy and high-rate laminated lithium battery during the formation process can be more effectively suppressed, that is, the expansion rate of the modified silicon-carbon laminated lithium battery after formation is relatively small. For details, please refer to Figure 2 .

[0056] In one of the embodiments, the modified silicon-carbon laminated lithium battery is subjected to a vacuum sealing operation after being left standing at room temperature to effectively remove the gas in the modified silicon-carbon laminated lithium battery and seal it.

[0057] In one embodiment, when the pressure F1 is 1 kgf / cm 2 ~2kgf / cm 2 The first stage of low-temperature, low-voltage, small-current constant-current charging operation is carried out under the conditions of a temperature of 30°C to 40°C and a current of 0.1C to 0.2C. While realizing the first stage of slow charging operation of the modified silicon-carbon laminated lithium battery, it also realizes the preliminary heating of the polymer diaphragm.

[0058] In one embodiment, when the pressure F2 is 3 kgf / cm 2 ~4kgf / cm 2 The second stage of low-temperature, medium-voltage, medium-current constant-current charging operation is carried out under the conditions of a temperature of 30°C to 40°C and a current of 0.3C to 0.4C. While achieving a faster second-stage charging operation for the modified silicon-carbon laminate lithium battery, it also achieves secondary heating of the polymer diaphragm.

[0059] In one embodiment, the pressure F3 is 6 kgf / cm 2 ~8kgf / cm 2The third stage of high temperature, high pressure, large current constant current charging operation is carried out under the conditions of temperature of 80℃~90℃ and current of 0.5C~1.0C, so as to realize the third stage faster charging operation of the modified silicon-carbon laminated lithium battery, so that the modified silicon-carbon laminated lithium battery is easier to form under full charge conditions; at the same time, it also ensures that the polymer surface of the polymer diaphragm can be softened, so that the softened polymer diaphragm can better bond with the expanded silicon-carbon material, effectively avoiding the expansion and peeling of the silicon-carbon material under the condition of maximum expansion rate, and further suppressing the expansion and peeling of the silicon-carbon material.

[0060] It should be noted that the general formation temperature of lithium-ion batteries is 30°C to 60°C. When the formation temperature is higher than 60°C, the protective interface film in the modified silicon-carbon laminate lithium battery will be decomposed or the organic solvent in the electrolyte will volatilize. Therefore, in order to solve the above problems, in the present disclosure, 6kgf / cm 2 ~8kgf / cm 2 The high voltage and high current of 0.5C~1.0C are used for constant current fast charging to effectively shorten the time of the third stage of high temperature, high pressure and large current constant current charging operation, thereby ensuring that the modified silicon-carbon laminated lithium battery can reach 100% SOC within 1min~2min, especially in conjunction with the fourth stage of low temperature, high pressure and large current constant current discharge operation, which effectively avoids the problem that the modified silicon-carbon laminated lithium battery is easily decomposed and damaged in the protective interface film or the organic solvent in the electrolyte is volatilized under high temperature conditions for a long time, and the fourth stage of low temperature, high pressure and large current constant current discharge operation is still a large current, which not only saves charging time, but also improves the utilization rate of the formation equipment.

[0061] Furthermore, in one of the embodiments, the electrolyte is a high temperature resistant electrolyte to avoid the problem of the electrolyte being easily decomposed and damaged under high temperature conditions.

[0062] In one embodiment, when the pressure F4 is 6 kgf / cm 2 ~8kgf / cm 2 The fourth stage of low-temperature, high-voltage, and high-current constant-current discharge is carried out under the conditions of a temperature of 30°C to 40°C and a current of 0.5C to 1.0C. On the premise of ensuring that the stress difference of the silicon-based negative electrodes on the outermost sides of the cell of the modified silicon-carbon laminated lithium battery after discharge is small, it also ensures that the liquid retention of the modified silicon-carbon laminated lithium battery is sufficient, which is conducive to forming a more uniform protective interface film; it also makes the polymer diaphragm lose its viscosity as the temperature of the fourth stage decreases, which is conducive to a more comprehensive peeling off from the silicon-carbon material; it also achieves a relatively rapid cooling of the modified silicon-carbon laminated lithium battery, effectively avoiding the problem of decomposition and destruction of the protective interface film or volatilization of the organic solvent in the electrolyte caused by the modified silicon-carbon laminated lithium battery being under high temperature conditions for a long time.

[0063] In one embodiment, the time of the room temperature static operation is 1 hour to 4 hours.

