Method for preparing non-dehumidified perfluoropolymer membrane, non-dehumidified perfluoropolymer membrane and filtering device

The removal of fluorine atoms on the surface of the perfluoropolymer film by gamma radiation solves the problem of reduced fluorine polymer film flux under small pore size, and prepares a perfluoropolymer film that does not dehumidify, achieving good moisturization Wetness and separation properties, suitable for filtration applications in the semiconductor industry.

CN118874236APending Publication Date: 2024-11-01알리오스 바이오테크 (상하이) 컴퍼니 리미티드

Patent Information

Application Number
CN202410932690.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the prior art, hydrophilic modification methods for perfluoropolymer films in the semiconductor industry lead to a significant reduction in flux under small pore sizes, and common methods cause damage to the membrane or reduce flux.

Method used

Gamma radiation removes some fluorine atoms on the surface of the perfluoropolymer film, and pre-wetting treatment and gamma radiation source radiation to prepare a perfluoropolymer film that does not dehumidify to maintain the film's flux and separation performance. .

Benefits of technology

The good contact wetting and dehumidification resistance of perfluoropolymer film is achieved, and the separation performance such as flux and bubble point pressure are not affected, with low gamma radiation dose and good mechanical strength, suitable for filtration Preparation of the instrument.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004940613570000091
    Figure BDA0004940613570000091
  • Figure BDA0004940613570000131
    Figure BDA0004940613570000131
  • Figure BDA0004940613570000141
    Figure BDA0004940613570000141
Patent Text Reader

Abstract

The invention discloses a method for preparing a non-dehumidified perfluoropolymer film. The non-dehumidified perfluoropolymer film is obtained by irradiating, washing and drying a pre-wetted perfluoropolymer film by adopting a gamma radiation source. The preparation method provided by the invention has simple steps, and no chemical crosslinking reaction occurs in the modification process; the non-dehumidification perfluoropolymer membrane has good contact wettability and dehumidification resistance, and meanwhile, the separation performance such as flux, bubble point pressure value and the like is not affected.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of special industrial filtration, and in particular relates to a method for preparing a non-dehumidifying perfluoropolymer membrane, a non-dehumidifying perfluoropolymer membrane and a filtration device. Background Art

[0002] Fluoropolymer is a straight-chain alkane polymer in which some or all hydrogen atoms in its molecular structure are replaced by fluorine. Fluoropolymers include ethylene-tetrafluoroethylene copolymer (ETFE), polytetrafluoroethylene (PTFE), fluorinated ethylene-propylene copolymer (FEP), perfluoroalkoxy resin (PFA), polychlorotrifluoroethylene (PCTFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), polyvinylidene fluoride (PVDF) and polyvinyl fluoride.

[0003] In the semiconductor industry, wet etching and cleaning processes are required to remove organic and inorganic pollutants from the surface of the wafer. The SPM cleaning process is one of the wet etching and cleaning processes. The high oxidation capacity of SPM is used to oxidize inorganic pollutants and dissolve them in the cleaning solution, while oxidizing organic matter to generate carbon dioxide and water. Specifically, the SPM cleaning solution is composed of sulfuric acid (H2SO4), hydrogen peroxide (H2O2) and water (H2O). The SPM cleaning solution is usually used for cleaning at a temperature of 120℃-150℃ for about 10 minutes. It is usually necessary to control the contamination of the solvent delivered to the surface of the wafer through a large number of filtration processes. Since the SPM cleaning process requires high-temperature concentrated sulfuric acid, in order to maintain the integrity of the filter, a fluoropolymer membrane resistant to acid and alkali corrosion is required. However, ordinary fluoropolymer membranes have strong hydrophobicity and will attract tiny bubbles in the feed flow to form local dehumidification points, thereby reducing the flow rate of the filter. As the number of dehumidification points increases, the flux of the filter will be significantly reduced. In order to avoid the accumulation of bubbles in the porous perfluoropolymer membrane, the fluoropolymer membrane needs to be hydrophilically modified.

[0004] W. Moyer et al. disclosed in US6179132 in 2001 the hydrophilic modification of a 0.1 μm PTFE membrane coated with a nafion (Nafion membrane, the foreign name is nafion nr 50 (beads 10-35mesh), perfluorosulfonic acid membrane) solution. However, when the pore size of the PTFE membrane becomes smaller, the coated polymer blocks the pore size, resulting in a significant reduction in the flux of the PTFE membrane. A. Signh disclosed a very similar coating process in US20170028359A1 in 2017, which prevents the PTFE membrane from dehumidifying, but when the pore size becomes smaller, it brings about an unavoidable reduction in flux. In summary, the use of a coating process to hydrophilically modify a perfluoropolymer membrane with a very small pore size (especially a pore size below 0.1 microns) will result in a sharp decrease in the flux of the membrane.

[0005] In order to solve the problem of reduced flux after modification of perfluoropolymer membranes with very small pore sizes, several inventors disclosed a method of increasing hydrophilicity by removing part of the fluorine atoms from the perfluoropolymer membrane, and no significant reduction in flux occurred after modification. D. Abdoulayer disclosed a method of treating a PTFE membrane with ultraviolet light after pre-wetting with a Na2SO3 solution in W2004 / 007060 in 2004. By this method, no significant flux reduction was observed after modification even if the pore size of the membrane was very small. J. Ge disclosed a PTFE membrane treated by atmospheric plasma in US8789708B2 in 2014, and disclosed an Ebeam treated PTFE membrane in US2013 / 0043183A in 2013. In both cases, the treated PTFE membrane did not dehumidify after wet heat sterilization, and no significant flux reduction was observed when the pore size of the membrane was very small. However, the modification method using ultraviolet light and atmospheric plasma is not thorough in modifying the polymer membrane because of the low penetration of ultraviolet light and atmospheric plasma. Therefore, high doses of ultraviolet light or atmospheric plasma are required to modify the membrane, which will damage the polymer membrane. Compared with ultraviolet light and atmospheric plasma, electron beam (Ebeam) has better penetration ability, but its energy source is very large and will also cause significant damage to the perfluoropolymer membrane.

[0006] In the prior art, gamma rays are often used to induce polymerization or grafting reactions, thereby generating hydrophilic compounds on the surface of the membrane pores to improve the hydrophilicity of the polymer membrane. In the existing technical solutions, due to the addition of new compounds to the membrane pores, the pore size of the membrane will be reduced, resulting in a sharp decrease in the flux of the modified membrane. When the membrane pore size is less than 0.2μm, the reduction in flux can reach 50% or more, resulting in the performance of the membrane being too poor to be used.