[0064] In one embodiment, the polymer diaphragm is a PVDF polymer diaphragm. Since PVDF is an adhesive used for silicon-based negative electrode sheets or positive electrode sheets, the added PVDF polymer will not affect the electrical properties of the modified silicon-carbon laminated lithium battery. Moreover, when the PVDF polymer diaphragm is subjected to the third stage of high temperature, high pressure, and high current constant current charging operation at 80°C to 90°C, the polymer surface of the polymer diaphragm can be softened, while the interior of the PVDF layer and the base membrane of the PVDF polymer diaphragm will not be deformed.

[0065] In one embodiment, the PVDF polymer separator includes a base film and a PVDF layer coated on the base film. Specifically, the thickness of the PVDF layer is 2um to 3um to ensure that the PVDF is well softened at 80°C to 90°C.

[0066] In one embodiment, the molecular weight of PVDF is 400,000 Da to 600,000 Da, so as to ensure that the PVDF polymer is well softened at 80° C. to 90° C.

[0067] In one embodiment, the negative electrode active material layer includes graphite, silicon-carbon material, linear single-walled carbon nanotubes, mesh carbon fibers and a highly elastic binder; wherein the linear single-walled carbon nanotubes, the mesh carbon fibers and the highly elastic binder are mixed to form the highly elastic wound three-dimensional conductive mesh; the highly elastic wound three-dimensional conductive mesh is mixed with the silicon-carbon material and the graphite to obtain a negative electrode slurry; the negative electrode slurry is coated on a negative electrode current collector to form the negative electrode active material layer.

[0068] It can be understood that by using mesh carbon fibers as a matrix, adding linear single-walled carbon nanotubes and a highly elastic binder under mixing conditions, a highly elastically wound three-dimensional conductive mesh can be formed, and then the highly elastically wound three-dimensional conductive mesh is mixed with graphite and silicon-carbon materials, so that the highly elastically wound three-dimensional conductive mesh can wrap the silicon-carbon material and graphite, that is, the highly elastically wound three-dimensional conductive mesh is mixed inside the negative electrode active material layer, so as to effectively reduce the expansion rate of the silicon-based negative electrode sheet itself.

[0069] In one embodiment, the length of the linear single-walled carbon nanotube is 8nm to 10nm; in particular, the length of the mesh carbon fiber is 100um to 200um and the high elastic binder includes at least one of PMA (Propylene GlycolMethyl Ether Acetate), PAA (Polyacrylic Acid) and SBR (Styrene-Butadiene Rubber), so as to ensure the formation of a highly elastic entangled three-dimensional conductive network.

[0070] In one embodiment, the mass percentage of PMA is 0.3% to 1%, the mass percentage of PAA is 1% to 1.5%; and the mass percentage of SBR is 1.2% to 2%.

[0071] In a preferred embodiment, the high elastic binder is a mixture of PMA, PAA and SBR to ensure that the high elastic binder has a high elastic modulus, thereby increasing the elastic modulus of the silicon-based negative electrode material and effectively inhibiting the expansion of the silicon-based negative electrode material. Specifically, the mass percentage of PMA, PAA and SBR is 0.3:1:1.5.

[0072] Specifically, the linear single-walled carbon nanotubes, the mesh carbon fibers and the high-elastic binder are mixed at a stirring speed of 3000 r / min to 4000 r / min for 30 min to 60 min to ensure the formation of a highly elastic entangled three-dimensional conductive network; the highly elastic entangled three-dimensional conductive network is mixed with graphite and silicon-carbon materials at a stirring speed of 5000 r / min to 6000 r / min for 100 min to 120 min to obtain a negative electrode slurry.

[0073] In one embodiment, the negative electrode active material layer includes the following mass percentages: 81.2% to 85.5% graphite; 13% to 16% silicon-carbon material, 0.1% to 0.5% linear single-walled carbon nanotubes, 0.4% to 0.8% mesh carbon fiber and 1% to 1.5% high elastic binder to improve the conductivity of the negative electrode active material layer, which is beneficial to improving the high-rate performance of the modified silicon-carbon laminated lithium battery, while also increasing the elastic modulus of the negative electrode active material layer and reducing expansion deformation, thereby improving the high-temperature cycle performance of the modified silicon-carbon laminated lithium battery.