[0007] The present invention uses gamma radiation to selectively remove some fluorine atoms from the membrane surface to reduce the hydrophobicity of the membrane and achieve non-dehumidification performance. Since gamma has high penetrating power, low-dose gamma radiation can be used to modify the membrane. The non-dehumidification perfluoropolymer membrane prepared by the preparation method of the present invention has good contact wettability and anti-dehumidification properties, and separation performance such as flux, bubble point pressure value, etc. is not affected. Summary of the invention

[0008] In order to overcome the defects of the prior art, one object of the present invention is to provide a method for preparing a non-dehumidifying perfluoropolymer membrane, another object of the present invention is to provide a non-dehumidifying perfluoropolymer membrane, and yet another object of the present invention is to provide a filtering device. To achieve the above objects, the technical solutions adopted by the present invention are as follows:

[0009] One aspect of the present invention provides a method for preparing a non-dewetting perfluoropolymer membrane, comprising the following steps:

[0010] Pre-wetting the perfluoropolymer membrane;

[0011] irradiating the pre-wetted perfluoropolymer membrane with a gamma radiation source of appropriate dose;

[0012] The irradiated perfluoropolymer membrane is rinsed and dried to obtain the non-dehumidifying perfluoropolymer membrane.

[0013] Preferably, the pre-wetting treatment of the perfluoropolymer membrane comprises:

[0014] pre-wetting the perfluoropolymer membrane with a first solution;

[0015] The first solution is exchanged for a second solution.

[0016] Preferably, the first solution is an alcohol solution, and the second solution is water or an inorganic salt solution.

[0017] Preferably, the first solution is at least one of methanol, ethanol and isopropanol.

[0018] Preferably, the second solution is a 0.1 M inorganic salt solution.

[0019] Preferably, the inorganic salt solution is at least one of Na2SO3 and Na2SO4 solutions.

[0020] Preferably, the dose of the gamma radiation source is between 30 kGy and 40 kGy.

[0021] Preferably, the dose of the gamma radiation source is between 30 kGy and 35 kGy.

[0022] Preferably, the irradiated perfluoropolymer membrane is rinsed with a third solution and dried, and the third solution is water.

[0023] Preferably, the non-dewetting perfluoropolymer membrane can be contact wetted by a fourth solution having a surface tension of less than or equal to 24.37 mN / m.

[0024] Preferably, the bubble point pressure value of the non-dewetting perfluoropolymer membrane varies by less than or equal to 15% compared with the bubble point pressure value of the perfluoropolymer membrane.

[0025] Preferably, the bubble point pressure value of the non-dewetting perfluoropolymer membrane varies by less than or equal to 5% compared with the bubble point pressure value of the perfluoropolymer membrane.

[0026] Preferably, the flux of the non-dewetting perfluoropolymer membrane varies by 20% or less compared to the flux of the perfluoropolymer membrane.

[0027] Preferably, the flux of the non-dewetting perfluoropolymer membrane varies by 10% or less compared to the flux of the perfluoropolymer membrane.

[0028] Preferably, the non-dewetting perfluoropolymer film has a breaking strain greater than or equal to 15%.

[0029] Preferably, the non-dewetting perfluoropolymer film has a breaking strain greater than or equal to 20%.

[0030] Preferably, the non-dehumidifying perfluoropolymer membrane is a microporous membrane, and the pore size of the microporous membrane is less than or equal to 0.2 μm.

[0031] Preferably, the pore size of the microporous membrane is less than or equal to 50 nm.

[0032] Another aspect of the present invention provides a non-dewetting perfluoropolymer membrane, which is prepared according to the above method for preparing a non-dewetting perfluoropolymer membrane, and the non-dewetting perfluoropolymer membrane can be wetted by a fourth solution having a surface tension of less than or equal to 24.37 mN / m.

[0033] Preferably, the non-dehumidifying perfluoropolymer membrane is a microporous membrane, and the pore size of the microporous membrane is less than or equal to 0.2 μm.

[0034] Preferably, the pore size of the microporous membrane is less than or equal to 50 nm.

[0035] Preferably, the bubble point pressure value of the non-dewetting perfluoropolymer membrane varies by less than or equal to 15% compared with the bubble point pressure value of the perfluoropolymer membrane.

[0036] Preferably, the bubble point pressure value of the non-dewetting perfluoropolymer membrane varies by less than or equal to 5% compared with the bubble point pressure value of the perfluoropolymer membrane.

[0037] Preferably, the flux of the non-dewetting perfluoropolymer membrane varies by 20% or less compared to the flux of the perfluoropolymer membrane.

[0038] Preferably, the flux of the non-dewetting perfluoropolymer membrane varies by 10% or less compared to the flux of the perfluoropolymer membrane.

[0039] Preferably, the non-dewetting perfluoropolymer film has a breaking strain greater than or equal to 15%.

[0040] Preferably, the non-dewetting perfluoropolymer film has a breaking strain greater than or equal to 20%.

[0041] Preferably, the non-dewetting perfluoropolymer membrane is applied to a filtration device.

[0042] Another aspect of the present invention provides a filtering device, comprising a housing having a fluid inlet and a fluid outlet, wherein the housing is provided with the non-dehumidifying perfluoropolymer membrane as described above.

[0043] The method for preparing a non-dehumidifying perfluoropolymer membrane of the present invention comprises irradiating a pre-wetted perfluoropolymer membrane with a gamma radiation source, rinsing and drying to obtain a non-dehumidifying perfluoropolymer membrane. The present invention irradiates the perfluoropolymer with a small irradiation dose using a high-penetration gamma radiation source to obtain the non-dehumidifying perfluoropolymer membrane. The non-dehumidifying perfluoropolymer membrane of the present invention has good contact wettability and anti-dehumidification properties, while separation performance such as flux, bubble point pressure value, etc. is not affected. Since the dose used by the gamma radiation source is relatively low, the non-dehumidifying perfluoropolymer membrane has good mechanical strength and can meet the foldability requirements for filter preparation. DETAILED DESCRIPTION

[0044] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0045] The perfluoropolymer membrane of the present invention includes polytetrafluoroethylene (PTFE), fluorinated ethylene-propylene copolymer (FEP), perfluoroalkoxy resin (PFA), or copolymers thereof.

[0046] The perfluoropolymer film of the present invention may be a single-layer film or a multi-layer film.

[0047] The perfluoropolymer membrane of the present invention may be a microporous membrane with a pore size not greater than 0.2 μm, preferably a microporous membrane with a pore size less than or equal to 50 nm.

[0048] For the convenience of comparison, Examples 1 to 4 of the present invention and Comparative Examples 1 to 28 all use Gore 0.1 μm polytetrafluoroethylene (PTFE) membranes, which are single-layer membranes. When a multi-layer membrane is used, the experimental results are similar.

[0049] The preparation steps of non-dewetting perfluoropolymer membrane are as follows:

[0050] The polytetrafluoroethylene membrane is pre-wetted by pre-wetting the polytetrafluoroethylene membrane with a first solution, and the first solution is replaced with a second solution. Specifically, the first solution is an alcohol solution, and further, the first solution is at least one of methanol, ethanol, and isopropanol; the second solution is water or an inorganic salt solution, and further, the second solution is a 0.1M inorganic salt solution, and further, the inorganic salt solution is at least one of Na2SO3 and Na2SO4 solutions.

[0051] In order to prevent the pre-wetted polytetrafluoroethylene film from drying out before gamma irradiation, in some embodiments and comparative examples of the present invention, the pre-wetted polytetrafluoroethylene film is sandwiched between two layers of polyethylene films (PE) to prevent the polytetrafluoroethylene film from drying out. In other embodiments and comparative examples of the present invention, when the polytetrafluoroethylene film is irradiated with a gamma radiation source immediately after pre-wetting, the wetted polytetrafluoroethylene film will not dry out due to the short interval time, so it is not necessary to sandwich the pre-wetted polytetrafluoroethylene film between two layers of polyethylene films to maintain the moisture therein.

[0052] The pre-moistened polytetrafluoroethylene membrane is irradiated with a gamma radiation source of appropriate dose.

[0053] The irradiated polytetrafluoroethylene membrane is rinsed and dried to obtain the non-dehumidifying perfluoropolymer membrane. Specifically, the irradiated perfluoropolymer membrane is rinsed and dried with a third solution, and the third solution is water.

[0054] Comparative Example 1:

[0055] The polytetrafluoroethylene film is not pre-wetted, the polytetrafluoroethylene film is sandwiched between two layers of PE film, and the polytetrafluoroethylene film is irradiated with a gamma radiation source of 6.2 to 6.6 kGy. The irradiated polytetrafluoroethylene film is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer film.

[0056] Comparative Example 2:

[0057] The polytetrafluoroethylene membrane is subjected to a pre-wetting treatment; specifically, the first solution is methanol (MeOH), and the polytetrafluoroethylene membrane is immersed in the methanol solution. Specifically, the second solution is water, and the methanol solution is exchanged with water. Specifically, the polytetrafluoroethylene membrane is immersed in an aqueous solution to replace the methanol with water. The pre-wetting polytetrafluoroethylene membrane is sandwiched between two layers of PE films to maintain the wettability of the polytetrafluoroethylene membrane. The pre-wetting polytetrafluoroethylene membrane is irradiated with a gamma radiation source of 6.2 to 6.6 kGy. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0058] Comparative Example 3:

[0059] The polytetrafluoroethylene membrane is subjected to a pre-wetting treatment; specifically, the first solution is methanol (MeOH), and the polytetrafluoroethylene membrane is immersed in the methanol solution. Specifically, the second solution is a 0.1M Na2SO3 solution, and the methanol solution is exchanged with a 0.1M Na2SO3 solution. Specifically, the polytetrafluoroethylene membrane is immersed in a 0.1M Na2SO3 solution to replace the methanol with a 0.1M Na2SO3 solution. The pre-wetting polytetrafluoroethylene membrane is sandwiched between two layers of PE films to maintain the wettability of the polytetrafluoroethylene membrane. The pre-wetting polytetrafluoroethylene membrane is irradiated with a gamma radiation source of 6.2 to 6.6 kGy. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0060] Comparative Example 4:

[0061] The polytetrafluoroethylene membrane is subjected to a pre-wetting treatment; specifically, the first solution is methanol (MeOH), and the polytetrafluoroethylene membrane is immersed in the methanol solution. Specifically, the second solution is a 0.1M Na2SO4 solution, and the methanol solution is exchanged with a 0.1M Na2SO4 solution. Specifically, the polytetrafluoroethylene membrane is immersed in a 0.1M Na2SO4 solution to replace the methanol with a 0.1M Na2SO4 solution. The pre-wetting polytetrafluoroethylene membrane is sandwiched between two layers of PE films to maintain the wettability of the polytetrafluoroethylene membrane. The pre-wetting polytetrafluoroethylene membrane is irradiated with a gamma radiation source of 6.2 to 6.6 kGy. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0062] Comparative Example 5:

[0063] The polytetrafluoroethylene film is not pre-wetted, the polytetrafluoroethylene film is sandwiched between two layers of PE films, and the polytetrafluoroethylene film is irradiated with a gamma radiation source of 11.2 to 11.4 kGy. The irradiated polytetrafluoroethylene film is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer film.

[0064] Comparative Example 6:

[0065] The polytetrafluoroethylene membrane is subjected to a pre-wetting treatment; specifically, the first solution is methanol (MeOH), and the polytetrafluoroethylene membrane is immersed in the methanol solution. Specifically, the second solution is water, and the methanol solution is exchanged with water. Specifically, the polytetrafluoroethylene membrane is immersed in an aqueous solution to replace the methanol with water. The pre-wetting polytetrafluoroethylene membrane is sandwiched between two layers of PE films to maintain the wettability of the polytetrafluoroethylene membrane. The pre-wetting polytetrafluoroethylene membrane is irradiated with a gamma radiation source of 11.2 to 11.4 kGy. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0066] Comparative Example 7:

[0067] The polytetrafluoroethylene membrane is subjected to a pre-wetting treatment; specifically, the first solution is methanol (MeOH), and the polytetrafluoroethylene membrane is immersed in the methanol solution. Specifically, the second solution is a 0.1M Na2SO3 solution, and the methanol solution is exchanged with a 0.1M Na2SO3 solution. Specifically, the polytetrafluoroethylene membrane is immersed in a 0.1M Na2SO3 solution to replace the methanol with a 0.1M Na2SO3 solution. The pre-wetting polytetrafluoroethylene membrane is sandwiched between two layers of PE films to maintain the wettability of the polytetrafluoroethylene membrane. The pre-wetting polytetrafluoroethylene membrane is irradiated with a gamma radiation source of 11.2 to 11.4 kGy. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0068] Comparative Example 8:

[0069] The polytetrafluoroethylene membrane is subjected to a pre-wetting treatment; specifically, the first solution is methanol (MeOH), and the polytetrafluoroethylene membrane is immersed in the methanol solution. Specifically, the second solution is a 0.1M Na2SO4 solution, and the methanol solution is exchanged with a 0.1M Na2SO4 solution. Specifically, the polytetrafluoroethylene membrane is immersed in a 0.1M Na2SO4 solution to replace the methanol with a 0.1M Na2SO4 solution. The pre-wetting polytetrafluoroethylene membrane is sandwiched between two layers of PE films to maintain the wettability of the polytetrafluoroethylene membrane. The pre-wetting polytetrafluoroethylene membrane is irradiated with a gamma radiation source of 11.2 to 11.4 kGy. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0070] Comparative Example 9:

[0071] The polytetrafluoroethylene film is not pre-wetted, the polytetrafluoroethylene film is sandwiched between two layers of PE film, and the polytetrafluoroethylene film is irradiated with a gamma radiation source of 21.0 to 21.1 kGy. The irradiated polytetrafluoroethylene film is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer film.