[0074] The present disclosure provides a modified silicon-carbon laminated lithium battery, which is prepared by the formation method of the modified silicon-carbon laminated lithium battery described in any of the above embodiments. It can be understood that the formation method of the present disclosure allows the polymer diaphragm to change with the temperature change of the formation process, and at the same time, with the use of the added high-elastic winding three-dimensional conductive mesh, the expansion and peeling problem of the silicon-based negative electrode of the high-energy and high-rate laminated lithium battery during the formation process is effectively suppressed, and the elastic modulus of the negative electrode active material layer is increased, and the expansion deformation is reduced, thereby improving the high-temperature cycle performance of the modified silicon-carbon laminated lithium battery.

[0075] In one embodiment, the modified silicon-carbon laminated lithium battery includes a shell and a battery cell, the battery cell is arranged in the shell, and the battery cell includes a plurality of alternately stacked silicon-based negative electrode sheets, positive electrode sheets and silicon-based negative electrode sheets to fully utilize the positive electrode material, thereby ensuring the preparation of high-energy and high-rate silicon-carbon laminated lithium batteries; the silicon-based negative electrode sheet is separated from the positive electrode sheet by a diaphragm, and the diaphragm extends to the outer side surfaces of the silicon-based negative electrode sheets located on the outermost sides of the battery cell respectively; the two outermost silicon-based negative electrode sheets are provided with a PVDF layer on one side facing away from the positive electrode sheet, so that the PVDF layer changes with the temperature change of the formation process disclosed in the present invention, so as to effectively suppress the problem of silicon-carbon material peeling off on the side of the two outermost silicon-based negative electrode sheets facing away from the positive electrode sheet.

[0076] Compared with the prior art, the present invention has at least the following advantages:

[0077] 1) The first stage of low-temperature, low-voltage, small-current constant-current charging operation, the second stage of low-temperature, medium-voltage, medium-current constant-current charging operation, and the third stage of high-temperature, high-voltage, large-current constant-current charging operation are adopted to realize the slow charging operation of the modified silicon-carbon laminated lithium battery in stages, so as to avoid the problem of the silicon-carbon material expanding too fast and causing expansion and peeling due to the modified silicon-carbon laminated lithium battery being charged too fast; at the same time, when the modified silicon-carbon laminated lithium battery is fully charged to 100% SOC, it is ensured that the active materials in the modified silicon-carbon laminated lithium battery can achieve full, comprehensive and rapid reaction, that is, the modified silicon-carbon laminated lithium battery is easier to form under the condition of full charge, which is conducive to the modification. A uniform protective interface film is formed inside the modified silicon-carbon laminated lithium battery, thereby improving the high-rate performance and high-temperature cycle performance of the modified silicon-carbon laminated lithium battery; and the added fourth low-temperature, high-voltage, high-current constant-current discharge operation enables the modified silicon-carbon laminated lithium battery to discharge to 30%-50% DOD, which, on the one hand, reduces the stress difference of the silicon-based negative electrode sheets on the outermost sides of the cell of the modified silicon-carbon laminated lithium battery, and effectively reduces the phenomenon of negative electrode active material peeling off the negative electrode current collector; on the other hand, it also better ensures that the liquid retention of the modified silicon-carbon laminated lithium battery at this time is sufficient, so as to ensure that a more uniform protective interface film is formed inside the modified silicon-carbon laminated lithium battery.

[0078] 2) Since a highly elastic wound three-dimensional conductive mesh is formed in the negative active material layer of the silicon-based negative electrode sheet, the highly elastic wound three-dimensional conductive mesh plays a restraining role at the beginning stage of the expansion of the silicon-carbon material, so as to more comprehensively restrain the expansion of the internal silicon-carbon material that restrains the negative active material layer; effectively reducing the expansion rate of the silicon-based negative electrode sheet itself; especially in conjunction with the optimized process disclosed in the present invention, the problem of expansion and peeling of the silicon-carbon material can be more effectively suppressed; and the added highly elastic wound three-dimensional conductive mesh improves the conductive properties of the silicon-based negative electrode sheet, so as to improve the conductive capacity of the negative active material layer, which is beneficial to improving the high-rate performance of the modified silicon-carbon laminated lithium battery, while also increasing the elastic modulus of the negative active material layer, reducing expansion deformation, and thus improving the high-temperature cycle performance of the modified silicon-carbon laminated lithium battery.