[0072] Comparative Example 10:

[0073] The polytetrafluoroethylene membrane is subjected to a pre-wetting treatment; specifically, the first solution is methanol (MeOH), and the polytetrafluoroethylene membrane is immersed in the methanol solution. Specifically, the second solution is water, and the methanol solution is exchanged with water. Specifically, the polytetrafluoroethylene membrane is immersed in an aqueous solution to replace the methanol with water. The pre-wetting polytetrafluoroethylene membrane is sandwiched between two layers of PE films to maintain the wettability of the polytetrafluoroethylene membrane. The pre-wetting polytetrafluoroethylene membrane is irradiated with a gamma radiation source of 21.0 to 21.1 kGy. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0074] Comparative Example 11:

[0075] The polytetrafluoroethylene membrane is subjected to a pre-wetting treatment; specifically, the first solution is methanol (MeOH), and the polytetrafluoroethylene membrane is immersed in the methanol solution. Specifically, the second solution is a 0.1M Na2SO3 solution, and the methanol solution is exchanged with a 0.1M Na2SO3 solution. Specifically, the polytetrafluoroethylene membrane is immersed in a 0.1M Na2SO3 solution to replace the methanol with a 0.1M Na2SO3 solution. The pre-wetting polytetrafluoroethylene membrane is sandwiched between two layers of PE films to maintain the wettability of the polytetrafluoroethylene membrane. The pre-wetting polytetrafluoroethylene membrane is irradiated with a gamma radiation source of 21.0 to 21.1 kGy. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0076] Comparative Example 12:

[0077] The polytetrafluoroethylene membrane is subjected to a pre-wetting treatment; specifically, the first solution is methanol (MeOH), and the polytetrafluoroethylene membrane is immersed in the methanol solution. Specifically, the second solution is a 0.1M Na2SO4 solution, and the methanol solution is exchanged with a 0.1M Na2SO4 solution. Specifically, the polytetrafluoroethylene membrane is immersed in a 0.1M Na2SO4 solution to replace the methanol with a 0.1M Na2SO4 solution. The pre-wetting polytetrafluoroethylene membrane is sandwiched between two layers of PE films to maintain the wettability of the polytetrafluoroethylene membrane. The pre-wetting polytetrafluoroethylene membrane is irradiated with a gamma radiation source of 21.0 to 21.1 kGy. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0078] The ability of the test liquid to fill the pores of the porous film on the thickness of the film is called contact wettability. Test liquids with different surface tensions are added dropwise to the porous film surface, and the liquid can penetrate the film through the wetted portion of the porous film, and the wetted portion of the film is transparent compared to the non-wetted portion. When the test liquid is added dropwise to its surface, within five seconds, the wetted portion of its surface is observed to become transparent, that is, the porous film can be contact-wetted by the test liquid, which is marked as Y. When the test liquid is added dropwise to its surface, the porous film remains opaque, or the part of the porous film contacting the test liquid slowly (greater than about 5 to about 15 seconds) begins to wet, that is, the porous film cannot be contact-wetted by the test liquid, which is marked as N.

[0079] Polytetrafluoroethylene (PTFE) has a low surface energy, so a liquid with a lower surface tension is required to wet it. Water is a fluid with a relatively high surface tension, while methanol (MeOH) is a fluid with a relatively low surface tension. The surface tension of water can be changed by adding different doses of methanol to water. In the embodiments and comparative examples of the present invention, the contact wettability of the membrane is tested using a fourth solution having a surface tension of less than or equal to 24.37 m / Nm. Specifically, the contact wettability of the membrane is tested using 87wt%, 90wt%, and 95wt% methanol solutions. It is not difficult to understand that the methanol solution required for wetting the membrane has a lower MeOH content, indicating that the surface energy of the membrane is higher, and the ability to be contact-wetted by a lower content of methanol solution indicates that the membrane has good wetting properties.

[0080] The wetting properties of the non-dehumidifying perfluoropolymer membrane prepared by the preparation method described in Comparative Examples 1 to 12 were tested with a fourth solution. Specifically, the fourth solution was a methanol solution of different concentrations. The first solution, the second solution, the third solution, the gamma radiation source dose, the fourth solution, and the wetting properties test results of Comparative Examples 1 to 12 are shown in Table 1:

[0081] Table 1

[0082]

[0083] The results in Table 1 show that none of the control examples 1 to 12 can be wetted by 87 wt % MeOH, 90 wt % MeOH, and 95 wt % MeOH, indicating that the wettability of the polytetrafluoroethylene membranes described in the control examples 1 to 12 has not been improved. Therefore, it is necessary to increase the dose of the gamma radiation source to improve the wettability of the polytetrafluoroethylene membrane.

[0084] In the following comparative examples 13 to 27 and embodiments 1 to 5, the dose of the gamma radiation source was increased. Among them, comparative examples 13 to 17 only pre-wetted the polytetrafluoroethylene membrane without irradiating it with a gamma radiation source, for comparative analysis; comparative examples 18 to 27 and embodiments 1 to 5 irradiated the polytetrafluoroethylene membrane with different doses of gamma radiation sources.

[0085] Comparative Example 13:

[0086] The polytetrafluoroethylene membrane of this comparative example was not subjected to pre-wetting treatment.

[0087] Comparative Example 14:

[0088] The polytetrafluoroethylene membrane is pre-wetted, specifically, the polytetrafluoroethylene membrane is pre-wetted with a first solution; the first solution is replaced with a second solution, the first solution is methanol (MeOH), and the second solution is water.

[0089] Comparative Example 15:

[0090] The polytetrafluoroethylene membrane is pre-wetted, specifically, the polytetrafluoroethylene membrane is pre-wetted with a first solution; the first solution is replaced with a second solution, the first solution is methanol (MeOH), and the second solution is a 0.1 M Na2SO3 solution.

[0091] Comparative Example 16:

[0092] The polytetrafluoroethylene membrane is pre-wetted; specifically, the polytetrafluoroethylene membrane is pre-wetted with a first solution, and the first solution is exchanged with a second solution, the first solution is methanol (MeOH), and the second solution is a 0.1M Na2SO4 solution.

[0093] Comparative Example 17:

[0094] The polytetrafluoroethylene membrane is pre-wetted, specifically, the polytetrafluoroethylene membrane is pre-wetted with a first solution, and the first solution is replaced with a second solution, wherein the first solution is methanol (MeOH) and the second solution is a 0.1wt% Nafion solution. The Nafion solution is a perfluorosulfonic acid type polymer solution, which is generally composed of a fluorinated solvent containing a Nafion polymer and some additives.

[0095] Comparative Example 18:

[0096] The polytetrafluoroethylene membrane is not pre-wetted, and is irradiated with a 25-30 kGy gamma radiation source. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0097] Comparative Example 19:

[0098] The polytetrafluoroethylene membrane is pre-wetted; specifically, the first solution is methanol (MeOH), and the polytetrafluoroethylene membrane is immersed in the methanol solution. Specifically, the second solution is water, and the methanol solution is exchanged with water. Specifically, the polytetrafluoroethylene membrane is immersed in an aqueous solution to replace the methanol with water. The pre-wetted polytetrafluoroethylene membrane is irradiated with a 25-30 kGy gamma radiation source. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0099] Comparative Example 20:

[0100] The polytetrafluoroethylene membrane is subjected to a pre-wetting treatment; specifically, the first solution is methanol (MeOH), and the polytetrafluoroethylene membrane is immersed in the methanol solution. Specifically, the second solution is a 0.1M Na2SO3 solution, and the methanol solution is exchanged with a 0.1M Na2SO3 solution. Specifically, the polytetrafluoroethylene membrane is immersed in a 0.1M Na2SO3 solution to replace the methanol with a 0.1M Na2SO3 solution. The pre-wetting polytetrafluoroethylene membrane is sandwiched between two layers of PE films to maintain the wettability of the polytetrafluoroethylene membrane. A 25-30kGy gamma radiation source is used to irradiate the pre-wetting polytetrafluoroethylene membrane. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0101] Comparative Example 21:

[0102] The polytetrafluoroethylene membrane is subjected to a pre-wetting treatment; specifically, the first solution is methanol (MeOH), and the polytetrafluoroethylene membrane is immersed in the methanol solution. Specifically, the second solution is a 0.1M Na2SO4 solution, and the methanol solution is exchanged with a 0.1M Na2SO4 solution. Specifically, the polytetrafluoroethylene membrane is immersed in a 0.1M Na2SO4 solution to replace the methanol with a 0.1M Na2SO4 solution. The pre-wetting polytetrafluoroethylene membrane is sandwiched between two layers of PE films to maintain the wettability of the polytetrafluoroethylene membrane. The pre-wetting polytetrafluoroethylene membrane is irradiated with a 25-30kGy gamma radiation source. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0103] Comparative Example 22:

[0104] The polytetrafluoroethylene membrane is pre-wetted, specifically, the perfluoropolymer membrane is pre-wetted with a first solution; the first solution is replaced with a second solution, the first solution is methanol (MeOH), and the second solution is a 0.1wt% Nafion solution. The pre-wetted polytetrafluoroethylene membrane is irradiated with a 25-30kGy gamma radiation source. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidified perfluoropolymer membrane.

[0105] Comparative Example 23:

[0106] The polytetrafluoroethylene membrane is not pre-wetted, and is irradiated with a gamma radiation source of 30-35 kGy. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0107] Comparative Example 24:

[0108] The polytetrafluoroethylene membrane is pre-wetted, specifically, the perfluoropolymer membrane is pre-wetted with a first solution; the first solution is replaced with a second solution, the first solution is methanol (MeOH), and the second solution is water; the pre-wetted polytetrafluoroethylene membrane is irradiated with a 30-35 kGy gamma radiation source; the irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water, and dried at room temperature to obtain the non-dehumidified perfluoropolymer membrane.

[0109] Embodiment 1:

[0110] The polytetrafluoroethylene membrane is pre-wetted, specifically, the polytetrafluoroethylene membrane is pre-wetted with a first solution, and the first solution is exchanged with a second solution, the first solution is methanol (MeOH), and the second solution is a 0.1M Na2SO3 solution. Specifically, the polytetrafluoroethylene membrane is immersed in a methanol solution until the surface of the polytetrafluoroethylene membrane is wetted by methanol, and the air in the micropores is replaced by methanol with low surface tension. Pre-wetting the membrane can protect the membrane during irradiation with a gamma radiation source. Specifically, because polytetrafluoroethylene is hydrophobic, it can only be wetted with a fluid with low surface tension. In this embodiment, methanol is used. In other embodiments of the present invention, alcohol solutions such as ethanol and isopropanol can also be used. Specifically, since methanol has high volatility, in order to avoid the impact of methanol volatilization on subsequent processes, it is necessary to use a second solution to exchange the methanol. In this embodiment, a 0.1M Na2SO3 solution is used to exchange the methanol. In other embodiments of the present invention, water or other inorganic salt solutions can also be used to exchange the methanol. Specifically, the polytetrafluoroethylene membrane was immersed in a 0.1 M Na 2 SO 3 solution to replace the methanol with the 0.1 M Na 2 SO 3 solution.

[0111] The pre-wetting polytetrafluoroethylene membrane is irradiated with a 30-35 kGy gamma radiation source; in this embodiment, when the polytetrafluoroethylene membrane needs to be placed for a period of time before irradiation, the pre-wetting polytetrafluoroethylene membrane is sandwiched between two layers of PE films to maintain the wettability of the polytetrafluoroethylene membrane. Specifically, when the gamma radiation source irradiates the polytetrafluoroethylene membrane, a portion of the CF bonds of the polytetrafluoroethylene membrane will be broken, that is, defluorination occurs, thereby increasing the surface energy of the polytetrafluoroethylene membrane and improving the wetting performance.

[0112] The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0113] Embodiment 2:

[0114] A non-dewetting perfluoropolymer membrane was prepared by the method described in Example 1, except that the second solution was a 0.1 M Na2SO4 solution.

[0115] Comparative Example 25:

[0116] A non-dewetting perfluoropolymer membrane was prepared by the method described in Example 1, except that the second solution was a 0.1 wt % Nafion solution.

[0117] Comparative Example 26:

[0118] The polytetrafluoroethylene membrane is not pre-wetted, and is irradiated with a gamma radiation source of 35-40 kGy, and the irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidifying perfluoropolymer membrane.

[0119] Embodiment 3:

[0120] The polytetrafluoroethylene membrane is pre-wetted, specifically, the polytetrafluoroethylene membrane is pre-wetted with a first solution, the first solution is exchanged with a second solution, the first solution is methanol (MeOH), and the second solution is water. The pre-wetted polytetrafluoroethylene membrane is irradiated with a 35-40 kGy gamma radiation source. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidified perfluoropolymer membrane.

[0121] Embodiment 4:

[0122] The polytetrafluoroethylene membrane is pre-wetted, specifically, the polytetrafluoroethylene membrane is pre-wetted with a first solution; the first solution is replaced with water or a second solution, the first solution is methanol (MeOH), and the second solution is a 0.1M Na2SO3 solution. The pre-wetted polytetrafluoroethylene membrane is irradiated with a 35-40 kGy gamma radiation source. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidified perfluoropolymer membrane.

[0123] Embodiment 5:

[0124] The polytetrafluoroethylene membrane is pre-wetted, specifically, the polytetrafluoroethylene membrane is pre-wetted with a first solution, and the first solution is replaced with a second solution, wherein the first solution is methanol (MeOH) and the second solution is a 0.1M Na2SO4 solution. The pre-wetted polytetrafluoroethylene membrane is irradiated with a 35-40 kGy gamma radiation source. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidified perfluoropolymer membrane.

[0125] Comparative Example 27:

[0126] The polytetrafluoroethylene membrane is pre-wetted, specifically, the perfluoropolymer membrane is pre-wetted with a first solution, the first solution is exchanged with a second solution, the first solution is methanol (MeOH), and the second solution is a 0.1wt% Nafion solution. The pre-wetted polytetrafluoroethylene membrane is irradiated with a 35-40kGy gamma radiation source. The irradiated polytetrafluoroethylene membrane is thoroughly rinsed with water and dried at room temperature to obtain the non-dehumidified perfluoropolymer membrane.