[0079] 3) Since the diaphragm of the modified silicon-carbon laminated lithium battery is a polymer diaphragm, the surface of the polymer diaphragm can be softened as the temperature of the formation process increases. When the modified silicon-carbon laminated lithium battery is in the third stage of high-temperature, high-voltage, high-current constant-current charging operation, the expansion rate of the silicon-carbon material is the largest at this time, so that the softened polymer diaphragm can better bond with the expanded silicon-carbon material, effectively avoiding the phenomenon of expansion and peeling of the silicon-carbon material under the condition of maximum expansion rate, and further suppressing the problem of expansion and peeling of the silicon-carbon material; and, when the modified silicon-carbon laminated lithium battery is in the fourth stage of low-temperature, high-voltage, high-current constant-current discharge operation, the polymer diaphragm will gradually harden and lose its viscosity due to the drop in temperature, which is conducive to a more comprehensive peeling of the polymer diaphragm and the silicon-carbon material, effectively avoiding the negative electrode active material layer from adhering to the polymer diaphragm and affecting the cycle performance of the modified silicon-carbon laminated lithium battery, and coordinating with the use of the high-elastic winding three-dimensional conductive mesh and the optimized process disclosed in the present invention, so as to more effectively suppress the expansion and peeling of the silicon-based negative electrode of the high-energy and high-rate laminated lithium battery in the formation process.

[0080] Compared with the prior art, the present invention has at least the following advantages:

[0081] Some specific examples are given below, and if % is mentioned, it means percentage by weight. It should be noted that the following examples do not exhaust all possible situations, and the materials used in the following examples can be obtained from commercial sources unless otherwise specified.

[0082] Table 1 Recipe

[0083]

[0084]

[0085] The formulations of Examples 1 to 3 and Comparative Examples 1 to 6 in Table 1 were prepared according to the following steps:

[0086] S1. Prepare materials according to the formula in Table 1;

[0087] S2, adding linear single-walled carbon nanotubes, mesh carbon fibers, PMA, PAA and SBR to a high-speed mixer in sequence for stirring and mixing, and controlling the stirring speed to be 3000 r / min; the mixing time is 40 min; and a highly elastic entangled three-dimensional conductive network is obtained;

[0088] S3, then add silicon-carbon material and graphite to stir and mix, and control the stirring speed to 6000r / min; the mixing time is 100min; to obtain negative electrode slurry;

[0089] S4, coating the negative electrode slurry on the negative electrode current collector and drying it to obtain a silicon-based negative electrode sheet;

[0090] S5, stacking a plurality of silicon-based negative electrode sheets, a plurality of positive electrode sheets (high-nickel ternary positive electrode sheets) and a plurality of PVDF-based polymer separators in an alternating stacking process of negative electrode sheet-positive electrode sheet-negative electrode sheet, and extending the PVDF-based polymer separators to the outer side surfaces of the silicon-based negative electrode sheets located on the outermost sides of the battery core, respectively; to prepare a modified silicon-carbon laminated lithium battery core;

[0091] S5, casing the modified silicon-carbon laminated lithium battery core and injecting a high temperature resistant electrolyte to obtain a modified silicon-carbon laminated lithium battery injected with electrolyte;

[0092] S6, performing a fixture forming process on the modified silicon-carbon laminated lithium battery that has been injected with liquid;

[0093] S61, at pressure F1 of 1kgf / cm 2 , the first stage of low temperature, low voltage, small current constant current charging operation is carried out at a temperature of 30°C and a current of 0.1C to 20% SOC;

[0094] S62, at pressure F2 of 4kgf / cm 2 , the second stage of low temperature medium voltage medium current constant current charging operation was carried out at a temperature of 40°C and a current of 0.4C to 60% SOC;

[0095] S63, at pressure F3 of 8kgf / cm 2 , the third stage of high temperature, high pressure, high current constant current charging operation is carried out at a temperature of 85°C and a current of 1.0C to 100% SOC;

[0096] S64, at pressure F4 of 8kgf / cm 2 , the fourth stage of low temperature, high voltage and high current constant current discharge is carried out to 50% DOD under the conditions of temperature of 30℃ and current of 1.0C;

[0097] S65, leaving the modified silicon-carbon laminate lithium battery after step S64 at room temperature for 2 hours to complete the formation process;

[0098] S7, performing evacuation and sealing operation on the modified silicon-carbon laminated lithium battery after step S65.

[0099] Comparative Example 7

[0100] The difference from Example 2 is that in Comparative Example 7, step S61 is omitted, and the rest remains unchanged.

[0101] Comparative Example 8

[0102] The difference from Example 2 is that: Comparative Example 8 omits step S62, and the rest remains unchanged.