[0127] Comparative Examples 13 to 17 are films that have not been irradiated with a gamma radiation source, and Comparative Examples 18 to 27 and Examples 1 to 5 are films that have been irradiated with gamma radiation sources of different doses. The wettability test method described above was used for testing, and the first solution, the second solution, the third solution, the gamma radiation dose, the fourth solution, and the wettability test results are shown in Table 2:

[0128] Table 2

[0129]

[0130]

[0131] The results in Table 2 show that after increasing the dose of the gamma radiation source, the wetting properties of the polytetrafluoroethylene membrane are significantly improved. Among them, when the second solution is 0.1wt% Nafion, the improvement of the wetting properties of the membrane is more prominent. However, in addition to the wetting properties, the performance of the membrane also includes separation properties (flux, bubble point pressure value), mechanical properties, etc. Therefore, it is necessary to further test the performance of the non-dehumidifying perfluoropolymer membrane to ensure that other properties can also meet the needs of practical applications.

[0132] Embodiment 6:

[0133] In this embodiment, the non-dehumidifying perfluoropolymer membrane is subjected to a bubble point pressure value test and a flux test, and the test method is as follows:

[0134] 1. Bubble point pressure value test:

[0135] The bubble point pressure value is a key parameter for characterizing microporous filtration membranes. It refers to the pressure required to force the wetting liquid (usually water or alcohol) to flow out of the largest pores in the membrane and induce a stable bubble flow. For the pore size of the membrane, a higher bubble point pressure value indicates that the membrane has a smaller pore size and has better particle retention and separation efficiency; for the integrity of the membrane, a bubble point pressure value lower than expected may indicate the presence of larger pores or defects, which will affect the membrane filtration performance and reliability; the principle of the bubble point pressure value test is: as long as the capillary pressure is greater than the pressure outside the pores, the pores filled with liquid in the membrane will retain the liquid. When the pressure outside the pores increases to a certain extent, the liquid in the pores will be displaced to form bubbles.

[0136] This experiment was tested using a bubble point tester, and the test fluid for the bubble point was isopropyl alcohol. The non-dehumidifying perfluoropolymer membrane was cut into membrane sheets, and the bubble point pressure value of the membrane sheet was tested. The test was repeated 3 times, and the highest pressure was determined as the bubble point pressure value of the non-dehumidifying perfluoropolymer membrane.

[0137] 2. Flux test

[0138] After the bubble point pressure value test is completed, the membrane is thoroughly rinsed with deionized water, the pressure of the compressed air is adjusted to 1 bar, and water passes through the membrane under the pressure difference. After reaching a balanced state, the water flux passing through the membrane is measured, which is the flux of the membrane. The test is repeated 3 times, and the average value is the flux of the non-dehumidifying perfluoropolymer membrane.

[0139] The above method was used to perform bubble point pressure value test and flux test on Control Examples 13, 15, 17 and Examples 1 to 5. The test results are shown in Table 3.

[0140] Table 3

[0141] First solution Second solution Gamma dose (kGy) The third solution Bubble point pressure value (psi) Flux (LMH / psi) Comparative Example 13 - - 0 water 27.5 720 Comparative Example 15 MeOH <![CDATA[0.1M Na2SO3]]> 0 water 29.0 780 Comparative Example 17 MeOH 0.1wt%Nafion 0 water 30.8 473 Example 1 MeOH <![CDATA[0.1M Na2SO3]]> 30-35 water 29.5 800 Example 2 MeOH <![CDATA[0.1M Na2SO4]]> 30-35 water 29.3 790 Example 3 MeOH water 35-40 water 28.8 820 Example 4 MeOH <![CDATA[0.1M Na2SO3]]> 35-40 water 29.8 816 Example 5 MeOH <![CDATA[0.1M Na2SO4]]> 35-40 water 30.2 768

[0142] According to the test results in Table 3, the bubble point pressure and flux of the membranes not irradiated by the gamma radiation source (Comparative Examples 13 and 15) did not change much.

[0143] Compared with the control example 13, the flux of the control example 17 decreased by about 34%, and the bubble point pressure value increased by about 12%. It can be seen that although the control example 17 can be wetted by the 87wt% MeOH solution, since the second solution is a Nafion solution, although the Nafion solution is helpful to improve the wetting property of the membrane, the Nafion solution is coated on the surface of the membrane pores and causes blockage, which will cause a significant decrease in the membrane flux.

[0144] Compared with the control example 15, the increase of the bubble point pressure values ​​of Examples 1 to 5 is within 15%, among which the bubble point pressure value of Example 3 is increased within 5%; the flux reduction is within 20%, among which the flux reduction of Example 2 is within 10%. The test results in Table 3 also show that it is necessary to irradiate the membrane with a gamma radiation source dose of 30 kGy or more to improve the wetting properties of the membrane while ensuring that the bubble point pressure value and flux of the membrane are not affected.

[0145] Compared with Example 2, no difference in the effect of Na2SO3 and Na2SO4 as the second solution on the wetting performance was observed in Example 1. When the dose of the gamma radiation source is 30-35 kGy, the second solution is Na2SO3 or Na2SO4, indicating that the inorganic salt solution has a certain help in improving the wetting performance of the membrane.

[0146] Compared with Example 1 and Example 2, when the dose of the gamma radiation source is increased to 35-40 kGy, the second solution can be water or an inorganic salt solution.

[0147] Embodiment 7:

[0148] In this example, the non-dehumidifying perfluoropolymer membrane is tested for dehumidification resistance. Dehumidification may occur when exposed to air for a long time or in other environments that promote dehumidification. Dehumidification resistance refers to the porous membrane being wetted by liquid after contacting or filtering a gas-containing liquid. The dehumidification resistance test method is as follows:

[0149] First, the non-dewetting perfluoropolymer membrane is pre-wetted, and then the non-dewetting perfluoropolymer membrane is thoroughly rinsed with water and placed on a workbench. Since the non-wetting portion of the non-dewetting perfluoropolymer membrane is non-transparent, when the non-dewetting perfluoropolymer membrane dewets, white spots will appear on the dewetting portion. The dewetting resistance of the non-dewetting perfluoropolymer membrane is tested by observing the time when the white spots appear. The longer the time when the white spots appear, the better the dewetting resistance of the non-dewetting perfluoropolymer membrane.

[0150] The dehumidification test was conducted at ambient temperature (21 degrees Celsius), relative humidity of 21-25%, and no airflow in the laboratory. Comparative Example 15 and Examples 1 to 5 were pre-wetted with IPA and then thoroughly rinsed with water. The non-dehumidified perfluoropolymer membranes used for testing were then placed side by side on the workbench. When white spots appeared on the membranes, it showed signs of dehumidification, and the time when the white spots appeared was recorded. The test results are shown in Table 4.

[0151] Table 4

[0152] First solution Second solution Gamma dose (kGy) The third solution Air dehumidification time Comparative Example 15 MeOH <![CDATA[0.1M Na2SO3]]> 0 water 6'41" Example 1 MeOH <![CDATA[0.1M Na2SO3]]> 30-35 water 11'16" Example 2 MeOH <![CDATA[0.1M Na2SO4]]> 30-35 water 11'14" Example 3 MeOH water 35-40 water 11'1" Example 4 MeOH <![CDATA[0.1M Na2SO3]]> 35-40 water 10'12" Example 5 MeOH <![CDATA[0.1M Na2SO4]]> 35-40 water 10'58"

[0153] According to the test results in Table 4, compared with the control example 15, the examples 1 to 5 need about 2 times the time to show signs of dehumidification in the air, indicating that the examples 1 to 5 are not easy to dehumidify. In practical applications, the presence of bubbles in the fluid may cause the membrane to dehumidify. Since the anti-dehumidification performance of the non-dehumidifying perfluoropolymer membrane is significantly improved, it can be expected that the service life of the filtration device using the non-dehumidifying perfluoropolymer membrane will be significantly improved.

[0154] Embodiment 8:

[0155] This example tests the mechanical properties of the non-dewetting perfluoropolymer membrane to test whether the non-dewetting perfluoropolymer membrane can be used in a filtration device using a pleated filter membrane.

[0156] Mechanical strength includes fracture stress and fracture strain, where fracture stress is a measure of the test sample's ability to resist tensile forces, expressed as the maximum load the sample can withstand when stretched to fracture, and the unit is cN. Fracture strain is the degree to which the test sample can deform or elongate before it breaks or fractures, and is a measure of the deformation that the material can withstand under tensile stress before failure. Fracture strain is usually expressed as a percentage or fractional value, indicating the elongation or deformation of the material compared to its original length.

[0157] The mechanical strength of the non-dehumidifying perfluoropolymer membrane was tested using a 6 mm wide strip of a Lian Gong CMT-05L. The test results are shown in Table 5.

[0158] Table 5

[0159] First solution Second solution Gamma dose (kGy) The third solution Fracture stress (cN) Fracture strain (%) Example 1 MeOH <![CDATA[0.1M Na2SO3]]> 30-35 water 44.8 24 Example 2 MeOH <![CDATA[0.1M Na2SO4]]> 30-35 water 44.1 24.3 Example 3 MeOH water 35-40 water 35.1 19.4 Example 4 MeOH <![CDATA[0.1M Na2SO3]]> 35-40 water 35.9 19.2 Example 5 MeOH <![CDATA[0.1M Na2SO4]]> 35-40 water 36.9 20.1

[0160] According to the test results in Table 5, the higher the gamma radiation dose, the smaller the fracture strain. Generally speaking, the fracture strains of Examples 1 to 5 are all greater than or equal to 15%, which can meet the requirements of the folded filter membrane, among which the fracture strains of Examples 1, 2 and 5 are all greater than 20%.

[0161] Embodiment 9:

[0162] This example tests the fluorine-to-carbon ratio and the fluorine-to-oxygen ratio of the non-dehumidifying perfluoropolymer membrane to prove that defluorination occurs in the perfluoropolymer membrane by adopting the technical solution of the present invention.

[0163] Perfluoropolymer membranes have a high degree of stability because the CF bond has the highest bond energy among single bonds. Moreover, the van der Waals radius of fluorine atoms is larger than that of hydrogen atoms, which makes the van der Waals interaction between atoms in polytetrafluoroethylene molecules larger, resulting in stronger repulsion. Fluorine atoms have an appropriate atomic radius, so that each fluorine atom can just fit in close proximity to the fluorine atoms on the intervening carbon atoms. This conformation enables the fluorine atoms to surround the CC main chain to form a protective layer with low surface energy. This is also an important reason why perfluoropolymer membranes have excellent chemical stability and thermal stability. At the same time, it also makes the perfluoropolymer hydrophobic. The technical solution of the present invention breaks a portion of the CF bonds of the perfluoropolymer, causing defluorination and improving the wetting properties of the perfluoropolymer.

[0164] XPS (X-ray photoelectron spectroscopy) was used to analyze the fluorine-to-carbon ratio and the fluorine-to-oxygen ratio of Control Example 13 and Example 4. The test results are shown in Table 6.

[0165] Table 6

[0166] First solution Second solution Gamma dose (kGy) The third solution C(%) O(%) F(%) F / C O / C Comparative Example 13 - - 0 water 38.20% 0.00% 61.80% 162.00% 0.00% Example 4 MeOH <![CDATA[0.1M Na2SO3]]> 35-40 water 47.70% 5.00% 47.30% 99.10% 10.60%

[0167] According to the test results in Table 6, compared with the control example 13, the fluorine-carbon ratio of Example 4 decreased, indicating that the perfluoropolymer film had defluorination, and the oxygen-carbon ratio increased, indicating an increase in CO bonds. Since the bond energy of the CO bond is less than the bond energy of the CF bond, the wetting properties of the non-dewetting perfluoropolymer film can be improved. The oxygen atoms can come from water, air, or residual oxygen atoms in the second solution.

[0168] Embodiment 10:

[0169] This embodiment provides the use of any of the non-dehumidifying perfluoropolymer membranes described in embodiments 1 to 5. In this embodiment, the non-dehumidifying perfluoropolymer membrane is used in a filtering device. The filtering device includes a stacked filter, a cartridge filter, a capsule filter, and a spiral wound filter.

[0170] The non-dehumidifying perfluoropolymer membrane may be a flat membrane or a hollow fiber membrane.

[0171] Embodiment 11:

[0172] This embodiment provides a filtering device. The filtering device comprises a housing having a fluid inlet and a fluid outlet, and the non-dehumidifying perfluoropolymer membrane as described in embodiments 1 to 5 is arranged in the housing.

[0173] In this embodiment, the filtering device includes a stacked filter, a cartridge filter, a capsule filter, a spiral wound filter, and the like.

[0174] The non-dewetting perfluoropolymer membrane may be a flat sheet membrane or a hollow fiber membrane.

[0175] The method for preparing a non-dehumidifying perfluoropolymer membrane of the present invention comprises irradiating a pre-wetted perfluoropolymer membrane with a gamma radiation source, rinsing and drying to obtain a non-dehumidifying perfluoropolymer membrane. The present invention irradiates the perfluoropolymer with a small irradiation dose using a high-penetration gamma radiation source to obtain the non-dehumidifying perfluoropolymer membrane. The non-dehumidifying perfluoropolymer membrane of the present invention has good contact wettability and anti-dehumidification properties, while separation performance such as flux, bubble point pressure value, etc. is not affected. At the same time, since the dose used by the gamma radiation source is relatively low, the non-dehumidifying perfluoropolymer membrane has good mechanical strength and can meet the foldability requirements for filter preparation.