[0103] Comparative Example 9

[0104] The difference from Example 9 is that the step S63 is omitted in Comparative Example 9, and the rest remains unchanged.

[0105] Comparative Example 10

[0106] The difference from Example 2 is that: Comparative Example 10 omits step S64, and the rest remains unchanged.

[0107] Comparative Example 11

[0108] The difference from Example 2 is that the temperature in step S63 of Comparative Example 11 is 78° C., and the rest remain unchanged.

[0109] Comparative Example 12

[0110] The difference from Example 2 is that the temperature in step S63 of Comparative Example 12 is 92° C., and the rest remains unchanged.

[0111] Comparative Example 13

[0112] The difference from Example 2 is that the temperature in step S64 of Comparative Example 13 is 10° C., and the rest remains unchanged.

[0113] Comparative Example 14

[0114] The difference from Example 2 is that the diaphragm of Comparative Example 14 is a ceramic diaphragm, and the rest remains unchanged.

[0115] The modified silicon-carbon laminate lithium batteries prepared in the above Examples 1 to 3 and Comparative Examples 1 to 14 were subjected to electrical performance tests as shown in Table 2 below to obtain the experimental data in Table 2.

[0116] Table 2

[0117]

[0118]

[0119] From the comparison between Examples 1 to 3 and Comparative Examples 1 to 2 in the above table, it can be seen that, because Examples 1 to 3 use both linear single-walled carbon nanotubes and mesh carbon fibers, the comprehensive indicators of Examples 1 to 3 are significantly better than those of Comparative Examples 1 to 2. Among them, the comprehensive indicators of Example 2 are the best.

[0120] From the comparison between Example 2 and Comparative Examples 3-5 in the above table, it can be seen that since Example 2 uses PMA, PAA and SBR at the same time, the comprehensive indicators of Example 2 are obviously better than those of Comparative Examples 3-5.

[0121] From the comparison between Example 2 and Comparative Example 6 in the above table, it can be seen that the comprehensive indicators of Example 2 are significantly better than those of Comparative Example 6 because Example 2 uses a PVDF polymer membrane.

[0122] From the comparison between Example 2 and Comparative Examples 7-10 in the above table, it can be seen that, since Example 2 adopts the formation optimization process, the comprehensive indicators of Example 2 are obviously better than those of Comparative Examples 7-10.

[0123] From the comparison between Example 2 and Comparative Examples 11-12 in the above table, it can be seen that since the temperature of S63 in Example 2 is controlled at 80°C-90°C, the comprehensive indicators of Example 2 are significantly better than those of Comparative Examples 11-12.

[0124] From the comparison between Example 2 and Comparative Example 13 in the above table, it can be seen that since the temperature of S64 in Comparative Example 13 is lower than the temperature of S64 in Example 2, the comprehensive indicators of Comparative Example 13 are significantly worse than those of Example 2.

[0125] From the comparison between Example 2 and Comparative Example 14 in the above table, it can be seen that since Comparative Example 14 is a ceramic diaphragm, it is unable to effectively suppress the expansion of the modified silicon-carbon laminate lithium battery during the formation process, resulting in various comprehensive indicators of Comparative Example 14 being significantly worse than those of Example 2.

[0126] The above-mentioned embodiments only express several implementation methods of the present disclosure, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the disclosed patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present disclosure, and these all belong to the protection scope of the present disclosure. Therefore, the protection scope of the disclosed patent shall be subject to the attached claims.

Claims

1. A formation method for a modified silicon-carbon laminate lithium battery, characterized in that: The steps include: Obtaining a modified silicon-carbon laminated lithium battery filled with liquid; wherein a highly elastic winding three-dimensional conductive mesh is formed in the negative electrode active material layer of the silicon-based negative electrode sheet of the modified silicon-carbon laminated lithium battery, and the highly elastic winding three-dimensional conductive mesh is used to inhibit the expansion and peeling of the silicon-carbon material; the diaphragm of the modified silicon-carbon laminated lithium battery is a polymer diaphragm; The modified silicon-carbon laminated lithium battery injected with liquid is subjected to a first stage of low-temperature, low-voltage, small-current constant-current charging operation to charge the modified silicon-carbon laminated lithium battery to 15% to 20% SOC; The modified silicon-carbon laminated lithium battery that has undergone the first stage of low-temperature, low-voltage, small-current constant-current charging operation is subjected to a second stage of low-temperature, medium-voltage, medium-current constant-current charging operation, so that the modified silicon-carbon laminated lithium battery is charged to 40% to 60% SOC; The modified silicon-carbon laminated lithium battery that has undergone the second stage of low-temperature, medium-voltage, medium-current constant-current charging operation is subjected to a third stage of high-temperature, high-voltage, large-current constant-current charging operation, so that the modified silicon-carbon laminated lithium battery is charged to 100% SOC; The modified silicon-carbon laminated lithium battery that has undergone the third stage of high-temperature, high-pressure, high-current constant-current charging operation is subjected to a fourth stage of low-temperature, high-voltage, high-current constant-current discharging operation, so that the modified silicon-carbon laminated lithium battery is discharged to 30% to 50% DOD; The modified silicon-carbon laminated lithium battery that has undergone the fourth stage of low-temperature, high-voltage, high-current constant-current discharge operation is subjected to a room-temperature static operation.