[0176] Obviously, the above embodiments of the present invention are only examples for clearly explaining the present invention, and are not intended to limit the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. The embodiments of the present invention cannot exhaust all implementation methods. All obvious changes or modifications derived from the technical solutions of the present invention are still within the scope of protection of the present invention. All documents mentioned in the present invention are cited as references in this application, just as if a document is cited as a reference alone.

Claims

1. A method for preparing a non-dehumidifying perfluoropolymer membrane, characterized in that: The following steps are involved: Pre-wetting the perfluoropolymer membrane; irradiating the pre-wetted perfluoropolymer membrane with a gamma radiation source of appropriate dose; The irradiated perfluoropolymer membrane is rinsed and dried to obtain the non-dehumidifying perfluoropolymer membrane.

2. The method for preparing a non-dehumidifying perfluoropolymer membrane according to claim 1, characterized in that: The pre-wetting treatment of the perfluoropolymer membrane comprises: pre-wetting the perfluoropolymer membrane with a first solution; The first solution is exchanged for a second solution.

3. The method for preparing a non-dehumidifying perfluoropolymer membrane according to claim 2, characterized in that: The first solution is an alcohol solution, and the second solution is water or an inorganic salt solution.

4. The method for preparing a non-dehumidifying perfluoropolymer membrane according to claim 2, characterized in that: The first solution is at least one of methanol, ethanol and isopropanol.

5. The method for preparing a non-dehumidifying perfluoropolymer membrane according to claim 2, characterized in that: The second solution is a 0.1 M inorganic salt solution.

6. The method for preparing a non-dehumidifying perfluoropolymer membrane according to claim 5, characterized in that: The inorganic salt solution is at least one of Na2SO3 and Na2SO4 solutions.

7. The method for preparing a non-dewetting perfluoropolymer membrane according to claim 3, characterized in that: The dose of the gamma radiation source is between 30 kGy and 40 kGy.

8. The method for preparing a non-dewetting perfluoropolymer membrane according to claim 5, characterized in that: The dose of the gamma radiation source is between 30 kGy and 35 kGy.

9. The method for preparing a non-dewetting perfluoropolymer membrane according to claim 1, characterized in that: The irradiated perfluoropolymer membrane is rinsed with a third solution and dried, wherein the third solution is water.

10. The method for preparing a non-dewetting perfluoropolymer membrane according to claim 1, characterized in that: The non-dewetting perfluoropolymer membrane can be contact wetted by a fourth solution having a surface tension less than or equal to 24.37 mN / m.

11. The method for preparing a non-dewetting perfluoropolymer membrane according to claim 1, characterized in that: The bubble point pressure value of the non-dewetting perfluoropolymer membrane varies by less than or equal to 15% compared with the bubble point pressure value of the perfluoropolymer membrane.

12. The method for preparing a non-dewetting perfluoropolymer membrane according to claim 11, characterized in that: The bubble point pressure value of the non-dewetting perfluoropolymer membrane varies by less than or equal to 5% compared with the bubble point pressure value of the perfluoropolymer membrane.

13. The method for preparing a non-dewetting perfluoropolymer membrane according to claim 1, characterized in that: The flux of the non-dewetting perfluoropolymer membrane varies by 20% or less compared to the flux of the perfluoropolymer membrane.

14. The method for preparing a non-dewetting perfluoropolymer membrane according to claim 13, characterized in that: The flux of the non-dewetting perfluoropolymer membrane varies by 10% or less compared to the flux of the perfluoropolymer membrane.

15. The method for preparing a non-dewetting perfluoropolymer membrane according to claim 1, characterized in that: The non-dewetting perfluoropolymer film has a breaking strain greater than or equal to 15%.

16. The method for preparing a non-dewetting perfluoropolymer membrane according to claim 15, characterized in that: The fracture strain of the non-dewetting perfluoropolymer film is greater than or equal to 20%.

17. The method for preparing a non-dewetting perfluoropolymer membrane according to claim 1, characterized in that: The non-dehumidifying perfluoropolymer membrane is a microporous membrane, and the pore size of the microporous membrane is less than or equal to 0.2 μm.

18. The method for preparing a non-dewetting perfluoropolymer membrane according to claim 17, characterized in that: The pore size of the microporous membrane is less than or equal to 50 nm.

19. A non-dewetting perfluoropolymer membrane, prepared according to the method for preparing a non-dewetting perfluoropolymer membrane according to any one of claims 1 to 9, characterized in that: The non-dewetting perfluoropolymer membrane can be contact wetted by a fourth solution having a surface tension less than or equal to 24.37 mN / m.

20. The non-dewetting perfluoropolymer membrane according to claim 19, characterized in that The non-dehumidifying perfluoropolymer membrane is a microporous membrane, and the pore size of the microporous membrane is less than or equal to 0.2 μm.

21. The non-dewetting perfluoropolymer membrane according to claim 20, characterized in that The pore size of the microporous membrane is less than or equal to 50 nm.

22. The non-dewetting perfluoropolymer membrane according to claim 19, characterized in that The bubble point pressure value of the non-dewetting perfluoropolymer membrane varies by less than or equal to 15% compared with the bubble point pressure value of the perfluoropolymer membrane.

23. The non-dewetting perfluoropolymer membrane according to claim 22, characterized in that The bubble point pressure value of the non-dewetting perfluoropolymer membrane varies by less than or equal to 5% compared with the bubble point pressure value of the perfluoropolymer membrane.

24. The non-dewetting perfluoropolymer membrane according to claim 19, characterized in that The flux of the non-dewetting perfluoropolymer membrane varies by 20% or less compared to the flux of the perfluoropolymer membrane.

25. The non-dewetting perfluoropolymer membrane according to claim 24, characterized in that The flux of the non-dewetting perfluoropolymer membrane varies by 10% or less compared to the flux of the perfluoropolymer membrane.

26. The non-dewetting perfluoropolymer membrane according to claim 19, characterized in that The non-dehumidifying perfluoropolymer film has a breaking strain greater than or equal to 15%.

27. The non-dewetting perfluoropolymer membrane according to claim 26, characterized in that The non-dehumidifying perfluoropolymer film has a fracture strain greater than or equal to 20%.

28. The non-dewetting perfluoropolymer membrane according to claim 19, characterized in that The non-dewetting perfluoropolymer membrane is applied to a filtering device.

29. A filtering device, comprising a housing, the housing having a fluid inlet and a fluid outlet, characterized in that: The non-dehumidifying perfluoropolymer membrane as claimed in claim 19 is disposed in the housing.

Citation Information

Patent Citations

  • Coated PTFE membrane

    US20170028359A1

  • Surface modified polymeric substrate and process

    US6179132B1

  • Atmospheric pressure microwave plasma treated porous membranes

    US8789708B2

Cited By

  • Preparation method of anti-dehumidification fluorine-containing polymer filter membrane