2. The formation method of the modified silicon-carbon laminate lithium battery according to claim 1, characterized in that: At pressure F1 of 1kgf / cm 2 ~2kgf / cm 2 The first stage of low-temperature, low-voltage, small-current constant-current charging operation is carried out under the conditions of temperature of 30℃~40℃ and current of 0.1C~0.2C.

3. The formation method of the modified silicon-carbon laminate lithium battery according to claim 1, characterized in that: At pressure F2 of 3kgf / cm 2 ~4kgf / cm 2 The second stage of low-temperature, medium-voltage, medium-current constant-current charging operation is carried out under the conditions of temperature of 30℃~40℃ and current of 0.3C~0.4C.

4. The formation method of the modified silicon-carbon laminate lithium battery according to claim 1, characterized in that: At pressure F3 of 6kgf / cm 2 ~8kgf / cm 2 The third stage of high temperature, high voltage, high current constant current charging operation is carried out under the conditions of temperature of 80℃~90℃ and current of 0.5C~1.0C.

5. The formation method of the modified silicon-carbon laminate lithium battery according to claim 1, characterized in that: At pressure F4 of 6kgf / cm 2 ~8kgf / cm 2 The fourth stage of low-temperature, high-voltage, and high-current constant-current discharge is carried out under the conditions of a temperature of 30°C to 40°C and a current of 0.5C to 1.0C.

6. The formation method of the modified silicon-carbon laminate lithium battery according to claim 1, characterized in that: The time of the normal temperature static operation is 1 hour to 4 hours.

7. The formation method of modified silicon-carbon laminate lithium battery according to claim 1, characterized in that: The negative electrode active material layer includes graphite, silicon-carbon material, linear single-walled carbon nanotubes, mesh carbon fibers and a highly elastic binder; The linear single-walled carbon nanotubes, the mesh carbon fibers and the highly elastic binder are mixed to form the highly elastic winding three-dimensional conductive mesh; The highly elastic wound three-dimensional conductive mesh is mixed with the silicon-carbon material and the graphite to obtain a negative electrode slurry; the negative electrode slurry is coated on a negative electrode current collector to form the negative electrode active material layer.

8. The formation method of the modified silicon-carbon laminate lithium battery according to claim 7, characterized in that: The length of the linear single-walled carbon nanotube is 8 nm to 10 nm; and / or, The length of the mesh carbon fiber is 100um to 200um; and / or, The highly elastic binder includes at least one of PMA, PAA and SBR.

9. A modified silicon-carbon laminate lithium battery, characterized in that: The modified silicon-carbon laminate lithium battery is prepared by the formation method according to any one of claims 1 to 8.

10. The modified silicon-carbon laminate lithium battery according to claim 9, characterized in that: The modified silicon-carbon laminate lithium battery includes a shell and a battery cell, wherein the battery cell is arranged in the shell, and the battery cell includes a plurality of alternately stacked silicon-based negative electrode sheets, positive electrode sheets and silicon-based negative electrode sheets, wherein the silicon-based negative electrode sheets are separated from the positive electrode sheets by a diaphragm, and the diaphragm extends to the outer side surfaces of the silicon-based negative electrode sheets located on the outermost sides of the battery cell respectively.

Citation Information

Patent Citations

  • Lithium battery negative pole piece with excellent cycle performance and manufacturing method thereof, and lithium ion battery

    CN110556511A

  • Lithium battery based on silicon-carbon negative electrode and formation method thereof

    CN117080592A

  • Formation method of silicon negative electrode soft package lithium ion battery

    CN117080594A

  • Butter cutting device

    KR102509967B1

Cited By

  • Formation process of silicon-based soft package battery

    CN120527493A